Sodium silicate modified carbon-based composite wave-absorbing material as well as preparation method and application thereof

Through the preparation of sodium silicate modified carbon-based composite materials, the heterogeneous interface and microstructure design are used to solve the skin effect problem caused by the high conductivity of carbon-based materials, significantly improve the electromagnetic wave absorption performance, and achieve high efficiency and low efficiency Cost electromagnetic wave absorption effect.

CN118900552APending Publication Date: 2024-11-05HARBIN INST OF TECH AT WEIHAI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981788.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing carbon-based materials have skin effects due to their high conductivity, which limits their absorption performance on electromagnetic waves. The microstructure and impedance matching characteristics of pure material cannot meet the needs of high-performance absorbing materials.

Method used

Sodium silicate is used as a modifier to compound glucose, and through hydrothermal reaction and high-temperature carbonization treatment, heterogeneous interfaces and microstructures are constructed, impedance matching and polarization loss of the material are optimized, and electromagnetic wave absorption performance is improved.

Benefits of technology

The excellent electromagnetic wave absorption performance of composite materials is achieved, and the absorption performance is significantly improved by regulating the addition of sodium silicate. It is low in cost, simple in process, green and environmentally friendly, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900552A_ABST
    Figure CN118900552A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wave-absorbing materials, in particular to a sodium silicate modified carbon-based composite wave-absorbing material and a preparation method and application thereof. The preparation method comprises the following steps: adding sodium silicate and glucose into water, uniformly mixing, evaporating a solvent to obtain a gelatinous substance, then carrying out hydrothermal reaction, and then carrying out high-temperature carbonization treatment to obtain the sodium silicate modified carbon-based composite wave-absorbing material. The preparation method of the sodium silicate modified carbon-based composite wave-absorbing material, provided by the invention, has the advantages of low cost, simple process, environment friendliness, easily available raw materials, easiness in large-scale production and the like. By adjusting the ratio and the preparation process of the composite material, the crystalline phase composition, the microstructure and the dielectric property of the composite material can be optimized, so that efficient absorption of electromagnetic waves is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of absorbing materials, and in particular to a sodium silicate-modified carbon-based composite absorbing material and a preparation method and application thereof. Background Art

[0002] With the rapid development and popularization of electronic devices, they have become an indispensable part of people's lives and work. However, the electromagnetic radiation generated by them will have adverse effects on human health, electronic equipment, instruments and meters, communication signals, etc., and even threaten military security. Absorbing materials solve the above problems by absorbing electromagnetic waves. Therefore, it is particularly important to develop efficient absorbing materials to control and reduce electromagnetic radiation problems.

[0003] In recent years, researchers have reported various electromagnetic wave absorbing materials, including carbon materials, magnetic materials, semiconductor materials and polymer materials. Pure material has limited scattering and multiple reflection capabilities of electromagnetic waves due to its simple microstructure. Impedance matching characteristics and loss capacity also make these materials unable to meet the demand for high-performance absorbing materials. Glucose, as a carbon-containing precursor used to prepare carbon sources, is an ideal candidate for electromagnetic wave absorbing materials due to its abundant sources and multiple functional groups. However, the high conductivity of carbon-based materials induces skin current, causing strong reflection of electromagnetic waves on the surface, which is not conducive to further consumption of electromagnetic waves. Therefore, the rational regulation of the electromagnetic parameters and microstructure design of materials has become the key research direction of current researchers. Summary of the invention

[0004] The purpose of the present invention is to provide a sodium silicate modified carbon-based composite absorbing material and its preparation method and application, so as to solve the problems existing in the above-mentioned prior art. The present invention uses carbon-containing precursor glucose as a carbon matrix, which has rich oxygen-containing functional groups inside, providing the material with conduction loss and dipole polarization loss. Sodium silicate is used as a modifier, because it has a low dielectric constant, good chemical stability and durability, and after being composited with carbon materials, it can improve the skin effect brought about by the high conductivity of the carbon material itself, so that its impedance matching is optimized. The alkaline environment generated by sodium silicate dissolving in water is used to catalyze the degradation reaction of glucose. After hydrothermal reaction and high-temperature carbonization treatment, a special heterogeneous interface and microstructure are constructed inside the composite material. The interface and structural design are achieved by controlling the material ratio. The composite material exhibits excellent absorbing performance by utilizing the strong conductivity loss of the carbon material itself, combining the polarization loss brought about by various heterogeneous interfaces, and the internal structural design. The dielectric properties, components and morphology of the composite material can be simply regulated by controlling the amount of sodium silicate added. This method also has the advantages of simple preparation process, green environmental protection and low cost.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention is to provide a method for preparing a sodium silicate modified carbon-based composite absorbing material, the steps comprising: adding sodium silicate and glucose into water, mixing evenly, evaporating the solvent to obtain a colloidal substance, then performing a hydrothermal reaction, and then performing a high-temperature carbonization treatment to obtain the sodium silicate modified carbon-based composite absorbing material.

