Conductor manufacturing method, electromagnetic wave shield manufacturing method, and conductor
By using a combination of heating and light irradiation to cure metal salt or metal complex inks on a substrate, a conductive film with excellent abrasion resistance is formed, solving the problem of insufficient abrasion resistance on the surface of conductive film laminates and achieving electromagnetic wave shielding effect.
Patent Information
- Application Number
- CN202380028300.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-05
Smart Images

Figure BDA0005047020450000351 
Figure BDA0005047020450000361 
Figure BDA0005047020450000371
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a conductor, a method for manufacturing an electromagnetic wave shielding body, and the conductor. Background Art
[0002] Semiconductor devices and the like may be hindered from operating normally due to interference caused by electromagnetic waves, resulting in the possibility of failure. In addition, when semiconductor devices and the like generate electromagnetic waves, the electromagnetic waves may interfere with other semiconductor devices or electronic parts, also possibly hindering normal operation.
[0003] Therefore, in order to avoid interference caused by electromagnetic waves from other electronic devices or to avoid interference caused by electromagnetic waves to other electronic devices, it is necessary to shield electromagnetic waves. As a technology for shielding electromagnetic waves, it is known that there is a technology of covering the shielding object, i.e., a semiconductor device, by a shielding can. However, the shielding can has problems such as thick film thickness, heavy and small degree of freedom in design, and a technology to replace the shielding can is needed. For example, it is known that an insulating film and an electromagnetic wave shielding layer are stacked on a printed circuit board on which a semiconductor device is installed to form an electromagnetic wave shielding body.
[0004] For example, Patent Document 1 discloses a technique related to a method for manufacturing an electromagnetic wave shielding film, which includes an insulating film forming stage of forming an insulating film on a first release film and a metal pattern forming stage of printing a metal pattern on the insulating film.
[0005] Previous technical literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-126230 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] The present inventors referred to the technology described in Patent Document 1 and found that in order to make the thickness of the conductive film thicker, the conductive film is repeatedly formed to produce a conductive film stack. As a result, the abrasion resistance of the surface of the obtained conductive film stack is insufficient, and there is room for improvement.
[0010] In view of the above-mentioned actual situation, an object of the present invention is to provide a method for producing a conductor capable of forming a conductive film having excellent abrasion resistance. In addition, an object of the present invention is to provide a method for producing an electromagnetic shield and a conductor.
[0011] Means for solving technical problems
[0012] As a result of intensive studies on the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by the following configuration.
[0013] [1] A method for manufacturing a conductor, comprising: an ink preparation step of preparing a first ink containing at least a metal salt or a metal complex and a second ink containing at least a metal salt or a metal complex; step 1 of forming a first coating film on a substrate using the first ink, and then subjecting the first coating film to a first curing treatment selected from the group consisting of a heat treatment and a light irradiation treatment to form a first conductive film; and step 2 of forming a second coating film on the first conductive film using the second ink, and then subjecting the second coating film to a second curing treatment selected from the group consisting of a heat treatment and a light irradiation treatment to form a second conductive film, wherein the method for manufacturing a conductor satisfies at least one of the following formulas (1) and (2).
[0014] [2] The method for producing a conductor according to [1], wherein:
[0015] The first ink and the second ink are the same.
[0016] [3] The method for producing a conductor according to [1] or [2], wherein:
[0017] In the step 1, the heating treatment is performed as the first curing treatment, and in the step 2, the heating treatment is performed as the second curing treatment.
[0018] [4] The method for producing a conductor according to [1] or [2], wherein:
[0019] In the step 1, the light irradiation treatment is performed as the first curing treatment, and in the step 2, the light irradiation treatment is performed as the second curing treatment.
[0020] [5] The method for producing a conductor according to [1] or [2], wherein:
[0021] In the step 1, both the heating treatment and the light irradiation treatment are performed as the first curing treatment, and in the step 2, both the heating treatment and the light irradiation treatment are performed as the second curing treatment.
[0022] [6] The method for producing a conductor according to any one of [1] to [5], wherein:
[0023] The thickness of the second coating film formed in the step 2 is smaller than the thickness of the first coating film formed in the step 1.
[0024] [7] A method for manufacturing a conductor according to any one of [1] to [6], which also includes a step 3 of forming an insulating film on a substrate to produce a substrate with an insulating film, wherein the above-mentioned step 1 is a step of forming the above-mentioned first conductive film on the above-mentioned insulating film of the above-mentioned substrate with an insulating film produced by the above-mentioned step 3.
[0025] [8] A method for producing an electromagnetic wave shield, comprising the step of forming a conductive film on a substrate according to the method for producing a conductor described in any one of [1] to [7].
[0026] [9] The method for manufacturing an electromagnetic shield according to [8], wherein:
[0027] The base material is an electronic substrate on which electronic components are mounted.
[0028]
[10] A conductor produced by the method for producing a conductor according to any one of [1] to [7].
[0029] Effects of the Invention
[0030] According to the present invention, a method for producing a conductor capable of forming a conductive film having excellent abrasion resistance can be provided. In addition, according to the present invention, a method for producing an electromagnetic shield and a conductor can be provided. DETAILED DESCRIPTION
[0031] Hereinafter, the present invention will be described in detail.
[0032] The following description is made based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0033] In this specification, the numerical range represented by "to" refers to a range that includes the numerical values recorded before and after "to" as the lower limit and the upper limit. In the numerical range recorded in stages in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Furthermore, in the numerical range recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the value shown in the embodiment.
[0034] In this specification, each component may use a single substance corresponding to each component, or may use two or more substances. Here, when two or more substances are used for each component, unless otherwise specified, the content of the component refers to the total content of the two or more substances.
[0035] In the present specification, a combination of two or more preferred aspects is a more preferred aspect.
[0036] In the present specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0037] In this specification, "g" means "mass g".
[0038] In this specification, "pL" means "picoliter". 1pL is equal to 10 -12 L.
[0039] In this specification, angles represented by specific numerical values and expressions such as "parallel", "perpendicular", and "orthogonal" include an error range generally allowed in the technical field unless otherwise specified.
[0040] In this specification, "conductive" means a volume resistivity of less than 10 8 Properties of Ωcm.
[0041] [Method for producing an electrical conductor]
[0042] The method for producing an electric conductor of the present invention (hereinafter also referred to as "the present production method") comprises:
[0043] An ink preparation step of preparing a first ink containing at least a metal salt or a metal complex and a second ink containing at least a metal salt or a metal complex;
[0044] Step 1, after forming a first coating film on a substrate using a first ink, subjecting the first coating film to a first curing treatment of at least one selected from the group consisting of a heating treatment and a light irradiation treatment to form a first conductive film; and
[0045] In step 2, after forming a second coating film on the first conductive film using the second ink, the second coating film is subjected to a second curing treatment of at least one selected from the group consisting of a heat treatment and a light irradiation treatment to form a second conductive film.
[0046] The present production method satisfies at least one of the equations (1) and (2).
[0047] Formula (1) 1.2≤{(T2-23)×t2 / L2} / {(T1-23)×t1 / L1}
[0048] Formula (2) 2.0≤(E2 / L2) / (E1 / L1)
[0049] In the formula, L1 and L2 represent the thickness (μm) of the first coating film and the second coating film, respectively.
[0050] T1 and T2 respectively represent heating temperatures (° C.) of the heating treatments performed as the first curing treatment and the second curing treatment.
[0051] t1 and t2 respectively represent the heating time (minutes) of the heating treatments performed as the first curing treatment and the second curing treatment.
[0052] E1 and E2 represent the exposure doses (J / cm2) of the light irradiation treatments performed as the first curing treatment and the second curing treatment, respectively. 2 ).
[0053] That is, when the present manufacturing method satisfies formula (1), a heat treatment is performed as the first curing treatment of step 1, and a heat treatment is performed as the second curing treatment of step 2. Also, when the present manufacturing method satisfies formula (2), a light irradiation treatment is performed as the first curing treatment of step 1, and a light irradiation treatment is performed as the second curing treatment of step 2.
[0054] According to the present production method, a conductor having a conductive film having excellent abrasion resistance on the surface can be produced. The details of the reason are not clear, but the present inventors speculate as follows.
[0055] In the present manufacturing method, an ink containing a metal salt or a metal complex is used, so that in the first conductive film and the second conductive film formed, the metal component is difficult to granulate, and a conductive film with high continuity is formed, and as a result, it is estimated that the abrasion resistance is improved. In addition, it is estimated that when at least one of the formulas (1) and (2) is satisfied, more energy per unit film thickness is given to the coating film of the conductive ink in the second curing treatment compared to the first curing treatment, thereby promoting the reduction reaction of the metal salt or metal complex contained in the coating film, so that a conductive film with higher continuity and excellent abrasion resistance is formed on the surface side.
[0056] Hereinafter, each step included in the present production method will be described in detail.
[0057] 〔Ink preparation process〕
[0058] The ink preparation step is a step of preparing the first ink and the second ink.
[0059] The first ink and the second ink (hereinafter, these are also collectively referred to as "conductive ink") both contain at least a metal salt or a metal complex.
[0060] The conductive ink is, for example, an ink composition in which at least one selected from the group consisting of metal salts and metal complexes is dissolved in a solvent, and is used to form a film having conductivity (ie, a conductive film).
[0061] The "preparation" in the ink preparation step includes not only the act of preparing the conductive ink by synthesizing and / or blending the constituent components of the conductive ink containing the metal salt or the metal complex, but also the act of obtaining the conductive ink containing the metal salt or the metal complex by purchasing, etc.
[0062] The first ink and the second ink may be the same or different, preferably the same. In addition, the two inks being the same means that the types and contents of the components contained in the inks are the same, and the two inks being different means that at least one of the types and contents of the components contained in the inks is different from each other.
[0063] The first ink and the second ink can also be prepared by preparing a conductive ink containing a metal salt or a metal complex and then dividing the prepared conductive ink. Alternatively, the first ink and the second ink may be prepared separately.
[0064] <Conductive Ink>
[0065] The conductive ink will be described below.
[0066] The conductive ink contains at least a metal salt or a metal complex.
[0067] Examples of the metal constituting the metal salt or metal complex include silver, copper, gold, aluminum, magnesium, tungsten, molybdenum, zinc, nickel, iron, platinum, tin, copper, and lead. Among them, from the perspective of better conductivity, the metal constituting the metal salt or metal complex preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium, and copper, more preferably includes at least one of silver and copper, and even more preferably includes silver.
