Method for manufacturing conductive layer

By degassing the conductive ink, the stability problem of conductive ink during storage and ejection is solved, the conductivity of the conductive layer is improved, and the storage and ejection stability and conductivity of the ink are improved.

CN118900778APending Publication Date: 2024-11-05FUJIFILM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202380028299.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-27
Publication Date
2024-11-05

Smart Images

  • Figure BDA0005047018280000271
    Figure BDA0005047018280000271
Patent Text Reader

Abstract

The present invention addresses the problem of providing a method for producing a conductive layer with which it is possible to form a conductive layer having excellent storage stability and discharge stability of an ink and excellent conductivity. A method for manufacturing a conductive layer according to the present invention comprises: a degassing step for degassing a conductive ink contained in an ink container; and a conductive layer formation step for forming a conductive layer by discharging a degassed conductive ink from a nozzle using an ink jet recording method and applying the degassed conductive ink to the substrate, the conductive ink including at least one material selected from the group consisting of a metal salt, a metal complex, and metal particles. When the amount of dissolved oxygen in the conductive ink before the degassing step is defined as dissolved oxygen amount A and the amount of dissolved oxygen in the degassed conductive ink after the degassing step is defined as dissolved oxygen amount B, the value obtained by subtracting the amount of dissolved oxygen amount B from the amount of dissolved oxygen amount A is greater than 15 mg / L.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a conductive layer. Background Art

[0002] A method of forming a conductive layer by applying a conductive ink containing a metal component to a substrate using an inkjet recording method is widely known. As a conductive ink used in such an inkjet recording method, Patent Document 1 discloses a conductive composition comprising a branched metal carboxylate (e.g., silver neodecanoate) and an aromatic hydrocarbon solvent and an aliphatic solvent in which the branched metal carboxylate is soluble.

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-109273 Summary of the invention

[0006] Technical issues to be solved by the invention

[0007] It is required that the ink for inkjet recording be normally ejected from the nozzles of the inkjet recording apparatus, that is, the ink ejection stability be excellent.

[0008] Ink for inkjet recording may be ejected from the nozzle of the inkjet head after being stored in the ink container. For example, when using ink containing metal salts, metal complexes or metal particles, the metal salts, metal complexes or metal particles may be reduced during the storage of the ink, so that the physical properties of the ink before and after storage change greatly. Therefore, it is required to have less physical property changes before and after storage of the ink, that is, an ink with excellent storage stability.

[0009] Furthermore, the conductivity of the conductive layer formed using the ink for inkjet recording is required to be further improved.

[0010] The present inventors used the conductive composition described in Patent Document 1 as ink for inkjet recording and found that at least one of the storage stability of the ink, the ejection stability of the ink, and the conductivity of the conductive layer may not meet the level required in recent years, and that there is room for improvement.

[0011] Therefore, an object of the present invention is to provide a method for producing a conductive layer that can form a conductive layer having excellent ink storage stability and discharge stability and excellent conductivity.

[0012] Means for solving technical problems

[0013] The present inventors conducted intensive research to solve the above-mentioned problems, and as a result, found that in a method for manufacturing a conductive layer having a degassing step of degassing ink containing a metal component contained in an ink container and a conductive layer forming step of forming a conductive layer based on the degassed ink using an inkjet recording method, when the value obtained by subtracting the dissolved oxygen amount B in the degassed ink after the degassing step from the dissolved oxygen amount A in the ink before the degassing step is greater than 15 mg / L, the desired effect can be obtained, thereby completing the present invention.

[0014] That is, the present inventors have found that the above-mentioned problems can be solved by the following configuration. [1]

[0016] A method for manufacturing a conductive layer, comprising the following steps:

[0017] a degassing step of degassing the conductive ink contained in the ink container; and

[0018] The conductive layer forming step uses an inkjet recording method to eject degassed conductive ink from a nozzle and apply it to the substrate to form a conductive layer.