[0007] Preferably, the dosage ratio of the sodium silicate to glucose is 1-10 mmol:10 g; the dosage of the water is based on the amount that can completely dissolve the sodium silicate and glucose.

[0008] Preferably, the uniform mixing is performed by first stirring and then ultrasonic dispersion.

[0009] Preferably, the evaporation of the solvent is performed by heating at a temperature of 60-80° C., and the mixture is heated while being stirred until a colloid-like substance is obtained.

[0010] Preferably, the temperature of the hydrothermal reaction is 160-200° C. and the time is 22-26 h.

[0011] Preferably, the specific operation steps of the high temperature carbonization treatment include: heating to 600-800° C. at a heating rate of 2° C. / min in a nitrogen atmosphere, and treating for 2 hours.

[0012] The present invention utilizes the property that glucose and sodium silicate are easily soluble in water, and realizes uniform mixing of the two by ultrasonic dispersion and solvent evaporation. In addition, the alkaline environment provided by sodium silicate promotes catalytic degradation of glucose during heating. The degradation product decomposes during high-temperature carbonization and further reacts with sodium silicate to generate fibrous sodium carbonate. The presence of low-dielectric sodium carbonate / sodium silicate material optimizes the impedance matching of carbon materials, and charges accumulate at the heterogeneous interface under the alternating electric field, resulting in interface and dipole polarization, so that the composite material exhibits excellent electromagnetic wave absorption performance.

[0013] The second technical solution of the present invention is to provide a sodium silicate-modified carbon-based composite absorbing material prepared according to the above preparation method.

[0014] The third technical solution of the present invention is to provide an application of the above-mentioned sodium silicate modified carbon-based composite absorbing material in shielding electromagnetic radiation.

[0015] The present invention mainly improves the wave absorbing performance of carbon-based materials from the following aspects:

[0016] (1) Glucose, as a carbon-containing precursor, provides a carbon source, which causes the electromagnetic waves to be consumed in the form of conduction losses. At the same time, the abundant oxygen-containing functional groups inside it can act as polarization centers to induce dipole polarization.

[0017] (2) Glucose is catalyzed to degrade in the alkaline environment provided by sodium silicate to generate small molecular products. After hydrothermal treatment and high-temperature carbonization, carbon-containing gases such as CO2 and CO are released, leaving vacancies or defects in the carbon matrix, resulting in uneven charge distribution in the material and enhancing the electromagnetic wave loss caused by the polarization effect. The introduction of low-dielectric sodium silicate adjusts the impedance matching of the carbon material, which is conducive to the electromagnetic wave loss caused by entering the material.

[0018] (3) During the high-temperature carbonization process, the small molecular degradation products of glucose decompose, and the released carbon-containing gas (CO2 / CO) further reacts with sodium silicate to form fibrous sodium carbonate. At this time, there are multiple heterogeneous interfaces (sodium silicate-carbon, sodium carbonate-carbon, sodium silicate-sodium carbonate, etc.) inside the composite material. Under the action of electromagnetic waves, induced charges accumulate at the heterogeneous interfaces, resulting in interface polarization. The differences in dielectric, lattice constant and conductivity between different phases produce different charge accumulation phenomena, which respond to electromagnetic waves in different frequency bands. In addition, the complex microstructure formed by the interweaving of sodium carbonate fibers causes multiple reflections of the incident electromagnetic waves, which prolongs the transmission path of the electromagnetic waves and enhances the wave absorption effect of the composite material.