[0068] The content of the metal contained in the conductive ink is preferably 1 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 20% by mass, based on the total mass of the conductive ink, in terms of metal element.
[0069] The content of each metal salt and metal complex contained in the conductive ink (the total content when both the metal salt and the metal complex are contained) is preferably 10 to 90% by mass, and more preferably 10 to 40% by mass relative to the total mass of the conductive ink. If the above content is 10% by mass or more, the surface resistivity is further reduced. If the above content is 90% by mass or less, when the conductive ink is ejected from the nozzle by a spray coating method or an inkjet recording method, the ejection stability is further improved.
[0070] Hereinafter, the metal salt and the metal complex contained in the conductive ink will be described respectively.
[0071] (Metal Salt)
[0072] Examples of the metal salt contained in the conductive ink include metal benzoates, halides, carbonates, citrates, iodates, nitrites, nitrates, acetates, phosphates, sulfates, sulfides, trifluoroacetates, and carboxylates. Two or more salts may be used in combination.
[0073] Examples of the metal salt include benzoates, halides, carbonates, citrates, iodates, nitrites, nitrates, acetates, phosphates, sulfates, sulfides, trifluoroacetates, and carboxylates of metals. Two or more salts may be used in combination.
[0074] From the perspective of conductivity and storage stability, the metal salt is preferably a metal carboxylate. The carboxylic acid forming the metal carboxylate is preferably at least one selected from the group consisting of formic acid and carboxylic acids having 1 to 30 carbon atoms, more preferably a carboxylic acid having 8 to 20 carbon atoms, and further preferably a fatty acid having 8 to 20 carbon atoms. The fatty acid may be linear or branched, and may have a substituent.
[0075] Examples of the straight-chain fatty acid include acetic acid, propionic acid, butyric acid, valeric acid, pentanoic acid, hexanoic acid, heptanoic acid, behenic acid, oleic acid, octanoic acid, nonanoic acid, decanoic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, and undecanoic acid.
[0076] Examples of the branched-chain fatty acid include isobutyric acid, isovaleric acid, ethylhexanoic acid, neodecanoic acid, neopentanoic acid, 2-methylvaleric acid, 3-methylvaleric acid, 4-methylvaleric acid, 2,2-dimethylbutyric acid, 2,3-dimethylbutyric acid, 3,3-dimethylbutyric acid, and 2-ethylbutyric acid.
[0077] Examples of the carboxylic acid having a substituent include hexafluoroacetylaceruvic acid, 2-methylbutyric acid (Hydroangelic acid), 3-hydroxybutyric acid, 2-methyl-3-hydroxybutyric acid, 3-methoxybutyric acid, acetone dicarboxylic acid, 3-hydroxyglutaric acid, 2-methyl-3-hydroxyglutaric acid, and 2,2,4,4-hydroxyglutaric acid.
[0078] The metal salt may be a commercially available product or may be produced by a known method. The silver salt may be produced, for example, by the following method.
[0079] First, a silver compound (e.g., silver acetate) serving as a silver supply source and an amount of formic acid or a fatty acid having 1 to 30 carbon atoms equal to the molar equivalent of the silver compound are added to an organic solvent such as ethanol. The mixture is stirred for a predetermined time using an ultrasonic stirrer, and the resulting precipitate is washed and decanted with ethanol. All of these steps can be performed at room temperature. The mixing ratio of the silver compound to formic acid or a fatty acid having 1 to 30 carbon atoms is preferably 1:2 to 2:1, more preferably 1:1, in terms of molar ratio.
[0080] (Metal Complex)
[0081] The metal complex contained in the conductive ink is obtained, for example, by reacting a metal salt with a complexing agent. As a method for producing the metal complex, for example, a method of adding a metal salt and a complexing agent to an organic solvent and stirring for a predetermined time can be cited. The stirring method is not particularly limited and can be appropriately selected from known methods such as a method of stirring using a stirrer, a stirring blade or a mixer and a method of applying ultrasonic waves.
[0082] Examples of the metal salt for forming the metal complex include metal oxides, thiocyanates, sulfides, chlorides, cyanides, cyanates, carbonates, acetates, nitrates, nitrites, sulfates, phosphates, perchlorates, tetrafluoroborate, acetylacetonate complexes, and carboxylates.
[0083] Examples of the complexing agent include amines, ammonium carbamate compounds, ammonium carbonate compounds, ammonium bicarbonate compounds, and carboxylic acids. In particular, from the perspective of conductivity and stability of the metal complex, the complexing agent preferably contains at least one selected from the group consisting of ammonium carbamate compounds, ammonium carbonate compounds, alkylamines, and carboxylic acids having 8 to 20 carbon atoms.
[0084] The metal complex preferably has a structure derived from the complexing agent and a structure derived from at least one selected from the group consisting of ammonium carbamate compounds, ammonium carbonate compounds, amines, and carboxylic acids having 8 to 20 carbon atoms.
[0085] Examples of the amine compound as the complexing agent include ammonia, primary amines, secondary amines, tertiary amines, and polyamines.
[0086] Examples of the primary amine having a linear alkyl group include methylamine, ethylamine, 1-propylamine, n-butylamine, n-pentylamine, n-hexylamine, heptylamine, octylamine, nonylamine, n-decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecylamine and octadecylamine.
[0087] Examples of the primary amine having a branched alkyl group include isopropylamine, sec-butylamine, tert-butylamine, isopentylamine, 2-ethylhexylamine, and tert-octylamine.
[0088] Examples of the primary amine having an alicyclic structure include cyclohexylamine and dicyclohexylamine.
[0089] Examples of the primary amine having a hydroxyalkyl group include ethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, propanolamine, isopropanolamine, dipropanolamine, diisopropanolamine, tripropanolamine, and triisopropanolamine.
[0090] Examples of the primary amine having an aromatic ring include benzylamine, N,N-dimethylbenzylamine, aniline, diphenylamine, triphenylamine, aniline, N,N-dimethylaniline, N,N-dimethyl-p-toluidine, 4-aminopyridine, and 4-dimethylaminopyridine.
[0091] Examples of the secondary amine include dimethylamine, diethylamine, dipropylamine, dibutylamine, diphenylamine, dicyclopentylamine, and methylbutylamine.
[0092] Examples of the tertiary amine include trimethylamine, triethylamine, tripropylamine, and triphenylamine.
[0093] Examples of the polyamine include ethylenediamine, 1,3-diaminopropane, diethylenetriamine, triethylenetetramine, tetramethylenepentamine, hexamethylenediamine, tetraethylenepentamine, and combinations thereof.
[0094] The amine is preferably an alkylamine, more preferably an alkylamine having 3 to 10 carbon atoms, and still more preferably a primary alkylamine having 4 to 10 carbon atoms.
[0095] The amine constituting the metal complex may be one kind or two or more kinds.
[0096] When the metal salt and the amine are reacted, the ratio of the amount of the amine to the amount of the metal salt is preferably 1 to 15 times, more preferably 1.5 to 6 times. When the ratio is within the above range, the complex formation reaction is terminated to obtain a transparent solution.
[0097] Examples of the ammonium carbamate compound as the complexing agent include ammonium carbamate, methylammonium methylcarbamate, ethylammonium ethylcarbamate, 1-propylammonium 1-propylcarbamate, isopropylammonium isopropylcarbamate, butylammonium butylcarbamate, isobutylammonium isobutylcarbamate, amylammonium amylcarbamate, hexylammonium hexylcarbamate, heptylammonium heptylcarbamate, octylammonium octylcarbamate, 2-ethylhexylammonium 2-ethylhexylcarbamate, nonylammonium nonylcarbamate, and decylammonium decylcarbamate.
[0098] Examples of ammonium carbonate compounds as complexing agents include ammonium carbonate, methylammonium carbonate, ethylammonium carbonate, 1-propylammonium carbonate, isopropylammonium carbonate, butylammonium carbonate, isobutylammonium carbonate, pentylammonium carbonate, hexylammonium carbonate, heptylammonium carbonate, octylammonium carbonate, 2-ethylhexylammonium carbonate, nonylammonium carbonate, and decylammonium carbonate.
[0099] Examples of the ammonium bicarbonate compound as the complexing agent include ammonium bicarbonate, methylammonium bicarbonate, ethylammonium bicarbonate, 1-propylammonium bicarbonate, isopropylammonium bicarbonate, butylammonium bicarbonate, isobutylammonium bicarbonate, pentylammonium bicarbonate, hexylammonium bicarbonate, heptylammonium bicarbonate, octylammonium bicarbonate, 2-ethylhexylammonium bicarbonate, nonylammonium bicarbonate and decylammonium bicarbonate.
[0100] When reacting a metal salt with an ammonium carbamate compound, an ammonium carbonate compound or an ammonium bicarbonate compound, the ratio of the amount of the ammonium carbamate compound, the ammonium carbonate compound or the ammonium bicarbonate compound to the amount of the metal salt is preferably 0.01 to 1 times, more preferably 0.05 to 0.6 times.
[0101] Examples of the complexing agent, i.e., carboxylic acid, include caproic acid, caprylic acid, nonanoic acid, 2-ethylhexanoic acid, capric acid, neodecanoic acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, palmitoleic acid, oleic acid, linoleic acid, and linolenic acid. Among them, the carboxylic acid is preferably a carboxylic acid having 8 to 20 carbon atoms, and more preferably a carboxylic acid having 10 to 16 carbon atoms.
[0102] (Optional ingredient)
[0103] -Solvents-
[0104] The conductive ink preferably contains a solvent. The solvent is not particularly limited as long as it can dissolve components contained in the conductive ink, such as metal salts and metal complexes.
[0105] From the viewpoint of ease of production, the boiling point of the solvent is preferably 30 to 300°C, more preferably 50 to 200°C, and even more preferably 50 to 150°C.
[0106] The solvent is preferably contained in the conductive ink in such a manner that the concentration of the metal ions relative to the total content of the metal salt and the metal complex (the amount of the metal present as free ions relative to 1 g of the metal salt or the metal complex) is 0.01 to 3.6 mmol / g, and more preferably 0.05 to 2 mmol / g. When the concentration of the metal ions is within the above range, the conductive ink has excellent fluidity and exhibits excellent conductivity.