[0019] The conductive ink comprises at least one material selected from the group consisting of metal salts, metal complexes and metal particles.

[0020] When the amount of dissolved oxygen in the conductive ink before the degassing step is defined as dissolved oxygen amount A and the amount of dissolved oxygen in the degassed conductive ink after the degassing step is defined as dissolved oxygen amount B, a value obtained by subtracting the amount of dissolved oxygen B from the amount of dissolved oxygen A is greater than 15 mg / L. [2]

[0022] The method for manufacturing a conductive layer according to [1], wherein:

[0023] The dissolved oxygen amount B is 10 mg / L or less. [3]

[0025] The method for producing a conductive layer according to [1] or [2], wherein:

[0026] The metal constituting the metal salt, the metal complex, and the metal particles includes at least one of silver and copper. [4]

[0028] The method for producing a conductive layer according to any one of [1] to [3], wherein:

[0029] The conductive ink includes at least one of the metal salt and the metal complex. [5]

[0031] The method for producing a conductive layer according to any one of [1] to [4], wherein:

[0032] When the molar concentration of the metal in the conductive ink is represented by Mm and the molar concentration of dissolved oxygen in the degassed conductive ink after the degassing step is represented by Mb, the value of Mm / Mb is 1,700 to 100,000.

[0033] The units of the above-mentioned Mm and Mb are both mmol / L. [6]

[0035] The method for producing a conductive layer according to any one of [1] to [5], wherein:

[0036] The conductive layer forming step includes a curing process in which the degassed conductive ink applied to the substrate is cured by at least one of heating and light irradiation.

[0037] The time from when the degassed ink lands on the substrate to when the heating or light irradiation starts is within 1 second. [7]

[0039] The method for producing a conductive layer according to any one of [1] to [6], wherein:

[0040] The temperature of the conductive ink during the degassing step is 30° C. or higher.

[0041] Effects of the Invention

[0042] According to the present invention, there can be provided a method for producing a conductive layer capable of forming a conductive layer having excellent ink storage stability and discharge stability and excellent conductivity. DETAILED DESCRIPTION

[0043] Hereinafter, the present invention will be described in detail.

[0044] Although the description of the constituent elements described below may be made based on representative embodiments of the present invention, the present invention is not limited to such embodiments.

[0045] In addition, in this specification, the numerical range represented by "~" refers to a range that includes the numerical values ​​recorded before and after "~" as the lower limit and upper limit. In the numerical range recorded in stages in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Moreover, in the numerical range recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiment.

[0046] In this specification, each component may be used alone or in combination of two or more substances. When two or more substances are used for each component, the content of the component refers to the total content of the two or more substances unless otherwise specified.

[0047] In the present specification, a combination of two or more preferred aspects is a more preferred aspect.

[0048] In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0049] [Method for producing conductive layer]

[0050] The method for manufacturing a conductive layer of the present invention comprises: a degassing step of degassing a conductive ink contained in an ink container; and a conductive layer forming step of ejecting the degassed conductive ink from a nozzle using an inkjet recording method and applying it to a substrate, thereby forming a conductive layer. In addition, the conductive ink contains at least one material selected from the group consisting of metal salts, metal complexes, and metal particles. In addition, when the amount of dissolved oxygen in the conductive ink before the degassing step is set as dissolved oxygen amount A and the amount of dissolved oxygen in the degassed conductive ink after the degassing step is set as dissolved oxygen amount B, the value of subtracting the amount of dissolved oxygen B from the amount of dissolved oxygen A is greater than 15 mg / L.

[0051] According to the method for producing a conductive layer of the present invention, a conductive layer having excellent ink storage stability and discharge stability and excellent conductivity can be formed. The details of the reason are not clear, but it is roughly estimated as follows.