[0019] The present invention discloses the following technical effects:

[0020] The present invention prepares a sodium silicate-modified carbon-based composite absorbing material by combining solvent evaporation, hydrothermal treatment and high-temperature carbonization process. The present invention utilizes the alkaline environment provided by sodium silicate to promote the catalytic degradation reaction of glucose during the heating process. During the high-temperature carbonization process, the degradation products of glucose decompose to release carbon-containing gas (CO2 / CO) and react with sodium silicate to generate fibrous sodium carbonate. At this time, there are multiple heterogeneous interfaces (sodium silicate-carbon, sodium carbonate-carbon, sodium silicate-sodium carbonate, etc.) inside the composite material. Under the action of electromagnetic waves, induced charges accumulate at the interface to generate interface polarization. At the same time, the sodium carbonate fibers are interwoven vertically and horizontally to cause multiple reflections of the incident electromagnetic wave, extend the transmission path of the electromagnetic wave, and enhance the wave absorbing effect of the composite material. The introduction of sodium silicate improves the impedance matching of the carbon material, and the synergistic effect of interface polarization, dipole polarization and conduction loss enables the composite material to have excellent electromagnetic wave absorption performance.

[0021] The sodium silicate modified carbon-based composite absorbing material prepared by the present invention has a regular change in the microscopic morphology of the composite material under different sodium silicate addition amounts, and the absorbing performance is significantly enhanced. The quality of the absorbing performance can be reflected by the reflection loss (RL) value. It can be found that when sodium silicate is not added, the composite material has poor absorbing performance, and the maximum reflection loss of the absorber is -22.38dB when the thickness is 1.6mm. When 1mmol of sodium silicate is added, the maximum reflection loss of the composite material increases to -40.79dB, and the corresponding frequency is 15.76GHz. When the sodium silicate content is 3mmol, the maximum reflection loss at 5.68GHz increases to -44.69dB. When the sodium silicate content is 5mmol, because of its heterogeneous interface composed of multiple phases, and this addition makes the conduction loss and polarization loss achieve excellent matching, which jointly promotes the improvement of its electromagnetic wave absorption performance, and achieves a reflection loss value of -54.32dB at 5.68GHz at a thickness of 4.9mm. When the sodium silicate content reaches 10mmol, due to the introduction of excessive sodium silicate, the proportion of effective absorbing components decreases. When the thickness is 6mm, the minimum reflection loss at 13.67GHz is only -35.93dB.

[0022] Glucose, as a carbon-containing precursor, has a wide source and a relatively low price. It can be used to prepare carbon materials through processes such as pyrolysis and high-temperature carbonization, and has great application potential in the field of wave absorption. Sodium silicate, as an important industrial raw material, is widely used in papermaking, dyes, construction, glass and other fields because of its mature production process and low price. Sodium silicate can be used as an impedance matching regulator to optimize and control the dielectric constant of high dielectric materials by utilizing its low dielectric properties. Sodium silicate and glucose are both relatively environmentally friendly materials with a wide source and good biodegradability. The preparation method of a sodium silicate-modified carbon-based composite wave absorbing material provided by the present invention has the advantages of low cost, simple process, green environmental protection, easy availability of raw materials, and easy large-scale production. By adjusting the ratio and preparation process of the composite material, the crystal phase composition, micromorphology and dielectric properties of the composite material can be optimized, thereby achieving efficient absorption of electromagnetic waves. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1The following are scanning electron microscope (SEM) images of the materials obtained in Comparative Example 1 and Examples 1-4, wherein (a) is the SEM image of the material obtained in Comparative Example 1, and (b)-(e) are the SEM images of the composite absorbing materials prepared in Examples 1-4, respectively;

[0025] Figure 2 This is a SEM image of the material obtained after hydrothermal reaction in Example 3;

[0026] Figure 3 Schematic diagram of the wave absorbing performance of the sodium silicate modified carbon-based composite wave absorbing material prepared in Examples 1-8 in the frequency range of 2-18 GHz, wherein (a)-(h) are schematic diagrams of the wave absorbing performance of the composite wave absorbing materials prepared in Examples 1-8, respectively;

[0027] Figure 4 Schematic diagram of the wave absorbing performance of the material obtained in Comparative Example 1 in the frequency range of 2-18 GHz. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] The raw materials used in the examples and comparative examples of the present invention can all be purchased from the market, and the instruments and equipment used are all commonly used instruments and equipment in the art.

[0034] Example 1

[0035] Dissolve 10 g of glucose and 1 mmol of sodium silicate nonahydrate in 25 mL of deionized water, and then continue stirring for 1 hour. After the stirring is completed, ultrasonic dispersion is performed to obtain a sodium silicate-glucose mixed solution.

[0036] The sodium silicate-glucose mixed solution was heated and stirred at 70°C, and a gelatinous substance was obtained after 14 hours;

[0037] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 180°C to obtain a black solid after 24 hours of reaction.