[0107] Examples of the solvent include hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, carbamates, olefins, amides, ethers, esters, alcohols, thiols, thioethers, phosphines, and water. The conductive ink may contain only one solvent or two or more solvents.
[0108] The hydrocarbon is preferably a linear or branched hydrocarbon having a carbon number of 6 to 20. Examples of the hydrocarbon include pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, octadecane, nonadecane and eicosane.
[0109] The alicyclic hydrocarbon is preferably an alicyclic hydrocarbon having a carbon number of 6 to 20. Examples of the alicyclic hydrocarbon include cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, and decalin.
[0110] Examples of the aromatic hydrocarbon include benzene, toluene, xylene, and tetralin.
[0111] The ether may be any of a linear ether, a branched ether and a cyclic ether. Examples of the ether include diethyl ether, dipropyl ether, dibutyl ether, methyl-tert-butyl ether, tetrahydrofuran, tetrahydropyran, dihydropyran and 1,4-dioxane.
[0112] The alcohol may be any of a primary alcohol, a secondary alcohol and a tertiary alcohol.
[0113] Examples of the alcohol include ethanol, 1-propanol, 2-propanol, 1-methoxy-2-propanol, 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 1-hexanol, 2-hexanol, 3-hexanol, 1-octanol, 2-octanol, 3-octanol, tetrahydrofurfuryl alcohol, cyclopentanol, terpineol, decanol, isodecanol, lauryl alcohol, isolauryl alcohol, myristyl alcohol, isomyristyl alcohol, cetyl alcohol, isocetyl alcohol, stearyl alcohol, isostearyl alcohol, oleyl alcohol, isooleyl alcohol, linolenyl alcohol, isolinolenyl alcohol, palmityl alcohol, isopalmityl alcohol, eicosanol, and isoeicosanol.
[0114] Examples of the ketone include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.
[0115] Examples of the esters include methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, methoxybutyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate and 3-methoxybutyl acetate.
[0116] -reducing agent-
[0117] The conductive ink may contain a reducing agent. If the conductive ink contains a reducing agent, the reduction of the metal complex to the metal is promoted.
[0118] Examples of the reducing agent include metal borohydride salts, aluminum hydride salts, amine compounds, alcohols, organic acids, reducing sugars, sugar alcohols, sodium sulfite, hydrazine compounds, dextrin, hydroquinone, hydroxylamine, ethylene glycol, glutathione, and oxime compounds.
[0119] The reducing agent may be an oxime compound described in JP-A-2014-516463. Examples of the oxime compound include acetone oxime, cyclohexanone oxime, 2-butanone oxime, 2,3-butanedione monoxime, dimethylglyoxime, methyl acetoacetate monoxime, methyl pyruvate monoxime, benzaldehyde oxime, 1-indanone oxime, 2-adamantanone oxime, 2-methylbenzamide oxime, 3-methylbenzamide oxime, 4-methylbenzamide oxime, 3-aminobenzamide oxime, 4-aminobenzamide oxime, acetophenone oxime, benzamide oxime, and pinacolone oxime.
[0120] The reducing agent contained in the conductive ink may be one kind or two or more kinds.
[0121] The content of the reducing agent in the conductive ink is not particularly limited, but is preferably 0.1 to 20% by mass, more preferably 0.3 to 10% by mass, and further preferably 1 to 5% by mass, based on the total mass of the conductive ink.
[0122] -Resin-
[0123] The conductive ink may contain a resin. If the conductive ink contains a resin, the adhesion between the conductive ink and the substrate and the like is improved.
[0124] Examples of the resin include polyester, polyethylene, polypropylene, polyacetal, polyolefin, polycarbonate, polyamide, fluororesin, silicone resin, ethyl cellulose, hydroxyethyl cellulose, rosin, acrylic resin, polyvinyl chloride, polysulfone, polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene resin, polyacrylonitrile, polysulfide, polyamideimide, polyether, polyarylate, polyetheretherketone, polyurethane, epoxy resin, vinyl ester resin, phenolic resin, melamine resin and urea resin.
[0125] The resin contained in the conductive ink may be one kind or two or more kinds.
[0126] The conductive ink may further contain additives such as inorganic salts, organic salts, inorganic oxides such as silicon dioxide, surface conditioners, wetting agents, crosslinking agents, antioxidants, rust inhibitors, heat stabilizers, surfactants, plasticizers, curing agents, thickeners, and silane coupling agents within a range that does not impair the effects of the present invention. In the conductive ink, the total content of the additives is preferably 20% by mass or less relative to the total mass of the conductive ink.
[0127] (Physical properties of conductive ink)
[0128] The viscosity of the conductive ink is not particularly limited, but is preferably 0.001 to 5000 Pa·s, and more preferably 0.001 to 100 Pa·s.
[0129] When the coating film is formed by spray coating or inkjet recording, the viscosity of the conductive ink is preferably 1 to 100 mPa·s, more preferably 2 to 50 mPa·s, and even more preferably 3 to 30 mPa·s.
[0130] The viscosity of the conductive ink is a value measured using a viscometer at 25° C. The viscosity is measured using, for example, a V-SCOMETER TV-22 viscometer (manufactured by TOKI SANGYO CO., LTD.).
[0131] The surface tension of the conductive ink is not particularly limited, but is preferably 20 to 45 mN / m, and more preferably 25 to 35 mN / m.
[0132] The surface tension is a value measured using a surface tensiometer at 25° C. The surface tension is measured using, for example, DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).
[0133] [Process 1]
[0134] Step 1 is a step of forming a first conductive film by subjecting the first coating film to a first curing treatment of at least one selected from the group consisting of a heat treatment and a light irradiation treatment after forming the first coating film on the substrate using the first ink.
[0135] As the first ink used in step 1, the above-mentioned conductive ink can be used.
[0136] <Base Material>
[0137] As the substrate for forming the first coating film in step 1, a known substrate can be used.
[0138] The material of the substrate is not particularly limited and can be selected according to the purpose. As the material of the substrate, for example, synthetic resins such as polyimide, polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polycarbonate, polyurethane, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, acrylic resin, AS resin (acrylonitrile styrene resin), ABS resin (acrylonitrile-butadiene-styrene copolymer), triacetyl cellulose, polyamide, polyacetal, polyphenylene sulfide, polysulfone, epoxy resin, glass epoxy resin (impregnated resin formed by impregnating epoxy resin into glass fiber), melamine resin, phenolic resin, urea resin, alkyd resin, fluororesin and polylactic acid; inorganic materials such as copper, steel, aluminum, silicon, soda glass, alkali-free glass and indium tin oxide (ITO); and paper such as base paper, coated paper, coated paper, cast-coated paper, resin-coated paper and synthetic paper.
[0139] The substrate may be a single layer or may be two or more layers. When the substrate is two or more layers, two or more substrates made of different materials may be laminated.
[0140] The form of the substrate is preferably a sheet or a film.
[0141] The thickness of the substrate is preferably 20 to 2000 μm. When the thickness of the substrate is 20 μm or more, the conductive film including the first conductive film and the second conductive film (hereinafter also simply referred to as “conductive film”) can be stably maintained, and the conductor formed with the conductive film can be handled well.
[0142] The substrate may have an ink receiving layer. The ink receiving layer refers to a coating layer formed on the substrate in order to absorb ink and fix the ink.
[0143] The thickness of the ink receiving layer is preferably 1 to 20 μm. If the thickness of the ink receiving layer is 1 to 20 μm, the ink receiving layer can be more stably maintained, the uniformity of the wetting and diffusion of the ink is improved, and the quality of the conductive film is further improved.
[0144] Before applying the conductive ink to the substrate, the substrate may be pretreated. Examples of the pretreatment include ozone treatment, plasma treatment, corona treatment, primer treatment, and roughening treatment.
[0145] The substrate may be a substrate for a printed wiring board.
[0146] Examples of the printed wiring board substrate include electronic substrates on which electronic components are mounted. Examples of the electronic substrate include flexible printed substrates, rigid printed substrates, and rigid-flexible substrates formed of the above substrates.
[0147] Examples of electronic components include semiconductor devices, capacitors, transistors, and ground wiring.
[0148] The electronic substrate may be a wiring substrate having wiring on a base material and at least one side of the inside of the substrate. The wiring is preferably copper wiring.
[0149] The substrate may be a substrate with an insulating film having an insulating film.
[0150] As the material of the insulating film, known insulating materials can be used, such as epoxy resin, aramid resin, crystalline polyolefin resin, amorphous polyolefin resin, fluorine-containing resin (polytetrafluoroethylene, perfluorinated polyimide, perfluorinated amorphous resin, etc.), polyimide resin, polyether sulfone resin, polyphenylene sulfide resin, polyether ether ketone resin and acrylate resin.
[0151] The insulating film may be a so-called optical transparent adhesive sheet (OCA) or a solder resist film formed using a so-called solder resist.
[0152] Furthermore, the insulating film may be an insulating film formed in step 3 described later.
[0153] <Formation of the First Coating Film>
[0154] As a method of forming the first coating film, for example, there is a method of applying the first ink onto a substrate to form a coating film.
[0155] The first coating film may be formed to contact the surface of the substrate, or may be formed to contact other layers when other layers (such as an insulating film described later) are provided on the substrate. That is, the first coating film may be provided directly on the surface of the substrate, or may be provided on the substrate via other layers.
[0156] The method for applying the first ink to the substrate is not particularly limited, and examples thereof include known methods such as coating, inkjet recording, and dipping. Among them, it is preferred to apply the first ink using an inkjet recording method because a small amount of droplets can be ejected to reduce the thickness of the conductive film.
[0157] The thickness L1 of the first coating film is, for example, 0.1 to 20 μm, or preferably 0.2 to 10 μm.
[0158] The thickness L1 of the first coating film can be adjusted according to the coating amount of the first ink (in the case of the inkjet recording method, the droplet ejection amount and the resolution).
[0159] Furthermore, the thickness L1 of the first coating film can be calculated from the amount of the first ink applied and the area of the formed first coating film.
[0160] (Inkjet recording method)
[0161] The inkjet recording method can be any one of a charge control method that utilizes electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that utilizes the application of vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electrical signal into a sound beam and irradiates the ink and ejects the ink using radiation pressure, and a thermal inkjet (Bubble Jet (registered trademark)) method that heats the ink to form bubbles and utilizes the generated pressure.
