Hydrophilic and hydrophobic double-comb amphoteric composite membrane for vanadium battery and preparation method of hydrophilic and hydrophobic double-comb amphoteric composite membrane

By introducing hydrophobic and hydrophilic branched hydrophobic double-comb amphiphilic composite membranes into all vanadium flow batteries, the problems of microphase separation and proton conduction capacity of existing membranes are solved, and the voltage of vanadium batteries is significantly improved and Energy efficiency achieves more efficient ion migration and mechanical properties.

CN118899488AInactive Publication Date: 2024-11-05HANGZHOU DEHAI AIKE ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411393029.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118899488A_ABST
    Figure CN118899488A_ABST
Patent Text Reader

Abstract

The invention discloses a hydrophilic and hydrophobic double-comb type amphoteric composite membrane for a vanadium battery and a preparation method of the hydrophilic and hydrophobic double-comb type amphoteric composite membrane. The composite membrane is prepared by performing graft modification on sulfonated polybenzimidazole, so that the sulfonated polybenzimidazole is grafted with a hydrophobic branch chain and a hydrophilic branch chain to form a membrane. The preparation method further comprises the following steps: S1, preparing a sulfonated polybenzimidazole solution; s2, preparing hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole; s3, preparing a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole composite membrane; and S4, preparing the hydrophilic and hydrophobic double-comb amphoteric composite membrane. Hydrophobic and hydrophilic branched chains are introduced into a sulfonated polybenzimidazole polymer chain segment, so that aggregation of the hydrophobic chain segment is improved, the form of microphase separation is improved, and a three-dimensional ion channel can remarkably improve the ion mobility and transmission efficiency under the condition of low water absorption; meanwhile, imidazolyl of a PBI main chain forms an ionic cross-linked structure, so that the mechanical property of the membrane is improved, the proton transmission density of the membrane is increased, and the voltage and energy efficiency of the vanadium battery are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange membranes for all-vanadium liquid flow batteries, and in particular to a hydrophilic and hydrophobic double-comb type amphoteric composite membrane for vanadium batteries and a preparation method thereof. Background Art

[0002] Among the many ion exchange groups in the ion membrane for all-vanadium redox flow batteries (VRFB), positively charged groups such as imidazole, primary amine, and tertiary amine are often used as functional groups of membrane polymer segments. However, due to the interaction between cationic and anionic groups, the hydrophobic segments of the main chain of the membrane polymer are difficult to aggregate, thus limiting its microphase separation structure. In addition, the content of cations and anions is also limited due to the compatibility of the membrane. The ratio is limited, and the two groups cannot be increased or decreased at the same time, thereby limiting the ion exchange capacity, which in turn limits the conductivity, and there is an upper limit to the improvement of membrane performance.

[0003] The excellent vanadium resistance and antioxidant properties of polybenzimidazole give it great development and application prospects in vanadium flow batteries, but the sulfonated polybenzimidazole membrane still has problems with its microphase separation structure and limited proton conductivity. Summary of the invention

[0004] The purpose of the present invention is to provide a hydrophilic and hydrophobic double-comb type amphoteric composite membrane for vanadium batteries and a preparation method thereof to solve the above problems.

[0005] The technical solution adopted by the present invention is as follows: A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3-6 parts by mass of sulfonated polybenzimidazole to 100-150 parts by mass of a solvent, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution; Step S2, preparing a hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole: adding 0.1-0.4 parts by mass of bromoalkane, 0.1-0.4 parts by mass of sultone and 0.02-0.0.05 parts by mass of a catalyst to a sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 60-80° C. and reacting for 8-12 hours, and after the reaction is completed, pouring the solution in the bottle into acetone in a stirring state to precipitate, and then drying in an oven at 40-60° C. for 24 hours to obtain a hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole; Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: re-dissolving the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in a solvent to obtain a 5-10wt% solution, pouring the solution onto a clean glass plate, coating with a scraper, and raising the temperature to 70-90°C until the solvent is completely dried and volatilized to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane; Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 20-30wt% acid solution for 10-12h, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0006] Preferably, the solvent in steps S1 and S3 is any one of dimethyl sulfoxide, N,N-dimethylacetamide, and N,N-dimethylformamide.