[0052] When the value obtained by subtracting the dissolved oxygen amount B from the dissolved oxygen amount A is sufficiently large, the reduction of the metal salt, metal complex or metal particles contained in the conductive ink is suppressed during the storage of the conductive ink before the degassing process, so it is speculated that the ink has excellent storage stability. In addition, it is speculated that when the conductive ink is ejected, since the amount of dissolved oxygen in the conductive ink is small, the nozzle detachment and nozzle clogging caused by the generation of bubbles are suppressed, and as a result, the ink has excellent ejection stability. In addition, it is speculated that since there are few bubbles in the droplets of the conductive ink, the area (pores) where the conductive material does not exist in the obtained conductive layer becomes less, and as a result, the volume resistivity of the conductive layer decreases and a conductive layer with excellent conductivity is obtained. In addition, since there is less oxygen in the conductive ink that suppresses reduction, the reduction of the metal salt, metal complex or metal particles in the conductive ink ejected from the nozzle is accelerated, and as a result, a conductive layer with excellent conductivity can be obtained.

[0053] <Conductive ink>

[0054] Conductive ink refers to ink used to form a layer having conductivity (i.e., conductive layer). Conductivity means that the volume resistivity is less than 10 8 Properties of Ωcm.

[0055] The conductive ink includes at least one material selected from the group consisting of metal salts, metal complexes, and metal particles.

[0056] Among them, from the viewpoint of more excellent effects of the present invention, the conductive ink preferably contains at least one of a metal salt and a metal complex, and more preferably contains at least one of a metal salt and a metal complex and does not contain metal particles.

[0057] In the following, ink containing metal particles (hereinafter also referred to as "metal particle ink"), ink containing metal complexes (hereinafter also referred to as "metal complex ink"), and ink containing metal salts (hereinafter also referred to as "metal salt ink") are described respectively.

[0058] Among them, the conductive ink is preferably a metal salt ink or a metal complex ink from the viewpoint of achieving more excellent effects of the present invention.

[0059] (Metallic Particle Ink)

[0060] The metal particle ink is, for example, a conductive ink in which metal particles are dispersed in a dispersion medium.

[0061] -Metal particles-

[0062] As metals constituting the metal particles, for example, particles of base metals and noble metals can be cited. As base metals, for example, nickel, titanium, cobalt, copper, chromium, manganese, iron, zirconium, tin, tungsten, molybdenum and vanadium can be cited. As noble metals, for example, gold, silver, platinum, palladium, iridium, osmium, ruthenium, rhodium, rhenium and alloys containing these metals can be cited. Among them, from the viewpoint of conductivity, the metal constituting the metal particles preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium and copper, more preferably includes at least one of silver and copper, and further preferably includes silver.

[0063] In the present invention, the definition of "metal particles" does not include metal oxide particles such as titanium oxide.

[0064] The average particle size of the metal particles is not particularly limited, and is preferably 10 to 500 nm, more preferably 10 nm to 200 nm. If the average particle size is within the above range, the sintering temperature of the metal particles decreases, and the process suitability of the conductive layer is improved. In particular, since an inkjet recording method is used in the present invention, there is a tendency that the ejection property of the ink is improved, and the pattern formation and the uniformity of the thickness of the conductive layer are improved. The average particle size mentioned here refers to the average value of the primary particle size of the metal particles (average primary particle size).

[0065] The average particle size of the metal particles is measured by a laser diffraction / scattering method. The average particle size of the metal particles is, for example, a value calculated by measuring 3 times the 50% volume cumulative diameter (D50) and taking the average of the values ​​measured 3 times, and can be measured using a laser diffraction / scattering particle size distribution measuring device (product name "LA-960", manufactured by HORIBA, Ltd.).

[0066] Furthermore, the metal particle ink may contain metal particles having an average particle size of 500 nm or more as required. When metal particles having an average particle size of 500 nm or more are contained, the melting point of the nm-sized metal particles is lowered around the μm-sized metal particles, thereby enabling the metal particles to be bonded to each other.