[0162] As an inkjet recording method, the inkjet recording method described in Japanese Patent Application Laid-Open No. 54-059936 can be particularly effectively used. Ink undergoes a rapid volume change due to thermal energy, and the ink is ejected from a nozzle by a force based on the state change.
[0163] In addition, regarding the inkjet recording method, the method described in paragraphs 0093 to 0105 of Japanese Patent Application Laid-Open No. 2003-306623 can also be referred to.
[0164] Examples of inkjet heads used in inkjet recording methods include a shuttle method that uses a short serial head to scan the head in the width direction of the substrate and perform recording, and a line method that uses a line head in which recording elements are arranged over the entire area of one side of the substrate.
[0165] In the linear method, the pattern can be formed on the entire surface of the substrate by scanning the substrate in a direction intersecting the arrangement direction of the recording elements, and a transport system such as a carriage for scanning a short-sized head is not required. In addition, since the movement of the carriage and the complicated scanning control with the substrate are not required, only the substrate is moved, so the formation speed can be increased compared to the reciprocating method.
[0166] The ejection amount of droplets of the first ink ejected from the inkjet head is preferably 1 to 100 pL, more preferably 3 to 80 pL, and even more preferably 3 to 20 pL.
[0167] The temperature of the substrate when applying the first ink to the substrate is preferably 20 to 120° C., more preferably 40 to 80° C. When the substrate temperature is 20 to 120° C., the influence of substrate deformation due to heat is small, and drying of the first coating film is accelerated.
[0168] <First Curing Treatment>
[0169] The first curing treatment is to perform at least one treatment selected from the group consisting of a heating treatment and a light irradiation treatment on the formed first coating film. By performing the first curing treatment on the first coating film, the metal salt or metal complex contained in the first ink is reduced to form a first conductive film having conductivity.
[0170] The first curing treatment may be only one of the heating treatment and the light irradiation treatment, or may be both of the heating treatment and the light irradiation treatment. From the viewpoint of being able to shorten the sintering time, it is preferable to subject the first coating film to both the heating treatment and the light irradiation treatment.
[0171] There is no particular restriction on the number of times of the heat treatment and the light irradiation treatment. Also, there is no particular restriction on the order in which the heat treatment and the light irradiation treatment are performed. From the perspective of achieving better surface smoothness, it is preferred to perform the heat treatment after the light irradiation treatment.
[0172] (Heat treatment)
[0173] The conditions for the heat treatment for heating the first coating film are not particularly limited, and can be appropriately adjusted according to the type of the first ink, the characteristics of the substrate, the conditions for the light irradiation treatment when the light irradiation treatment is performed, and the like.
[0174] The heating temperature in the heat treatment is preferably 80° C. or higher, more preferably 100° C. or higher. From the viewpoint of reducing damage to the substrate and the like, the heating temperature is preferably 250° C. or lower, more preferably 200° C. or lower.
[0175] The heating time in the heat treatment (the total of the heating times in the case of multiple heat treatments) is preferably 1 minute or longer. From the perspective of reducing damage to the substrate, etc., the heating time is preferably 120 minutes or shorter, more preferably 60 minutes or shorter.
[0176] When the heating temperature and the heating time are within the above ranges, a conductive film can be formed while suppressing the influence of thermal modification, deformation of the substrate, and the like.
[0177] The method of heat treatment is not particularly limited, and examples thereof include known methods using a heating mechanism such as a hot plate, a heating oven, and an infrared heater.
[0178] The time from the moment when the formation of the first film ends to the moment when the heat treatment is started is preferably less than 60 seconds. If the above-mentioned time is less than 60 seconds, ink is suppressed from diffusing from the first film, and a film with thickness is easily formed. The lower limit of the above-mentioned time is not particularly limited, and the heat treatment can be started immediately after the formation of the first film ends.
[0179] In addition, the moment when the formation of the first coating film is completed refers to, for example, the moment when all the ink of the first ink is dripped onto the substrate when the first coating film is formed on the substrate using an inkjet recording method. In addition, the moment when the heating treatment is started refers to the moment when the temperature of the first coating film starts to rise by the heating mechanism.
[0180] (Light irradiation treatment)
[0181] The conditions for the light irradiation treatment of irradiating the first coating film with light are not particularly limited, and may be appropriately adjusted depending on the type of the first ink, the characteristics of the substrate, the conditions for the heat treatment when the heat treatment is performed, and the like.
[0182] Examples of the light irradiated in the light irradiation treatment include ultraviolet rays, visible rays, and infrared rays, and ultraviolet rays are preferred.
[0183] The peak wavelength of ultraviolet rays is preferably 200 to 405 nm, more preferably 250 to 400 nm, and further preferably 250 to 400 nm.
[0184] The exposure amount in the light irradiation treatment (when the light irradiation treatment is performed multiple times, the total exposure amount of the multiple light irradiations) is preferably 0.1 to 100 J / cm 2 , more preferably 0.1 to 20 J / cm 2 .
[0185] As a light source for ultraviolet irradiation, mercury lamps, gas lasers and solid lasers are mainly used, and mercury lamps, metal halide lamps and ultraviolet fluorescent lamps are widely known. In addition, UV-LED (light emitting diode) and UV-LD (laser diode) are expected to be small, long-life, high-efficiency and low-cost light sources.
[0186] As a light source for ultraviolet irradiation, a metal halide lamp, a high-pressure mercury lamp, a medium-pressure mercury lamp, a low-pressure mercury lamp, or a UV-LED is preferable.
[0187] The time from the moment of forming the first coating to the moment of starting the light irradiation treatment is preferably within 2 seconds, more preferably within 1 second. By starting the light irradiation within the above time, the ink is suppressed from diffusing from the first coating, and a film with thickness is easily formed. The lower limit of the above time is not particularly limited, and the light irradiation treatment can be started immediately after the formation of the first coating.
[0188] In addition, the time of forming the first coating film refers to the time when the ink of the first ink drips onto the substrate, for example, when the first coating film is formed on the substrate using an inkjet recording method. And the time of starting the light irradiation treatment refers to the time when the light irradiation is started. That is, in the light irradiation treatment, the light irradiation treatment can be started before all the ink of the first ink drips onto the substrate and the formation of the first coating film is completed.
[0189] In step 1, the treatment cycle including the formation of the first coating film and the first curing treatment may be performed only once or multiple times. In the second and subsequent treatment cycles, the first coating film is formed on the surface of the first conductive film formed in the previous treatment cycle, and the first curing treatment is performed on the formed first coating film, thereby forming a laminate of the first conductive film.
[0190] The number of treatment cycles including the formation of the first coating film and the first curing treatment in step 1 is, for example, 1 to 50, or preferably 4 to 20.
[0191] The thickness of the first conductive film formed in step 1 is preferably 50 to 98%, more preferably 80 to 98%, of the total thickness of the first conductive film formed in step 1 and the second conductive film formed in step 2. In this specification, "the thickness of the first conductive film" refers to the total thickness of the first conductive film formed in all the processing cycles of step 1. The "thickness" of the second conductive film and the insulating film described later also has the same meaning.
[0192] The thickness of the first conductive film can be adjusted by the thickness L1 of the first coating film and the number of processing cycles including the formation of the first coating film and the first curing process.
[0193] Furthermore, the thickness of the first conductive film and the thickness of the conductive film described later are obtained by obtaining a cross-sectional image of the first conductive film using a scanning electron microscope, measuring the lengths of 10 points at different positions corresponding to the thickness of the first conductive film, and arithmetically averaging the lengths of the 10 points to obtain an arithmetic mean value.
[0194] [Process 2]
[0195] Step 2 is a step of forming a second conductive film by forming a second coating film on the first conductive film formed in step 1 using a second ink and then subjecting the second coating film to a second curing treatment of at least one selected from the group consisting of a heat treatment and a light irradiation treatment to form a second conductive film.
[0196] As the second ink used in step 2, the above-mentioned conductive ink can be used.
[0197] <Formation of Second Coating Film>
[0198] The formation of the second coating film in step 2 adjusts the thickness L2 of the second coating film in a manner that satisfies at least one of the above-mentioned formulas (1) and (2). In addition, it also includes its preferred method, which is the same as the method for forming the first coating film in step 1, so detailed description is omitted.
[0199] The thickness L2 of the second coating film formed in step 2 is, for example, 0.2 to 5 μm, or preferably 0.2 to 1.0 μm.
[0200] Furthermore, it is preferable that the thickness L2 of the second coating film is shorter than the thickness L1 of the first coating film.
[0201] The adjustment method and calculation method of the thickness L2 of the second coating film are the same as those of the thickness L1 of the first coating film.
[0202] <Second Curing Treatment>
[0203] The second curing treatment is to perform at least one treatment selected from the group consisting of a heating treatment and a light irradiation treatment on the formed second coating film. By performing the second curing treatment on the second coating film, the metal salt or metal complex contained in the second ink is reduced to form a second conductive film having conductivity.
[0204] In the present manufacturing method, at least one of the heating treatment and the light irradiation treatment is performed in the first curing treatment and the second curing treatment in a manner that satisfies at least one of the above-mentioned formulas (1) and (2), and the processing conditions of the first curing treatment and the second curing treatment are adjusted respectively.
[0205] When the light irradiation treatment of the second curing treatment is described as being the same as the light irradiation treatment of the first curing treatment, “the same” means that the wavelength of light irradiated to each coating film is the same.
[0206] The second curing process is adjusted as described above, and other preferred aspects thereof are the same as those of the first curing process, so detailed description thereof will be omitted.
[0207] In the present production method, it is preferred that the heat treatment be performed as the first curing treatment and the heat treatment be performed as the second curing treatment in terms of achieving more excellent surface smoothness.
[0208] Furthermore, in the present production method, it is preferred that the light irradiation treatment be performed as the first curing treatment and the light irradiation treatment be performed as the second curing treatment in terms of further improving the electrical conductivity.
[0209] In the present production method, it is more preferable to perform both the heating treatment and the light irradiation treatment as the first curing treatment, and to perform both the heating treatment and the light irradiation treatment as the second curing treatment.
[0210] In the present manufacturing method, the value calculated by {(T2-23)×t2 / L2} / {(T1-23)×t1 / L1} in the above formula (1) (hereinafter also referred to as "variable A1") is preferably larger. This is because if variable A1 is larger, welding inside the conductive film proceeds, and the adhesion and abrasion resistance are further improved.