[0007] Preferably, the brominated alkane in step S2 is any one of octyl bromide, hexyl bromide, pentane bromide, propyl bromide and ethyl bromide.

[0008] Preferably, the sultone in step S2 is any one of 1,3-propane sultone, 3-fluoro-1,3-propane sultone and 1,4-butane sultone.

[0009] Preferably, the catalyst in step S2 is any one of 4-dimethylaminopyridine, ammonium formate and sodium hydride.

[0010] Preferably, in step S3, the thickness of the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane is 40-60 μm.

[0011] Preferably, the acid solution in step S4 is at least one of a sulfuric acid solution, a hydrochloric acid solution, and a phosphoric acid solution.

[0012] A hydrophilic and hydrophobic double-comb type amphoteric composite membrane for vanadium batteries is prepared by adopting the above-mentioned method for preparing a hydrophilic and hydrophobic double-comb type amphoteric composite membrane for vanadium batteries.

[0013] The beneficial effects of the present invention are:

[0014] 1. The present invention introduces hydrophobic side chains into the sulfonated polybenzimidazole polymer chain segments, which can hinder the shuttling of vanadium ions through the steric hindrance effect and improve the coulombic efficiency of the vanadium battery.

[0015] 2. The present invention introduces hydrophobic side chains into the sulfonated polybenzimidazole polymer chain segments, thereby improving the aggregation of the hydrophobic chain segments, thereby improving the morphology of microphase separation, so that the three-dimensional ion channel can significantly improve the ion mobility and transmission efficiency under low water absorption, thereby improving the voltage and energy efficiency of the vanadium battery.

[0016] 3. The hydrophilic sulfonic acid side chains with ionic properties are introduced into the sulfonated polybenzimidazole polymer chain segments of the present invention, which can form an ionic cross-linked structure with the imidazole group of the PBI main chain, thereby improving the mechanical properties of the membrane. In addition, the membrane proton transmission density can be increased to further improve the voltage and energy efficiency of the vanadium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1This is a diagram showing the preparation mechanism of hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole according to Example 1 of the present invention; Figure 2 This is the H NMR spectrum of the hydrophilic-hydrophobic double-comb sulfonated polybenzimidazole in Example 1 of the present invention; DETAILED DESCRIPTION

[0018] The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The present invention provides a method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery, comprising the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3-6 parts by mass of sulfonated polybenzimidazole to 100-150 parts by mass of a solvent, stirring at 60°C until completely dissolved, to obtain a sulfonated polybenzimidazole solution. The solvent is any one of dimethyl sulfoxide, N,N-dimethylacetamide, and N,N-dimethylformamide; Step S2, prepare hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole: add 0.1-0.4 parts by mass of brominated alkane, 0.1-0.4 parts by mass of sultone and 0.02-0.0.05 parts by mass of catalyst to the sulfonated polybenzimidazole solution, stir and mix evenly, heat to 60-80°C to react for 8-12 hours, pour the solution in the bottle into acetone in a stirring state after the reaction, precipitate, and then dry in an oven at 40-60°C for 24 hours to obtain hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole. Wherein, the brominated alkane is any one of bromooctane, hexyl bromide, pentane bromide, propane bromide, and ethyl bromide; the sultone is any one of 1,3-propane sultone, 3-fluoro-1,3-propane sultone, and 1,4-butane sultone; the catalyst is any one of 4-dimethylaminopyridine, ammonium formate, and sodium hydride; Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: re-dissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in a solvent to obtain a 5-10wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 70-90°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 40-60μm.

[0020] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 20-30wt% acid solution for 10-12h, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane. The acid solution is at least one of a sulfuric acid solution, a hydrochloric acid solution, and a phosphoric acid solution.