[0067] In the metal particle ink, the content of the metal particles is preferably 10 to 90% by mass, and more preferably 20 to 50% by mass, relative to the total mass of the metal particle ink. If the content of the metal particles is 10% by mass or more, the surface resistivity of the conductive film is further reduced. If the content of the metal particles is 90% by mass or less, the ejection stability of the metal particle ink is more excellent.

[0068] The metal particle ink may contain, in addition to the metal particles, for example, a dispersant, a resin, a dispersion medium, a thickener, and a surface tension adjuster.

[0069] -Dispersant-

[0070] The metal particle ink may contain a dispersant attached to at least a portion of the surface of the metal particles. The dispersant and the metal particles substantially constitute metal colloid particles. The dispersant has the function of coating the metal particles to improve the dispersibility of the metal particles and prevent aggregation. The dispersant is preferably an organic compound capable of forming metal colloid particles. From the viewpoint of conductivity and dispersion stability, the dispersant is preferably an amine, a carboxylic acid or a salt thereof, an alcohol or a resin dispersant.

[0071] The dispersant contained in the metal particle ink may be one kind or two or more kinds.

[0072] Examples of the amine include aliphatic amines and aromatic amines.

[0073] The aliphatic amine may be saturated or unsaturated. Among them, the aliphatic amine is preferably an aliphatic amine having 4 to 8 carbon atoms. The aliphatic amine having 4 to 8 carbon atoms may be linear, branched, or have a ring structure.

[0074] Specific examples of the aliphatic amine include butylamine, n-pentylamine, isopentylamine, hexylamine, 2-ethylhexylamine, and octylamine.

[0075] Specific examples of the amine having an alicyclic structure include cycloalkylamines such as cyclopentylamine and cyclohexylamine.

[0076] A specific example of the aromatic amine is aniline.

[0077] The amine may have a functional group other than an amino group. Examples of the functional group other than an amino group include a hydroxyl group, a carboxyl group, an alkoxy group, a carbonyl group, an ester group, and a mercapto group.

[0078] Specific examples of the carboxylic acid include formic acid, oxalic acid, acetic acid, caproic acid, acrylic acid, octanoic acid, oleic acid, tianshic acid, ricinoleic acid, gallic acid, and salicylic acid.

[0079] Examples of the carboxylate salt include metal salts of carboxylic acids. The metal ions forming the metal salt of carboxylic acids may be one type or two or more types.

[0080] The carboxylic acid and the carboxylate may have a functional group other than the carboxyl group. Examples of the functional group other than the carboxyl group include an amino group, a hydroxyl group, an alkoxy group, a carbonyl group, an ester group, and a mercapto group.

[0081] Specific examples of alcohol include terpene alcohol, allyl alcohol, and oleyl alcohol. Alcohols are easily coordinated to the surface of metal particles and can suppress aggregation of metal particles.

[0082] Examples of the resin dispersant include a dispersant having a nonionic group as a hydrophilic group and capable of being uniformly dissolved in a solvent.

[0083] Specific examples of the resin dispersant include polyvinyl pyrrolidone, polyethylene glycol, polyethylene glycol-polypropylene glycol copolymer, polyvinyl alcohol, polyallylamine, and polyvinyl alcohol-polyvinyl acetate copolymer.

[0084] The weight average molecular weight of the resin dispersant is preferably 1,000 to 50,000, more preferably 1,000 to 30,000.

[0085] In the metal particle ink, the content of the dispersant is preferably 0.5 to 50% by mass, more preferably 1 to 30% by mass, based on the total mass of the metal particle ink.

[0086] -Dispersion medium-

[0087] The metal particle ink preferably contains a dispersion medium. The type of the dispersion medium is not particularly limited, and examples thereof include hydrocarbons, alcohols, and water.

[0088] The dispersion medium contained in the metal particle ink may be one kind or two or more kinds.

[0089] The dispersion medium contained in the metal particle ink is preferably volatile.

[0090] The boiling point of the dispersion medium is preferably 50 to 250° C., more preferably 70 to 220° C., and even more preferably 80 to 200° C. When the boiling point of the dispersion medium is 50 to 250° C., there is a tendency that both stability and sinterability of the metal particle ink can be achieved.