[0211] From the above viewpoints, in the present manufacturing method, when heat treatment is performed as the first curing treatment and the second curing treatment, it is preferred to satisfy the above formula (1), more preferably to satisfy the following formula (1a), and even more preferably to satisfy the following formula (1b).
[0212] Formula (1a) 1.5 ≤ {(T2-23) × t2 / L2} / {(T1-23) × t1 / L1}
[0213] Formula (1b) 4≤{(T2-23)×t2 / L2} / {(T1-23)×t1 / L1}
[0214] Furthermore, in the present production method, when heat treatment is performed as the first curing treatment and the second curing treatment, it is preferable to satisfy the following formula (1c) from the viewpoint of preventing thermal damage to the substrate.
[0215] Formula (1c) {(T2-23)×t2 / L2} / {(T1-23)×t1 / L1}≤10
[0216] Furthermore, in the present manufacturing method, the value calculated by (E2 / L2) / (E1 / L1) in the above formula (2) (hereinafter also referred to as "variable A2") is preferably larger. This is because if variable A2 is large, the surface of the conductive film on the side opposite to the substrate and the inside are welded, and the adhesion and abrasion resistance are further improved.
[0217] From the above viewpoints, in the present manufacturing method, when light irradiation treatment is performed as the first curing treatment and the second curing treatment, it is preferred to satisfy the above formula (2), more preferably to satisfy the following formula (2a), and even more preferably to satisfy the following formula (2b).
[0218] Formula (2a) 4≤(E2 / L2) / (E1 / L1)
[0219] Formula (2b) 10≤(E2 / L2) / (E1 / L1)
[0220] Furthermore, in the present production method, when light irradiation treatment is performed as the first curing treatment and the second curing treatment, it is preferable that the following formula (2c) is satisfied from the viewpoint of achieving better surface smoothness.
[0221] Formula (2c) (E2 / L2) / (E1 / L1)≤50
[0222] In order to achieve a better effect of the present invention, the present production method preferably satisfies both the above formula (1) and the above formula (2). More preferred embodiments of the variables A1 and A2 when the present production method satisfies both the above formula (1) and the above formula (2) are as described above.
[0223] The thickness of the second conductive film formed in step 2 is preferably 2 to 50%, more preferably 2 to 20%, of the total thickness of the first conductive film formed in step 1 and the second conductive film formed in step 2.
[0224] The thickness of the second conductive film can be adjusted by the thickness L2 of the second coating film and the number of processing cycles including the formation of the second coating film and the first curing process.
[0225] The thickness of the second conductive film can be obtained, for example, by calculating the difference between the thickness of a conductive film composed of the first conductive film and the second conductive film and the thickness of the first conductive film.
[0226] [Process 3]
[0227] The method for producing an electrical conductor may further include step 3 of forming an insulating film on the substrate to produce a substrate with an insulating film, and preferably further includes step 3.
[0228] When the method for producing a conductor further includes step 3, in step 1, a first conductive film is formed on the insulating film of the substrate with an insulating film produced in step 3. That is, after a first coating film is formed on the insulating film of the substrate with an insulating film produced in step 3 using the first ink, a first curing treatment is performed on the formed first coating film, thereby forming the first conductive film.
[0229] As a method of forming an insulating film on a substrate, for example, there is a method including a step of applying insulating ink on a substrate to form a coating film and a step of curing the formed coating film of the insulating ink.
[0230] The insulating ink used for forming the insulating film will be described later.
[0231] The method of applying the insulating ink to the substrate is not particularly limited, and examples thereof include known methods such as coating, inkjet recording, and dipping. Among them, applying the insulating ink by inkjet recording is preferred because a small amount of droplets can be sprayed to reduce the thickness of the conductive film.
[0232] The method for forming a coating film using the inkjet recording method, including its preferred embodiment, is the same as the method for forming a first coating film by the inkjet recording method in step 1, and therefore a detailed description thereof will be omitted.
[0233] The method for curing the insulating ink coating film formed on the substrate is not particularly limited, but it is preferable to form the insulating film by irradiating the insulating ink coating film with active energy rays.
[0234] The exposure amount during irradiation with active energy rays is preferably 0.1 to 100 J / cm 2 , more preferably 1 to 50 J / cm 2 In addition, when the application of the insulating ink and the irradiation of the active energy ray are assumed to be one cycle, the exposure amount referred to herein means the exposure amount of the active energy ray in one cycle.
[0235] Furthermore, from the viewpoint of suppressing the generation of wrinkles in the insulating film, the illuminance during irradiation with active energy rays is preferably 8 W / cm 2 More preferably 10W / cm 2There is no particular upper limit on the illuminance, but it is, for example, 20 W / cm 2 .
[0236] As the light source for active energy ray irradiation, the light sources described in the description of the light irradiation treatment in the first curing treatment can be mentioned.
[0237] In step 3, the treatment cycle including the step of forming a coating film using the insulating ink and the step of irradiating the coating film with active energy rays may be performed only once or may be performed a plurality of times.
[0238] By performing the above-mentioned treatment cycle multiple times, the thickness of the insulating film can be more easily adjusted. In addition, the thickness of the insulating film can also be adjusted by the amount of insulating ink applied to the substrate.
[0239] <Insulation ink>
[0240] The insulating ink used for forming the insulating film will be described.
[0241] Insulating ink is an ink used to form an insulating film with electrical insulation. Electrical insulation refers to a volume resistivity of 10 10 Properties above Ωcm.
[0242] The insulating ink is preferably an active energy ray-curable ink.
[0243] Examples of the insulating ink include inks containing a polymerizable monomer and a polymerization initiator.
[0244] (Polymerizable Monomer)
[0245] A polymerizable monomer refers to a monomer having at least one polymerizable group in one molecule. The polymerizable group in the polymerizable monomer may be a cation polymerizable group or a radical polymerizable group, and is preferably a radical polymerizable group, and more preferably an ethylenically unsaturated group, from the perspective of curability.
[0246] A monomer refers to a compound having a molecular weight of not more than 1000. The molecular weight can be calculated from the types and numbers of atoms constituting the compound.
[0247] The polymerizable monomer may be a monofunctional polymerizable monomer having one polymerizable group, or may be a polyfunctional polymerizable monomer having two or more polymerizable groups.
[0248] The monofunctional polymerizable monomer is not particularly limited as long as it is a monomer having one polymerizable group. From the viewpoint of curability, the monofunctional polymerizable monomer is preferably a monofunctional free radical polymerizable monomer, and more preferably a monofunctional ethylenically unsaturated monomer.
[0249] Examples of the monofunctional ethylenically unsaturated monomer include monofunctional (meth)acrylates, monofunctional (meth)acrylamides, monofunctional aromatic vinyl compounds, monofunctional vinyl ethers, and monofunctional N-vinyl compounds.
[0250] Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, tert-octyl (meth)acrylate, isoamyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, bornyl (meth)acrylate, and isobornyl (meth)acrylate. , 2-ethylhexyl diglycol (meth)acrylate, butoxyethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 4-bromobutyl (meth)acrylate, cyanoethyl (meth)acrylate, benzyl (meth)acrylate, butoxymethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-(2-methoxyethoxy)ethyl (meth)acrylate, 2-(2-butoxyethoxy)ethyl (meth)acrylate, 2,2,2-tetrafluoroethyl (meth)acrylate, 1H,1H,2H,2H-perfluorodecyl (meth)acrylate, 4-butylphenyl (meth)acrylate, phenyl (meth)acrylate, 2,4,5-Tetramethylphenyl (meth)acrylate, 4-chlorophenyl (meth)acrylate, 2-phenoxymethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, glycidyloxybutyl (meth)acrylate, glycidyloxyethyl (meth)acrylate, glycidyloxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate , 4-hydroxybutyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, phenyl glycidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, trimethoxysilylpropyl (meth)acrylate, trimethylsilylpropyl (meth)acrylate, polyethylene oxide monomethyl ether (meth)acrylate, polyethylene oxide monomethyl ether (meth)acrylate, polyethylene oxide monomethyl ether (meth)acrylate ether esters, dipropylene glycol (meth)acrylate, polypropylene oxide monoalkyl ether (meth)acrylate, 2-methacryloyloxyethyl succinate, 2-methacryloyloxyhexahydrophthalate, 2-methacryloyloxyethyl-2-hydroxypropyl phthalate, ethoxydiethylene glycol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, trifluoroethyl (meth)acrylate, perfluorooctyl ethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, ethylene oxide (EO) modified phenol (meth)acrylate Ester, EO modified cresol (meth) acrylate, EO modified nonylphenol (meth) acrylate, propylene oxide (P0) modified nonylphenol (meth) acrylate, (meth) acrylate E0 modified-2-ethylhexyl ester, dicyclopentenyl (meth) acrylate, dicyclopentenyloxyethyl (meth) acrylate, dicyclopentanyl (meth) acrylate, (3-ethyl-3-oxetanylmethyl) (meth) acrylate, phenoxyethylene glycol (meth) acrylate, 2-carboxyethyl (meth) acrylate and 2-(meth)acryloyloxyethyl succinate. ,
[0251] Among them, from the perspective of improving heat resistance, the monofunctional (meth)acrylate is preferably a monofunctional (meth)acrylate having an aromatic ring or an aliphatic ring, and more preferably isobornyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, or dicyclopentanyl (meth)acrylate.
[0252] Examples of the monofunctional (meth)acrylamide include (meth)acrylamide, N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-n-butyl (meth)acrylamide, N-tert-butyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-methylol (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide and (meth)acryloyl morpholine.
[0253] Examples of the monofunctional aromatic vinyl compound include styrene, dimethylstyrene, trimethylstyrene, isopropylstyrene, chloromethylstyrene, methoxystyrene, acetoxystyrene, chlorostyrene, dichlorostyrene, bromostyrene, methyl vinylbenzoate, 3-methylstyrene, 4-methylstyrene, 3-ethylstyrene, 4-ethylstyrene, 3-propylstyrene, 4-propylstyrene, 3-butylstyrene, 4-butylstyrene, 3-hexylstyrene, 4-hexylstyrene, 3-octylstyrene, 4-octylstyrene, 3-(2-ethylhexyl)styrene, 4-(2-ethylhexyl)styrene, allylstyrene, isopropenylstyrene, butenylstyrene, octenylstyrene, 4-tert-butoxycarbonylstyrene and 4-tert-butoxystyrene.