[0021] Embodiment 1:

[0022] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 4 parts by mass of sulfonated polybenzimidazole to 120 parts by mass of dimethyl sulfoxide as a solvent, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0023] Step S2, preparing hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole: adding 0.2 parts by mass of hexyl bromide, 0.2 parts by mass of 1,3-propane sultone and 0.03 parts by mass of catalyst sodium hydride to the sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 60°C for reaction for 10 hours, and after the reaction, pouring the solution in the bottle into stirring acetone to precipitate, and then drying in a 50°C oven for 24 hours to obtain hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole. Figure 1 As shown in FIG. 1 , hexyl bromide and 1,3-propane sultone are grafted onto the sulfonated polybenzimidazole polymer chain segment under the action of a catalyst. Figure 2 As shown, the characteristic peaks of sultone are at 4.5ppm, 3.45ppm, and 2.5ppm, respectively. Due to the grafting of bromohexane and 1-3-propane sultone, the characteristic peaks of methyl and methylene in its side chain appear at 0.81ppm (Hm), 1.22ppm (Hl), 1.73ppm (Hk), 2.17ppm (Hg'), 2.49ppm (Hh'), and 4.51ppm (Hf), confirming the successful synthesis of PBI-PS-C.

[0024] Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in the solvent dimethyl sulfoxide to obtain a 5wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 70°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 50μm.

[0025] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 25wt% sulfuric acid solution for 10h, and drying it in a 60℃ oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane. Figure 1 As shown, under the action of a catalyst, bromhexane and 1,3-propane sultone are grafted onto the sulfonated polybenzimidazole polymer chain segment, and then protonated to obtain a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole.

[0026] Embodiment 2:

[0027] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3 parts by mass of sulfonated polybenzimidazole to 100 parts by mass of a solvent N,N-dimethylacetamide, stirring at 60° C. to completely dissolve, to obtain a sulfonated polybenzimidazole solution.

[0028] Step S2, preparing a hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole: adding 0.1 parts by mass of octane bromide, 0.1 parts by mass of 3-fluoro-1,3-propane sultone and 0.02 parts by mass of a catalyst 4-dimethylaminopyridine to a sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 70° C. to react for 8 hours, and after the reaction is completed, pouring the solution in the bottle into stirred acetone to precipitate, and then drying in an oven at 40° C. for 24 hours to obtain a hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole.

[0029] Step S3, preparing a hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole in the solvent N,N-dimethylacetamide to obtain an 8 wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 80°C until the solvent is completely dried and evaporated to obtain a hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole composite membrane. The thickness of the composite membrane is 40 μm.

[0030] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 20wt% hydrochloric acid solution for 12h, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0031] Embodiment 3:

[0032] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 6 parts by mass of sulfonated polybenzimidazole to 100 parts by mass of a solvent N,N-dimethylformamide, stirring at 60° C. to completely dissolve, to obtain a sulfonated polybenzimidazole solution.

[0033] Step S2, preparing a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole: adding 0.3 parts by mass of bromopropane, 0.3 parts by mass of 1,4-butanesulfonate and 0.04 parts by mass of catalyst ammonium formate to the sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 80°C and reacting for 9 hours, after the reaction is completed, pouring the solution in the bottle into stirring acetone, precipitating, and then drying in an oven at 60°C for 24 hours to obtain a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole.

[0034] Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in the solvent N,N-dimethylformamide to obtain a 10wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 90°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 60μm.

[0035] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 30wt% sulfuric acid solution for 11h, placing it in a 60°C oven and drying it completely to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0036] Embodiment 4:

[0037] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 5 parts by mass of sulfonated polybenzimidazole to 140 parts by mass of dimethyl sulfoxide as a solvent, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0038] Step S2, preparing a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole: adding 0.2 parts by mass of bromopentane, 0.2 parts by mass of 1,3-propane sultone and 0.02 parts by mass of catalyst sodium hydride to the sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 75°C and reacting for 11 hours, after the reaction is completed, pouring the solution in the bottle into stirring acetone, precipitating, and then drying in an oven at 55°C for 24 hours to obtain a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole.

[0039] Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in the solvent dimethyl sulfoxide to obtain a 7wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 80°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 55μm.

[0040] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 25wt% phosphoric acid solution for 10 hours, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0041] Embodiment 5:

[0042] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3 parts by mass of sulfonated polybenzimidazole to 100 parts by mass of dimethyl sulfoxide as a solvent, stirring at 60° C. until the polybenzimidazole is completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0043] Step S2, preparing a hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole: adding 0.4 parts by mass of ethyl bromide, 0.4 parts by mass of 1,4-butanesulfonate and 0.04 parts by mass of catalyst 4-dimethylaminopyridine to the sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 65°C to react for 12 hours, and after the reaction is completed, pouring the solution in the bottle into stirring acetone to precipitate, and then drying in an oven at 45°C for 24 hours to obtain a hydrophilic and hydrophobic double-comb type sulfonated polybenzimidazole.