[0091] In this specification, unless otherwise specified, the boiling point means the normal boiling point.

[0092] Examples of the hydrocarbons include aliphatic hydrocarbons and aromatic hydrocarbons.

[0093] Specific examples of aliphatic hydrocarbons include saturated or unsaturated aliphatic hydrocarbons such as tetradecane, octadecane, heptamethylnonane, tetramethylpentadecane, hexane, heptane, octane, nonane, decane, tridecane, methylpentane, normal paraffins, and isoparaffins.

[0094] Specific examples of aromatic hydrocarbons include toluene and xylene.

[0095] Examples of the alcohol include aliphatic alcohols and alicyclic alcohols. When an alcohol is used as the dispersion medium, the dispersant is preferably an amine or a carboxylic acid or a salt thereof.

[0096] Specific examples of aliphatic alcohols include aliphatic alcohols having 6 to 20 carbon atoms which may contain ether bonds in the saturated or unsaturated chain, such as heptanol, octanol (e.g., 1-octanol, 2-octanol, 3-octanol, etc.), decanol (e.g., 1-decanol, etc.), lauryl alcohol, tetradecanol, cetyl alcohol, 2-ethyl-1-hexanol, octadecanol, hexadecenol and oleyl alcohol.

[0097] Specific examples of alicyclic alcohols include cycloalkanols such as cyclohexanol; terpene alcohols such as terpineol (including α, β, γ isomers or any mixtures thereof) and dihydroterpineol; myrtenol, sobrerol, menthol, carveol, perillyl alcohol, pinocarveol, sobrerol and verbenol.

[0098] The dispersion medium may be water. From the viewpoint of adjusting physical properties such as viscosity, surface tension, and volatility, the dispersion medium may be a mixed solvent of water and other solvents.

[0099] The other solvent miscible with water is preferably an alcohol or a glycol ether. The alcohol or glycol ether used together with water is preferably an alcohol or glycol ether miscible with water and having a boiling point of 130° C. or less.

[0100] Specific examples of the alcohol include 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, and 1-pentanol.

[0101] Specific examples of the glycol ether include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and propylene glycol monomethyl ether.

[0102] In the metal particle ink, the content of the dispersion medium is preferably 1 to 50% by mass, more preferably 10 to 45% by mass, and further preferably 20 to 40% by mass relative to the total mass of the metal particle ink. If the content of the dispersion medium is 1 to 50% by mass, sufficient conductivity as a conductive ink can be obtained.

[0103] -Resin-

[0104] The metallic particle ink may contain a resin.

[0105] Examples of the resin include polyester, polyurethane, melamine resin, acrylic resin, styrene resin, polyether, and terpene resin.

[0106] The metal particle ink may contain one type of resin or two or more types of resin.

[0107] In the metal particle ink, the content of the resin is preferably 0.1 to 5% by mass relative to the total mass of the metal particle ink.

[0108] -Thickener-

[0109] The metallic particle ink may contain a thickener.

[0110] Specific examples of the thickener include clay minerals such as clay, bentonite, and lithium bentonite; cellulose derivatives such as methylcellulose, carboxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, and hydroxypropylmethylcellulose; and polysaccharides such as xanthan gum and guar gum.

[0111] The thickener contained in the metal particle ink may be one kind or two or more kinds.

[0112] In the metal particle ink, the content of the thickener is preferably 0.1 to 5% by mass relative to the total mass of the metal particle ink.

[0113] -Surfactant-

[0114] The metal particle ink may contain a surfactant. If the metal particle ink contains a surfactant, a uniform conductive ink film can be easily formed.

[0115] The surfactant may be any of anionic surfactants, cationic surfactants and nonionic surfactants. Among them, the surfactant is preferably a fluorine-based surfactant from the viewpoint of being able to adjust the surface tension with a small amount of content. In addition, the surfactant is preferably a compound having a boiling point exceeding 250°C.