[0254] Examples of the monofunctional vinyl ether include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, n-butyl vinyl ether, tert-butyl vinyl ether, 2-ethylhexyl vinyl ether, n-nonyl vinyl ether, lauryl vinyl ether, cyclohexyl vinyl ether, cyclohexyl methyl vinyl ether, 4-methylcyclohexyl methyl vinyl ether, benzyl vinyl ether, dicyclopentenyl vinyl ether, 2-dicyclopentenyloxyethyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, butoxyethyl vinyl ether, methoxyethoxyethyl vinyl ether, ethoxyethoxyethyl vinyl ether, methoxypolyethylene glycol vinyl ether, tetrahydrofurfuryl vinyl ether, 2-hydroxyethyl vinyl ether, 2-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, 4-hydroxymethylcyclohexyl methyl vinyl ether, diethylene glycol monovinyl ether, polyethylene glycol vinyl ether, chloroethyl vinyl ether, chlorobutyl vinyl ether, chloroethoxyethyl vinyl ether, phenylethyl vinyl ether, and phenoxypolyethylene glycol vinyl ether.
[0255] Examples of the monofunctional N-vinyl compound include N-vinyl-ε-caprolactam and N-vinyl pyrrolidone.
[0256] The polyfunctional polymerizable monomer is not particularly limited as long as it has two or more polymerizable groups. From the viewpoint of curability, the polyfunctional polymerizable monomer is preferably a polyfunctional free radical polymerizable monomer, and more preferably a polyfunctional ethylenically unsaturated monomer.
[0257] As a polyfunctional ethylenically unsaturated monomer, a polyfunctional (meth)acrylate compound and a polyfunctional vinyl ether are mentioned, for example.
[0258] Examples of the polyfunctional (meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, Neopentyl glycol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, heptanediol di(meth)acrylate, EO-modified neopentyl glycol di(meth)acrylate, PO-modified neopentyl glycol di(meth)acrylate, EO-modified hexanediol di(meth)acrylate, P0-modified hexanediol di(meth)acrylate, octanediol di(meth)acrylate (meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, dodecanediol di(meth)acrylate, glycerol di(meth)acrylate, pentaerythritol di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane EO addition tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(meth)acryloyloxyethoxy trimethylolpropane, glycerol polyglycidyl ether poly(meth)acrylate and tris(2-acryloyloxyethyl)isocyanurate.
[0259] Examples of the polyfunctional vinyl ether include 1,4-butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, 1,4-cyclohexanedimethanol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolethane trivinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, and the like. ether, glycerol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, EO addition trimethylolpropane trivinyl ether, PO addition trimethylolpropane trivinyl ether, EO addition ditrimethylolpropane tetravinyl ether, PO addition ditrimethylolpropane tetravinyl ether, EO addition pentaerythritol tetravinyl ether, P0 addition pentaerythritol tetravinyl ether, E0 addition dipentaerythritol hexavinyl ether and P0 addition dipentaerythritol hexavinyl ether.
[0260] From the viewpoint of curability, the polyfunctional polymerizable monomer is preferably a monomer having 3 to 11 carbon atoms in the part other than the (meth)acryloyl group. Among the monomers having 3 to 11 carbon atoms in the part other than the (meth)acryloyl group, 1,6-hexanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, PO-modified neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate (EO chain n=4) or 1,10-decanediol di(meth)acrylate is more preferred.
[0261] The polymerizable monomer may be used alone or in combination of two or more. The insulating ink preferably contains two or more polymerizable monomers.
[0262] The content of the polymerizable monomer is preferably 10 to 98% by mass, more preferably 50 to 98% by mass, based on the total mass of the insulating ink.
[0263] (Polymerization initiator)
[0264] Examples of the polymerization initiator contained in the insulating ink include oxime compounds, alkylphenone compounds, acylphosphine compounds, aromatic onium salt compounds, organic peroxides, sulfur compounds, hexaarylbisimidazole compounds, borate compounds, azinium compounds, titanocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamines.
[0265] Among them, the polymerization initiator contained in the insulating ink is preferably at least one selected from the group including oxime compounds, alkylphenone compounds and bismuth titanocene compounds, more preferably an alkylphenone compound, and further preferably at least one selected from the group including α-aminoalkylphenone compounds and benzyl ketal alkylphenone compounds.
[0266] The content of the polymerization initiator is preferably 0.5 to 20% by mass, more preferably 2 to 10% by mass, based on the total mass of the insulating ink.
[0267] (Optional ingredient)
[0268] The insulating ink may contain other components other than the polymerization initiator and the polymerizable monomer as optional components. Examples of other components include a chain transfer agent, a polymerization inhibitor, a sensitizer, a surfactant, and an additive.
[0269] -Chain transfer agent-
[0270] The insulating ink may contain at least one chain transfer agent.
[0271] From the viewpoint of improving the reactivity of the photopolymerization reaction, the chain transfer agent is preferably a polyfunctional thiol.
[0272] Examples of the polyfunctional thiol include aliphatic thiol compounds, aromatic thiol compounds, polyol poly(thioglycolate), polyol poly(3-mercaptopropionate), and poly(mercaptobutyrate).
[0273] -Polymerization Inhibitors-
[0274] The insulating ink may contain at least one polymerization inhibitor.
[0275] Examples of the polymerization inhibitor include p-methoxyphenol, quinones (e.g., hydroquinone, benzoquinone, methoxybenzoquinone, etc.), phenothiazines, catechols, alkylphenols (e.g., butylhydroxytoluene (BHT)), alkylbisphenols, zinc dimethyldithiocarbamate, copper dimethyldithiocarbamate, copper dibutyldithiocarbamate, copper salicylate, thiodipropionate esters, mercaptobenzimidazole, phosphorous acids, 2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPO), 2,2,6,6-tetramethyl-4-hydroxypiperidin-1-oxyl (TEMPOL), and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt (also known as CupferronAl).
[0276] When the insulating ink contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 2.0% by mass, more preferably 0.02 to 1.0% by mass, based on the total mass of the insulating ink.
[0277] -Sensitizer-
[0278] The insulating ink may contain at least one sensitizer.
[0279] As the sensitizer, for example, there can be mentioned polynuclear aromatic compounds (for example, pyrene, perylene, triphenylene and 2-ethyl-9,10-dimethoxyanthracene), xanthene compounds (for example, fluorescent yellow, eosin, erythrosine, rose red B and rose bengal), cyanine compounds (for example, thiacarbocyanine and oxacarbocyanine), merocyanine compounds (for example, merocyanine and carbomerocyanine), thiazine compounds (for example, thionine, methylene blue and toluidine blue), acridine compounds (for example, acridine orange, chloroflavin and acriflavin), anthraquinones (for example, anthraquinone), squarylium compounds (for example, squarylium), coumarin compounds (for example, 7-diethylamino-4-methylcoumarin), thioxanthone compounds (for example, isopropylthioxanthone) and dihydrochromanone compounds (for example, dihydrochromanone). Among them, the sensitizer is preferably a thioxanthone compound.
[0280] When the insulating ink contains a sensitizer, the content of the sensitizer is preferably 1.0 to 15.0% by mass, more preferably 1.5 to 5.0% by mass, based on the total mass of the insulating ink.
[0281] -Surfactant-
[0282] The insulating ink may contain at least one surfactant.
[0283] As the surfactant, there can be mentioned the surfactants described in Japanese Patent Application Laid-Open No. 62-173463 and Japanese Patent Application Laid-Open No. 62-183457. Also, as the surfactant, for example, there can be mentioned anionic surfactants such as dialkyl sulfosuccinates, alkylnaphthalene sulfonates and fatty acid salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycol and polyoxyethylene / polyoxypropylene block copolymers; and cationic surfactants such as alkylamine salts and quaternary ammonium salts. Also, the surfactant can be a fluorine-based surfactant or a silicone-based surfactant.
[0284] When the insulating ink contains a surfactant, the content of the surfactant is preferably 0.5% by mass or less, and more preferably 0.1% by mass or less, relative to the total mass of the insulating ink. The lower limit of the content of the surfactant is not particularly limited.
[0285] -Organic Solvents-
[0286] The insulating ink may contain at least one organic solvent.
[0287] Examples of the organic solvent include (poly)alkylene glycol monoalkyl ethers, (poly)alkylene glycol dialkyl ethers, (poly)alkylene glycol acetates, (poly)alkylene glycol diacetates, (poly)alkylene glycol monoalkyl ether acetates, ketones, lactones, esters, cyclic ethers and amides.
[0288] When the insulating ink contains an organic solvent, the content of the organic solvent is preferably 70% by mass or less, and more preferably 50% by mass or less, relative to the total mass of the insulating ink. The lower limit of the content of the organic solvent is not particularly limited.
[0289] The insulating ink may contain additives such as a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, and an alkaline compound as required.
[0290] (Physical properties of insulating ink)
[0291] The viscosity of the insulating ink is not particularly limited, and may be, for example, 0.001 to 5000 Pa·s. When the coating is formed by spraying or inkjet recording, the viscosity of the insulating ink is not particularly limited, and is preferably 0.5 to 100 mPa·s, and more preferably 2 to 60 mPa·s.
[0292] The viscosity of insulating ink and its measuring method are the same as those of conductive ink.
[0293] The surface tension of the insulating ink is not particularly limited, but is preferably 60 mN / m or less, more preferably 20 to 50 mN / m, and further preferably 25 to 45 mN / m.
[0294] The surface tension of insulating ink and its measurement method are the same as those of conductive ink.
[0295] A specific embodiment of the method for producing the conductor will be exemplified.
[0296] The method for producing an electrical conductor may be a method for producing a printed wiring board.
[0297] As a method for manufacturing a printed wiring board, for example, there can be cited a method including a step of forming a conductive film on a substrate for a printed wiring board such as an electronic substrate on which electronic components are mounted according to the method described in steps 1 and 2, and a method including a step of recording an image forming a wiring pattern on the substrate using conductive ink according to the method described in steps 1 and 2.
[0298] Furthermore, the method for producing a conductor may be a method for producing an electromagnetic wave shielding body including the step of forming a conductive film on a substrate according to the method described in the steps 1 and 2.