[0044] Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in the solvent dimethyl sulfoxide to obtain a 6wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 70°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 45μm.

[0045] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 20wt% hydrochloric acid solution for 12h, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0046] Embodiment 6:

[0047] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 4 parts by mass of sulfonated polybenzimidazole to 120 parts by mass of a solvent N,N-dimethylacetamide, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0048] Step S2, preparing a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole: adding 0.2 parts by mass of hexyl bromide, 0.2 parts by mass of 1,3-propane sultone and 0.05 parts by mass of catalyst sodium hydride to the sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 80°C to react for 10 hours, and after the reaction is completed, pouring the solution in the bottle into stirred acetone to precipitate, and then drying in a 50°C oven for 24 hours to obtain a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole.

[0049] Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in the solvent N,N-dimethylacetamide to obtain a 5wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 80°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 55μm.

[0050] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 25wt% phosphoric acid solution for 11h, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0051] Embodiment 7:

[0052] A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for a vanadium battery comprises the following steps: Step S1, preparing a sulfonated polybenzimidazole solution: adding 5 parts by mass of sulfonated polybenzimidazole to 140 parts by mass of a solvent N,N-dimethylacetamide, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0053] Step S2, preparing a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole: adding 0.2 parts by mass of hexyl bromide, 0.3 parts by mass of 1,4-butanesulfonate and 0.05 parts by mass of catalyst 4-dimethylaminopyridine to the sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 70°C to react for 12 hours, and after the reaction is completed, pouring the solution in the bottle into stirred acetone to precipitate, and then drying in an oven at 55°C for 24 hours to obtain a hydrophilic and hydrophobic double-comb sulfonated polybenzimidazole.

[0054] Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: redissolve the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in the solvent N,N-dimethylacetamide to obtain a 6 wt% solution, pour the solution onto a clean glass plate, apply it with a scraper, and increase the temperature to 70°C until the solvent is completely dried and evaporated to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane, the thickness of the composite membrane is 50 μm.

[0055] Step S4, preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane: soaking the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane in a 30wt% sulfuric acid solution for 10 hours, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb type amphoteric composite membrane.

[0056] Comparative Example 1 Step S1, preparing a sulfonated polybenzimidazole solution: adding 4 parts by mass of sulfonated polybenzimidazole to 120 parts by mass of dimethyl sulfoxide as a solvent, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution.

[0057] Step S2, preparing a blank sulfonated polybenzimidazole composite membrane: pouring the sulfonated polybenzimidazole solution onto a clean glass plate, coating it with a scraper, and raising the temperature to 70° C. until the solvent is completely dried and evaporated to obtain a blank sulfonated polybenzimidazole composite membrane having a thickness of 50 μm.

[0058] Comparative Example 2 Consistent with Example 1, no bromohexane is added in step S2.

[0059] Comparative Example 3 Consistent with Example 1, 1,3-propane sultone was not added in step S2.

[0060] 1. Mechanical properties test The mechanical properties of the films of the examples and comparative examples were measured using a SHIMADZUAG-I1KN universal testing machine. The film samples to be tested were cut into 5 mm×50 mm specifications and stretched at a stretching speed of 100 mm / min for mechanical property testing.

[0061] 2. The membrane is assembled into a battery stack for battery testing The embodiment and comparative example membranes were assembled into a stack for testing, and the coulombic efficiency, voltage efficiency and energy efficiency were tested and recorded under the same test conditions. The test results are shown in the following table: Table 1: Battery performance test table of battery stacks assembled using the membranes of the embodiments and the comparative examples