[0116] -Physical properties of metal particle ink-

[0117] The viscosity of the metal particle ink is preferably 1 to 100 mPa·s, more preferably 2 to 50 mPa·s, and even more preferably 3 to 30 mPa·s.

[0118] The viscosity of the metal particle ink is a value measured at 25° C. using a viscometer.

[0119] The viscosity is measured using, for example, a VISCOMETER TV-22 type viscometer (manufactured by TOKI SANGYO CO., LTD.).

[0120] The surface tension of the metal particle ink is not particularly limited, but is preferably 20 to 45 mN / m, more preferably 25 to 40 mN / m.

[0121] The surface tension is a value measured using a surface tensiometer at 25° C. The surface tension of the metal particle ink is measured using, for example, DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).

[0122] -Method for producing metal particles-

[0123] The metal particles can be commercially available products or metal particles manufactured by a known method. As a method for manufacturing metal particles, for example, a wet reduction method, a gas phase method and a plasma method can be cited. As a preferred method for manufacturing metal particles, a wet reduction method that can manufacture metal particles with an average particle size of less than 200 nm to narrow the particle size distribution can be cited. The method for manufacturing metal particles based on the wet reduction method can, for example, be the method described in Japanese Patent Publication No. 2017-037761, International Publication No. 2014-057633, etc., which method includes: a step of mixing a metal salt and a reducing agent to obtain a complex reaction solution; and a step of heating the complex reaction solution to reduce the metal ions in the complex reaction solution to obtain a slurry of metal nanoparticles.

[0124] In the manufacture of the metal particle ink, a heat treatment may be performed in order to adjust the content of each component contained in the metal particle ink to a predetermined range. The heat treatment may be performed under reduced pressure or under normal pressure. Furthermore, when performed under normal pressure, the heat treatment may be performed in the air or under an inert gas environment.

[0125] (Metal Complex Ink)

[0126] The metal complex ink is, for example, a conductive ink in which a metal complex is dissolved in a solvent.

[0127] -Metal Complex-

[0128] Examples of the metal constituting the metal complex include silver, copper, gold, aluminum, magnesium, tungsten, molybdenum, zinc, nickel, iron, platinum, tin, copper, and lead. Among them, from the viewpoint of conductivity, the metal constituting the metal complex preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium, and copper, more preferably includes at least one of silver and copper, and further preferably includes silver.

[0129] The content of the metal contained in the metal complex ink is preferably 1 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 20% by mass, based on the total mass of the metal complex ink, in terms of metal element.

[0130] The metal complex is obtained, for example, by reacting a metal salt with a complexing agent. As a method for producing the metal complex, for example, a method in which a metal salt and a complexing agent are added to an organic solvent and stirred for a predetermined time can be cited. The stirring method is not particularly limited and can be appropriately selected from known methods such as a method of stirring using a stirrer, a stirring blade or a mixer, and a method of applying ultrasonic waves.

[0131] Examples of the metal salt include metal oxides, thiocyanates, sulfides, chlorides, cyanides, cyanates, carbonates, acetates, nitrates, nitrites, sulfates, phosphates, perchlorates, tetrafluoroborates, acetylacetonato complexes, and carboxylates.

[0132] Examples of the complexing agent include amines, ammonium carbamate compounds, ammonium carbonate compounds, ammonium bicarbonate compounds, and carboxylic acids. From the viewpoint of conductivity and stability of the metal complex, the complexing agent preferably includes at least one selected from the group consisting of ammonium carbamate compounds, ammonium carbonate compounds, amines, and carboxylic acids having 8 to 20 carbon atoms.

[0133] The metal complex has a structure derived from the complexing agent, and is preferably a metal complex having a structure derived from at least one selected from the group consisting of ammonium carbamate compounds, ammonium carbonate compounds, amines, and carboxylic acids having 8 to 20 carbon atoms.