[0038] The black solid was placed in a tube furnace, heated to 700° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0039] Example 2

[0040] 10 g of glucose and 3 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 h. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0041] The sodium silicate-glucose mixed solution was heated and stirred at 70°C, and a gelatinous substance was obtained after 14 hours;

[0042] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 180°C to obtain a black solid after 24 hours of reaction.

[0043] The black solid was placed in a tube furnace, heated to 700° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0044] Example 3

[0045] 10 g of glucose and 5 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 h. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0046] The sodium silicate-glucose mixed solution was heated and stirred at 70°C, and a gelatinous substance was obtained after 14 hours;

[0047] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 180°C to obtain a black solid after 24 hours of reaction.

[0048] The black solid was placed in a tube furnace, heated to 700° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0049] Example 4

[0050] 10 g of glucose and 10 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 hour. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0051] The sodium silicate-glucose mixed solution was heated and stirred at 70°C, and a gelatinous substance was obtained after 14 hours;

[0052] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 180°C to obtain a black solid after 24 hours of reaction.

[0053] The black solid was placed in a tube furnace, heated to 700° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0054] Example 5

[0055] 10 g of glucose and 5 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 h. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0056] The sodium silicate-glucose mixed solution was heated and stirred at 70°C, and a gelatinous substance was obtained after 14 hours;

[0057] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 180°C to obtain a black solid after 24 hours of reaction.

[0058] The black solid was placed in a tube furnace, heated to 600° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0059] Example 6

[0060] 10 g of glucose and 5 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 h. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0061] The sodium silicate-glucose mixed solution was heated and stirred at 70°C, and a gelatinous substance was obtained after 14 hours;

[0062] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 180°C to obtain a black solid after 24 hours of reaction.

[0063] The black solid was placed in a tube furnace, heated to 800° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0064] Example 7

[0065] 10 g of glucose and 5 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 h. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0066] The sodium silicate-glucose mixed solution was heated at 80°C while stirring, and a gelatinous substance was obtained after 14 hours;

[0067] The colloid substance was placed in a high pressure reactor and subjected to a hydrothermal reaction at 160°C to obtain a black solid after 26 hours of reaction.

[0068] The black solid was placed in a tube furnace, heated to 700° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0069] Example 8

[0070] 10 g of glucose and 5 mmol of sodium silicate nonahydrate were dissolved in 25 mL of deionized water, and then stirred for 1 h. After the stirring was completed, ultrasonic dispersion was performed to obtain a sodium silicate-glucose mixed solution;

[0071] The sodium silicate-glucose mixed solution was heated at 60°C while stirring, and a gelatinous substance was obtained after 14 hours;

[0072] The colloid substance was placed in a high-pressure reactor and subjected to a hydrothermal reaction at 200°C. After 22 hours of reaction, a black solid was obtained.

[0073] The black solid was placed in a tube furnace, heated to 700° C. at a heating rate of 2° C. / min under a nitrogen atmosphere, and reacted for 2 h to obtain a sodium silicate-modified carbon-based composite absorbing material.

[0074] Comparative Example 1

[0075] Compared with Example 1, the only difference is that sodium silicate nonahydrate is not added.

[0076] Effect verification

[0077] 0.035 g of the materials obtained in Examples 1-8 and Comparative Example 1 were weighed respectively, and then mixed with 0.065 g of paraffin wax (melted by high temperature heating), and then pressed into absorbing sample rings with an outer diameter of 7 mm and an inner diameter of 3 mm using a mold.

[0078] The sample rings containing the materials obtained in Examples 1-8 and Comparative Example 1 prepared above were tested using a vector network analyzer of model Agilent N5245A (frequency range of 2-18 GHz). After obtaining the electromagnetic parameters of the samples, the electromagnetic parameters were converted into the reflection loss constant of the material by calculation. The microwave absorption test results are shown in Table 1.

[0079] Table 1 Microwave absorption test results

[0080]