[0299] The substrate used in the method for manufacturing an electromagnetic wave shield may be an electronic substrate on which the above-mentioned electronic components are mounted. In other words, the method for manufacturing a conductor may be a method for manufacturing a printed wiring board with an electromagnetic wave shield, comprising the step of forming a conductive film on an electronic substrate on which electronic components are mounted according to the method described in steps 1 and 2.
[0300] When forming a conductive film on an electronic substrate on which electronic components are mounted, it is preferred to form the conductive film so as to cover the electronic components from the viewpoint of better electromagnetic wave shielding properties. Furthermore, the conductive film is preferably electrically connected to a ground electrode.
[0301] In the above-mentioned method for manufacturing a printed wiring board or an electromagnetic wave shield, it is preferred that an insulating film is formed on the substrate according to the method described in step 3 before step 1, and then a conductive film covering the insulating film is formed according to the methods described in steps 1 and 2.
[0302] By providing an insulating film formed of insulating ink between the substrate and the conductive film, a printed wiring board or an electromagnetic shielding body with further improved adhesion of the conductive film can be produced. In addition, by the above method, an electromagnetic shielding body with better electromagnetic shielding properties can be produced.
[0303] When an insulating film and a conductive film are disposed on an electronic substrate on which electronic components are mounted, it is preferred to dispose the insulating film so as to cover all the electronic components except the ground electrode in terms of better electromagnetic wave shielding properties.
[0304] [Conductor]
[0305] The conductor manufactured by the present manufacturing method (hereinafter, also simply referred to as “conductor”) has at least a substrate and a conductive film composed of a first conductive film and a second conductive film.
[0306] The conductor may have other components besides the substrate and the conductive film. Examples of other components besides the substrate and the conductive film include an insulating film and electronic components (semiconductor devices, ground wiring, etc.) mounted on the substrate.
[0307] The base material of the conductor is the same as the base material used in step 1, and therefore detailed description thereof will be omitted.
[0308] 〔Conductive film〕
[0309] The conductive film included in the conductor is composed of the first conductive film and the second conductive film, and contains a metal constituting the metal salt or the metal complex included in the first ink and the second ink.
[0310] The above-mentioned metals are the same as the metals constituting the metal salt or the metal complex contained in the conductive ink, and therefore detailed description thereof is omitted.
[0311] The metal contained in the conductive film varies depending on the composition of the first ink and the second ink used in the present production method, but may be only one kind or may be two or more kinds.
[0312] The content of the metal contained in the conductive film is preferably 5 to 70% by mass, more preferably 7 to 50% by mass, based on the total mass of the conductive film.
[0313] The thickness of the conductive film is not particularly limited, but is preferably 0.1 to 100 μm, more preferably 1 to 50 μm, from the viewpoint of productivity and excellent conductivity.
[0314] The thickness of the conductive film can be adjusted by adjusting the thickness of the first conductive film and the second conductive film respectively by the above-mentioned method.
[0315] 〔Insulating film〕
[0316] The conductor preferably has an insulating film.
[0317] Among them, when the conductor is used as an electromagnetic wave shield, the conductor preferably has a base material, an insulating film, and a conductive film in this order.
[0318] The insulating film is a film having electrical insulating properties, and has a function of electrically insulating components disposed with the insulating film interposed therebetween.
[0319] Examples of the insulating film include an insulating film provided on the above-mentioned substrate with an insulating film and an insulating film formed using insulating ink by the method described in the above-mentioned step 3.
[0320] The thickness of the insulating film is preferably 30 to 3000 μm. When the thickness of the insulating film is within the above range, the conductive film can be formed more easily and the insulating property of the insulating film is further improved.
[0321] The thickness of the insulating film can be measured by the above-mentioned measuring method for the conductive film.
[0322] 〔Uses of Conductors〕
[0323] The conductor obtained as described above can be used in various applications.
[0324] As a use of the conductor, for example, an electromagnetic wave shield can be cited. The electromagnetic wave shield blocks electromagnetic waves such as radio waves and microwaves (ultra-short waves) generated from electronic devices, thereby suppressing the influence of interference from external electromagnetic waves on semiconductor devices and the influence of electromagnetic waves radiated from semiconductor devices on other semiconductor devices or electronic devices. In addition, the electromagnetic wave shield can prevent the generation of static electricity.
[0325] When a conductor is used as an electromagnetic wave shield, the conductive film is often electrically connected to a ground wiring provided on a substrate, etc. At least a portion of the conductive film is electrically connected to the ground wiring, whereby a current generated by an electromagnetic wave incident on the conductive film flows into the ground wiring, and the electromagnetic wave is attenuated. The current generated in the conductive film becomes easy to flow into the ground wiring, and the electromagnetic wave becomes easy to attenuate, so it is preferred that there are more areas where the conductive film and the ground wiring are electrically connected.
[0326] Such an electromagnetic wave shield can be used in electronic devices such as personal computers, workstations, imaging equipment, and electronic medical equipment.
[0327] Example
[0328] Hereinafter, the present invention will be further described in detail by giving examples. The materials, usage amounts, ratios, processing contents and processing sequences shown in the following examples can be appropriately changed without departing from the purpose of the present invention. Therefore, the present invention is not limited to the modes shown in the following examples. In addition, "parts" and "%" are weight references unless otherwise specified.
[0329] [Example 1]
[0330] <Ink preparation process>
[0331] 6.08 g of isobutylammonium carbonate and 15.0 g of isopropyl alcohol were added to a 50 mL three-necked flask, and the mixture was stirred to prepare a solution. Next, 2.0 g of silver oxide was added to the prepared solution, and the mixture was reacted at 23° C. for 2 hours to obtain a uniform solution. 0.3 g of 2-hydroxy-2-methylpropylamine was further added to the obtained solution, and the mixture was stirred to obtain a solution containing a silver complex. The solution was filtered using a PTFE (polytetrafluoroethylene) membrane filter having a pore size of 0.45 μm to obtain a conductive ink 1 containing a silver complex.
[0332] The obtained conductive ink 1 was used as the first ink in step 1 and the second ink in step 2.
[0333] <Process 1>
[0334] The conductive ink 1 was used as the first ink and filled into an ink cartridge (for 10 picoliters) of an inkjet recording device (product name "DMP-2850", manufactured by FUJIFILM DIMATIX). A UVSpot Cure device ("OmniCure S2000", manufactured by Lumen Dynamics, wavelength 385 nm) was installed on the side of the head of the inkjet recording device at a position 7 cm away from the nozzle position of the inkjet.
[0335] As image recording conditions of the inkjet recording apparatus, the resolution was set to 1200 dpi (dots per inch), the droplet ejection amount was set to 10 picoliters per dot, the ejection frequency was set to 4 kHz, and the head temperature during ejection was set to 30°C.
[0336] The substrate (a glass epoxy substrate with an insulating film composed of solder resist formed on the surface) was fixed to the workbench of the inkjet recording device, and when the substrate was viewed from above, the printing origin was aligned with the upper left corner of the frame-shaped ground electrode. Next, the conductive ink 1 was ejected onto the surface of the solder resist film under the above-mentioned image recording conditions to form a first coating film composed of a solid image with a size of 2 cm in width and 2 cm in length. At this time, immediately after the conductive ink 1 was ejected (within 2 seconds from the landing of the conductive ink 1), the first coating film was irradiated with UV light (exposure amount: 6 J / cm 2 ). And, the thickness of the formed first coating film was 20 μm. Then, after the formation of the first coating film, the substrate was heated at 160° C. for 20 minutes using a heating plate to obtain a single film of the first conductive film. In addition, the heating of the substrate was started 60 seconds after the formation of the first coating film was completed. A series of operations including the formation of the first coating film and the first curing treatment including the light irradiation treatment and the heat treatment were repeated as 10 cycles to form a 10-layer laminate consisting of the first conductive film.
[0337] <Process 2>
[0338] The conductive ink 1 described above was used as the second ink and filled into the ink tank of the inkjet recording device in the same manner as in step 1.
[0339] The heating temperature of the substrate during the heat treatment was changed to 180°C. In addition, a second coating film consisting of a solid image with a size of 2 cm in width and 2 cm in length was formed on the first conductive film formed by the process 1 according to the method described as process 1. Then, a second curing treatment consisting of a light irradiation treatment and a heat treatment was performed, thereby forming a single film of the second conductive film. A series of operations including the formation of the second coating film and the second curing treatment including the light irradiation treatment and the heat treatment were repeated 4 times as one cycle, and a laminated body consisting of 4 layers of the second conductive film was formed, thereby obtaining the conductor of Example 1.
[0340] The thickness of the conductive film of the produced conductor of Example 1 (the total thickness of the first conductive film and the thickness of the second conductive film) was 5.8 μm.
[0341] [Examples 2 to 12, 14 to 22 and Comparative Examples 1 to 4]
[0342] In at least one of process 1 and process 2, at least one of the image recording conditions (resolution), the heating temperature and heating time of the heat treatment, the exposure amount in the light irradiation treatment, and the number of cycles is changed to the conditions described in Tables 1 to 3 described later. In addition, the first conductive film and the second conductive film are formed according to the method described in Example 1, and each conductor is produced.
[0343] In Examples 3, 4, 7, 9 to 12, 15 to 18, and 20 to 22 and Comparative Example 3, in the second curing treatment included in Step 2, as the light irradiation treatment, in addition to irradiating with UV light (exposure amount: 6 J / cm 2 ), and the solid image subjected to heat treatment using a hot plate was irradiated with UV having an exposure amount described in Tables 1 to 3 using a UV-LED lamp (manufactured by KYOCERA Corporation, wavelength 385 nm) to form a single film of the conductive film.
[0344] [Example 13, Comparative Example 5]
[0345] <Step 3 (Formation of Insulating Film Using Insulating Ink)>
[0346] The following components were added to a 300 mL resin beaker, and the obtained mixture was stirred for 20 minutes at 25° C. and 5000 rpm using a mixer (product name “L4R”, manufactured by Silverson Nippon Limited) to obtain insulating ink 1.