[0062] It can be seen that comparative example 2 has higher tensile strength and voltage efficiency than comparative example 1, indicating that the hydrophilic sulfonic acid group side chain with ionic characteristics is introduced into the sulfonated polybenzimidazole polymer segment of the present invention, which can form an ionic cross-linked structure with the imidazole group of the PBI main chain, improve the mechanical properties of the membrane, and in addition, the membrane proton transmission density can be increased to further improve the voltage and energy efficiency of the vanadium battery. Comparative example 3 has a higher coulomb efficiency and voltage efficiency than comparative example 1. The present invention introduces a hydrophobic side chain into the sulfonated polybenzimidazole polymer segment, which can hinder the shuttle of vanadium ions through the steric hindrance effect, thereby improving the coulomb efficiency of the vanadium battery. In addition, the hydrophobic side chain improves the aggregation of the hydrophobic segment, thereby improving the morphology of microphase separation, so that the three-dimensional ion channel can significantly improve the ion mobility and transmission efficiency under low water absorption, thereby improving the voltage and energy efficiency of the vanadium battery. The embodiment has higher tensile strength and stack efficiency than comparative example 1, which is due to the beneficial effects of the hydrophobic side chain and the hydrophilic side chain on the hydrophilic and hydrophobic double comb type amphiphilic composite membrane of the present invention.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A hydrophilic and hydrophobic double-comb type amphoteric composite membrane for vanadium batteries, Features: The following steps are involved: Step S1, preparing a sulfonated polybenzimidazole solution: adding 3-6 parts by mass of sulfonated polybenzimidazole to 100-150 parts by mass of a solvent, stirring at 60° C. until completely dissolved, to obtain a sulfonated polybenzimidazole solution; Step S2, preparing a hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole: adding 0.1-0.4 parts by mass of bromoalkane, 0.1-0.4 parts by mass of sultone and 0.02-0.0.05 parts by mass of a catalyst to a sulfonated polybenzimidazole solution, stirring and mixing evenly, heating to 60-80° C. and reacting for 8-12 hours, and after the reaction is completed, pouring the solution in the bottle into acetone in a stirring state to precipitate, and then drying in an oven at 40-60° C. for 24 hours to obtain a hydrophilic and hydrophobic double comb type sulfonated polybenzimidazole; Step S3, preparing a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane: re-dissolving the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole in a solvent to obtain a 5-10wt% solution, pouring the solution onto a clean glass plate, coating with a scraper, and raising the temperature to 70-90° C. until the solvent is completely dried and volatilized to obtain a hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane; Step S4, preparing a hydrophilic-hydrophobic double-comb composite membrane: soaking the hydrophilic-hydrophobic double-comb sulfonated polybenzimidazole composite membrane in a 20-30wt% acid solution for 10-12h, and drying it completely in a 60°C oven to obtain a hydrophilic-hydrophobic double-comb composite membrane.

2. A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for vanadium batteries as claimed in claim 1, Features: The solvent in steps S1 and S3 is any one of dimethyl sulfoxide, N,N-dimethylacetamide and N,N-dimethylformamide.

3. A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for vanadium batteries as claimed in claim 1, Features: In step S2, the brominated alkane is any one of octyl bromide, hexyl bromide, pentane bromide, propyl bromide and ethyl bromide.

4. A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for vanadium batteries as claimed in claim 1, Features: In step S2, the sultone is any one of 1,3-propane sultone, 3-fluoro-1,3-propane sultone and 1,4-butane sultone.

5. A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for vanadium batteries as claimed in claim 1, Features: In step S2, the catalyst is any one of 4-dimethylaminopyridine, ammonium formate and sodium hydride.

6. A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for vanadium batteries as claimed in claim 1, Features: In step S3, the thickness of the hydrophilic-hydrophobic double-comb type sulfonated polybenzimidazole composite membrane is 40-60 μm.

7. A method for preparing a hydrophilic-hydrophobic double-comb type amphoteric composite membrane for vanadium batteries as claimed in claim 1, Features: The acid solution in step S4 is at least one of a sulfuric acid solution, a hydrochloric acid solution, and a phosphoric acid solution.

8. A hydrophilic and hydrophobic double-comb type amphoteric composite membrane for vanadium batteries, Features: The composite membrane is prepared by the method for preparing a hydrophilic-hydrophobic double-comb amphoteric composite membrane for vanadium batteries as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Polybenzimidazole with sulfonated side chain and preparation method thereof

    CN103073719A

  • Side-chain alkyl sulfonated polybenzimidazole ion exchange film and preparation method thereof

    CN108400362A

  • Hydrophobic side chain-modified alkyl sulfonated polybenzimidazole amphoteric membrane and preparation method thereof

    CN108878936A