[0081] Figure 1 The following are scanning electron microscope (SEM) images of the materials obtained in Comparative Example 1 and Examples 1-4, wherein (a) is the SEM image of the material obtained in Comparative Example 1, and (b)-(e) are the SEM images of the composite absorbing materials prepared in Examples 1-4, respectively. The addition of sodium silicate makes the solution alkaline, and the glucose undergoes catalytic degradation to make the surface rough. During the high-temperature carbonization process, the degradation products decompose and release carbon-containing gases (such as CO2, CO, etc.), which further react with sodium silicate to generate fibrous sodium carbonate. The degree of glucose degradation and the amount of sodium carbonate generated are proportional to the amount of sodium silicate added. Therefore, Figure 1 In (b)-(e), as the amount of sodium silicate added increases, the number of sodium carbonate fibers on the carbon surface increases significantly. Figure 1 In (d), it can be seen that there is granular sodium silicate. This is because the alkalinity in the solution is weak, the number of glucose degradation products is small, and the small amount of gas released cannot react with the excess sodium silicate to convert into sodium carbonate. Therefore, there are two types of crystals, sodium silicate and sodium carbonate, in which sodium silicate is granular and sodium carbonate is fibrous crystals. Sodium silicate / sodium carbonate is attached to the surface of the carbon matrix, which increases the contact area between the material and the electromagnetic wave. The interwoven fibers make the electromagnetic wave propagation more tortuous, which helps the material absorb electromagnetic waves. In contrast, since no sodium silicate is added to Comparative Example 1, the resulting material presents a smooth and flat surface.

[0082] Figure 2 This is a SEM image of the material obtained after hydrothermal reaction in Example 3. Figure 2 It can be seen that the degradation of glucose makes the surface rough. Since no particles / fibers can be observed attached to the surface, it can be determined that the crystallization of sodium silicate and sodium carbonate occurs during the high-temperature carbonization process.

[0083] Figure 3 The schematic diagram of the wave absorption performance of the sodium silicate modified carbon-based composite wave absorbing material prepared in Examples 1-8 in the frequency range of 2-18 GHz, and (a)-(h) in the figure are schematic diagrams of the wave absorption performance of the composite wave absorbing material prepared in Examples 1-8, respectively. Figure 3 It can be seen that the minimum reflection loss of the composite absorbing material prepared in Example 1 is -40.79 dB at 15.76 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 2 is -44.69 dB at 8.80 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 3 is -54.32 dB at 5.68 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 4 is -35.93 dB at 13.67 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 5 is -47.64 dB at 5.04 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 6 is -41.93 dB at 16.88 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 7 is -40.01 dB at 5.6 GHz; the minimum reflection loss of the composite absorbing material corresponding to Example 8 is -52.06 dB at 13.6 GHz. The sodium silicate modified carbon-based composite wave-absorbing material provided by the present invention has a strong ability to absorb electromagnetic waves and can effectively reduce the reflection and interference of electromagnetic waves.

[0084] Figure 4 This is a schematic diagram of the wave absorption performance of the material obtained in Comparative Example 1 in the frequency range of 2-18 GHz. Figure 4 It can be seen that in Comparative Example 1, no sodium silicate is added, and the minimum reflection loss of the obtained material is -22.38 dB, which is much greater than the minimum reflection loss of the materials obtained in the above Examples 1-8, indicating that the addition of sodium silicate for modification can effectively improve the absorption performance of the absorbing material, and the absorption frequency band can be regulated by adjusting the amount of sodium silicate added.

[0085] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a sodium silicate-modified carbon-based composite absorbing material, characterized in that the steps include: Sodium silicate and glucose are added into water, mixed evenly, the solvent is evaporated to obtain a colloidal substance, and then a hydrothermal reaction is carried out, and then a high-temperature carbonization treatment is carried out to obtain a sodium silicate-modified carbon-based composite absorbing material.

2. The method for preparing the sodium silicate modified carbon-based composite absorbing material according to claim 1, characterized in that: The dosage ratio of the sodium silicate to glucose is 1-10 mmol: 10 g; the dosage of the water is based on the amount of water that can completely dissolve the sodium silicate and glucose.

3. The method for preparing the sodium silicate modified carbon-based composite absorbing material according to claim 1, characterized in that: The uniform mixing is performed by first stirring and then ultrasonically dispersing.

4. The method for preparing the sodium silicate modified carbon-based composite absorbing material according to claim 1, characterized in that: The evaporating solvent is heated and evaporated at a temperature of 60-80° C., and the solvent is heated and stirred until a colloid substance is obtained.

5. The method for preparing the sodium silicate modified carbon-based composite absorbing material according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 160-200° C. and the time is 22-26 hours.

6. The method for preparing the sodium silicate modified carbon-based composite absorbing material according to claim 1, characterized in that: The specific operation steps of the high temperature carbonization treatment include: heating to 600-800° C. at a heating rate of 2° C. / min in a nitrogen atmosphere, and treating for 2 hours.

7. A sodium silicate-modified carbon-based composite absorbing material prepared according to the preparation method according to any one of claims 1 to 6.

8. Use of the sodium silicate modified carbon-based composite absorbing material according to claim 7 in shielding electromagnetic radiation.