[0347] Isobornyl acrylate (manufactured by FUJIFILM Wako Pure Chemical Corporation): 34.0 g
[0348] N-vinyl caprolactam: 22.0g
[0349] 1,6-Hexanediol diacrylate: 30.0 g
[0350] · Trimethylolpropane triacrylate (manufactured by FUJIFILM Wako Pure Chemical Corporation): 8.0 g
[0351] Polymerization initiator (2-(dimethylamino)-2-(4-methylbenzyl)-1-(4-morpholinophenyl)-butan-1-one, product name "Omnirad (registered trademark) 379", manufactured by IGM Resins BV): 4.0 g
[0352] Sensitizer (2-isopropylthioxanthone, product name "SPEEDCURE (registered trademark) ITX", manufactured by LAMBSON): 2.0 g
[0353] The insulating ink 1 was filled into an ink cartridge (for 10 picoliters) of an inkjet recording apparatus (product name "DMP-2850", manufactured by FUJIFILM DIMATIX). As described above, the UVSpot Cure apparatus was mounted on the inkjet recording apparatus.
[0354] As image recording conditions of the inkjet recording apparatus, the resolution was set to 1200 dpi, the droplet ejection amount was set to 10 picoliters per dot, the ejection frequency was set to 16 kHz, and the head temperature during ejection was set to 45°C.
[0355] The substrate (glass epoxy substrate with solder resist film formed on the surface) was fixed on the workbench of the inkjet recording device, and the printing origin was aligned with the upper left corner of the frame-shaped ground electrode. Next, the insulating ink 1 was ejected onto the surface of the solder resist film under the above-mentioned image recording conditions to form a solid image with a width of 3 cm and a length of 3 cm. The formed solid image was irradiated with UV light (exposure amount: 4 J / cm 2 ), thereby forming an insulating film 2. The thickness of the formed insulating film 2 was 21 μm.
[0356] <Production of Conductor>
[0357] Conductors of Example 13 and Comparative Example 5 were produced according to the methods described in Example 9 and Comparative Example 1, except that the first conductive film and the second conductive film were formed on the formed insulating film 2, respectively.
[0358] [evaluate]
[0359] <Abrasion resistance>
[0360] The conductive film of each conductor was rubbed 20 times using a white cotton swab, and then the changes in the appearance of the conductive film in the rubbed area (rubbed area) and the adhesion of the conductive film on the cotton swab were observed, and the abrasion resistance was evaluated according to the following criteria based on the observation results.
[0361] (Abrasion resistance evaluation standard)
[0362] 5: There is no change in the appearance of the rubbed area, and no conductive film is observed to be attached to the cotton swab.
[0363] 4: There was no change in the appearance of the rubbed area, but black or silver deposits were slightly observed on the cotton swab.
[0364] 3: Slight scratches were observed in the rubbed area, and black or silver deposits were also observed on the cotton swab, but exposure of the lower layer (insulating film) was not observed.
[0365] 2: Clear scratches from the rubbed area are observed, and the area ratio of the rubbed area to the area where the underlying layer is exposed is less than 10%.
[0366] 1: Clear scratches from scratching are observed in the scratched area, and the area ratio of the scratched area to the area where the lower layer is exposed is 10% or more.
[0367] <Adhesion>
[0368] The conductive film of each manufactured conductor was subjected to a cross-hatch test by the following method. Six cuts were made in mutually orthogonal directions relative to the surface of the conductive film. After a tape piece of transparent tape ("Cellotape (registered trademark) CT-18", manufactured by Nichiban Co. Ltd.) was attached to the conductive film with the cuts, the tape piece was peeled off from the conductive film. The peeling of the conductive film on the surface from which the tape piece was peeled (exposure of the lower layer) and the amount of the conductive film attached to the peeled tape piece were observed, and the adhesion was evaluated according to the following criteria based on the observation results.
[0369] (Adhesion Evaluation Criteria)
[0370] 5: No peeling was observed on the surface of the conductive film, and no black or silver attachment was observed on the tape piece.
[0371] 4: Peeling of the conductive film was observed only at the intersections of the cuts on the conductive film surface, and / or black or silver deposits were slightly observed on the tape piece.
[0372] 3: Peeling of the conductive film was observed only at the intersections of the cuts on the conductive film surface, and black or silver deposits were observed in the tape piece adhering to an area less than 10% of the area of the portion cut by the crosshatch.
[0373] 2: On the surface of the conductive film, peeling of the conductive film is observed over an area less than 10% of the area of the portion cut by the cross-hatch pattern, and / or black or silver attached matter is observed on the tape sheet over an area greater than 10% and less than 50% of the area of the portion cut by the cross-hatch pattern.
[0374] 1: On the surface of the conductive film, peeling of the conductive film is observed over an area of 10% or more relative to the area of the portion cut by the cross-hatch pattern, and / or black or silver deposits are observed on the tape sheet over an area of 50% or more relative to the area of the portion cut by the cross-hatch pattern.
[0375] The following Tables 1 to 3 show the production conditions and evaluation results of each production method.
[0376] In the table, “Substrate 1” in the “Substrate” column refers to a substrate with a solder resist film having a first conductive film formed on a surface of a solder resist film, and “Substrate 2” refers to a substrate with a first conductive film formed on a surface of an insulating film formed using insulating ink 1.
[0377] In the table, the columns of "Step 1" and "Step 2" respectively show the processing conditions of Step 1 and Step 2.
[0378] The numerical value in the column of "resolution (dpi)" indicates the resolution when the first coating film or the second coating film is formed by inkjet recording.
[0379] The numerical values in the columns of “film thickness L1 (μm)” and “film thickness L2 (μm)” indicate the thickness of the first coating film and the second coating film, respectively.
[0380] "Exposure E1a (J / cm 2 )" column and "Exposure E2a (J / cm 2 The values in the ")" column represent the exposure amount of UV light applied immediately after the conductive ink is discharged in each process.
[0381] The numerical values in the columns "Heating temperature T1 (° C.)" and "Heating temperature T2 (° C.)" indicate the heating temperatures in the heat treatments for the first coating film and the second coating film, respectively.
[0382] The numerical values in the columns of “heating time t1 (minutes)” and “heating time t2 (minutes)” indicate the heating time in the heat treatment for each of the first coating film and the second coating film.
[0383] "Exposure E2b (J / cm 2 The numerical values in the ")" column represent the exposure amount of UV light irradiated after the heat treatment of the second coating film.
[0384] "Exposure E1(J / cm 2 )" column and "Exposure E2 (J / cm 2 The numerical value in the ")" column represents the total exposure amount of UV light irradiated to each of the first coating film and the second coating film.
[0385] The numerical value in the column of “Number of Cycles” indicates the number of a series of treatment cycles including the formation of the coating film and the curing treatment performed in each step.
[0386] The column "Formula (1)" of "Conductor" indicates the value of variable A1 calculated by formula (1), and the column "Formula (2)" indicates the value of variable A2 calculated by formula (2). When the value in the column "Formula (1)" is 1.2 or more, it means that formula (1) is satisfied, and when the value in the column "Formula (2)" is 2.0 or more, it means that formula (2) is satisfied.
[0387]
[0388]
[0389]
[0390] From the results shown in the above table, it was confirmed that the production method of the present invention was superior in at least one of adhesion and abrasion resistance compared to the methods of Comparative Examples 1 to 5 which did not satisfy the formula (1) and the formula (2).
[0391] It was confirmed that the greater the variable A1 calculated by the formula (1), the better the adhesion and abrasion resistance (for example, comparison between Examples 1, 2, and 19).
[0392] Furthermore, it was confirmed that the greater the variable A2 calculated by the formula (2), the better the adhesion and abrasion resistance (for example, comparison between Examples 20, 3, and 4).
[0393] Furthermore, it was confirmed that at least one of the adhesion and abrasion resistance was superior compared to the case where the manufacturing method of the conductor satisfied both equations (1) and (2) or the case where only one of equations (1) and (2) was satisfied (for example, comparison between Examples 1, 2, 4, 21 and 22).
Claims
1. A method for manufacturing an electrical conductor, include: An ink preparation step of preparing a first ink containing at least a metal salt or a metal complex and a second ink containing at least a metal salt or a metal complex; Step 1, after forming a first coating film on a substrate using the first ink, subjecting the first coating film to a first curing treatment of at least one selected from the group consisting of a heating treatment and a light irradiation treatment to form a first conductive film; and Step 2, after forming a second coating film on the first conductive film using the second ink, subjecting the second coating film to a second curing treatment of at least one selected from the group consisting of a heat treatment and a light irradiation treatment to form a second conductive film, The method for manufacturing the conductor satisfies at least one of equations (1) and (2), Formula (1) 1.2≤{(T2-23)×t2 / L2} / {(T1-23)×t1 / L1} Formula (2) 2.0≤(E2 / L2) / (E1 / L1) Wherein, L1 and L2 represent the thickness of the first coating film and the second coating film, respectively, in μm. T1 and T2 represent the heating temperatures of the heating treatments performed as the first curing treatment and the second curing treatment, respectively, and the unit is °C. t1 and t2 represent the heating time of the heating treatment performed as the first curing treatment and the second curing treatment, respectively, in minutes. E1 and E2 represent the exposure doses of the light irradiation treatments performed as the first curing treatment and the second curing treatment, respectively, and the unit is J / cm 2 .
2. The method for producing an electrical conductor according to claim 1, in, The first ink and the second ink are the same.
3. The method for producing a conductor according to claim 1 or 2, in, In the step 1, the heat treatment is performed as the first curing treatment, and in the step 2, the heat treatment is performed as the second curing treatment.
4. The method for producing a conductor according to claim 1 or 2, in, In the step 1, the light irradiation treatment is performed as the first curing treatment, and in the step 2, the light irradiation treatment is performed as the second curing treatment.
5. The method for producing a conductor according to claim 1 or 2, in, In the step 1, both the heating treatment and the light irradiation treatment are performed as the first curing treatment, and in the step 2, both the heating treatment and the light irradiation treatment are performed as the second curing treatment.
6. The method for producing a conductor according to claim 1 or 2, in, The thickness of the second coating film formed in the step 2 is smaller than the thickness of the first coating film formed in the step 1.
7. The method for producing an electrical conductor according to claim 1 or 2, in, The method further includes forming an insulating film on the substrate to produce a substrate with an insulating film. The step 1 is a step of forming the first conductive film on the insulating film of the substrate with an insulating film produced in the step 3.
8. A method for producing an electromagnetic wave shield, comprising the step of forming a conductive film on a substrate according to the method for producing a conductor according to claim 1 or 2.