[0134] Examples of the amine as the complexing agent include ammonia, primary amines, secondary amines, tertiary amines, and polyamines.

[0135] Specific examples of the primary amine having a linear alkyl group include methylamine, ethylamine, 1-propylamine, n-butylamine, n-pentylamine, n-hexylamine, heptylamine, octylamine, nonylamine, n-decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecylamine and octadecylamine.

[0136] Specific examples of the primary amine having a branched alkyl group include isopropylamine, sec-butylamine, tert-butylamine, isopentylamine, 2-ethylhexylamine, and tert-octylamine.

[0137] Specific examples of the primary amine having an alicyclic structure include cyclohexylamine and dicyclohexylamine.

[0138] Specific examples of the primary amine having a hydroxyalkyl group include ethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, propanolamine, isopropanolamine, dipropanolamine, diisopropanolamine, tripropanolamine, and triisopropanolamine.

[0139] Specific examples of the primary amine having an aromatic ring include benzylamine, N,N-dimethylbenzylamine, phenylamine, diphenylamine, triphenylamine, aniline, N,N-dimethylaniline, N,N-dimethyl-p-toluidine, 4-aminopyridine, and 4-dimethylaminopyridine.

[0140] Specific examples of the secondary amine include dimethylamine, diethylamine, dipropylamine, dibutylamine, diphenylamine, dicyclopentylamine, and methylbutylamine.

[0141] Specific examples of the tertiary amine include trimethylamine, triethylamine, tripropylamine, and triphenylamine.

[0142] Specific examples of the polyamine include ethylenediamine, 1,3-diaminopropane, diethylenetriamine, triethylenetetramine, tetramethylenepentamine, hexamethylenediamine, tetraethylenepentamine, and combinations thereof.

[0143] The amine is preferably an alkylamine, more preferably an alkylamine having 3 to 10 carbon atoms, and still more preferably a primary alkylamine having 4 to 10 carbon atoms.

[0144] The amines constituting the metal complex may be one type or two or more types.

[0145] When the metal salt and the amine are reacted, the ratio of the amount of the amine to the amount of the metal salt is preferably 1 to 15 times, more preferably 1.5 to 6 times. When the ratio is within the above range, the complex formation reaction is completed and a transparent solution can be obtained.

[0146] Specific examples of the ammonium carbamate compounds used as complexing agents include ammonium carbamate, methylammonium methylcarbamate, ethylammonium ethylcarbamate, 1-propylammonium 1-propylcarbamate, isopropylammonium isopropylcarbamate, butylammonium butylcarbamate, isobutylammonium isobutylcarbamate, pentylammonium carbamate, hexylammonium carbamate, heptylammonium carbamate, octylammonium carbamate, 2-ethylhexylammonium carbamate, nonylammonium carbamate, and decylammonium carbamate.

[0147] Specific examples of ammonium carbonate compounds as complexing agents include ammonium carbonate, methyl ammonium carbonate, ethyl ammonium carbonate, 1-propyl ammonium carbonate, isopropyl ammonium carbonate, butyl ammonium carbonate, isobutyl ammonium carbonate, pentyl ammonium carbonate, hexyl ammonium carbonate, heptyl ammonium carbonate, octyl ammonium carbonate, 2-ethylhexyl ammonium carbonate, nonyl ammonium carbonate and decyl ammonium carbonate.

[0148] Specific examples of ammonium bicarbonate compounds as complexing agents include ammonium bicarbonate, methylammonium bicarbonate, ethylammonium bicarbonate, 1-propylammonium bicarbonate, isopropylammonium bicarbonate, butylammonium bicarbonate, isobutylammonium bicarbonate, pentylammonium bicarbonate, hexylammonium bicarbonate, heptylammonium bicarbonate, octylammonium bicarbonate, 2-ethylhexylammonium bicarbonate, nonylammonium bicarbonate and decylammonium bicarbonate.

[0149] When the metal salt is reacted with an ammonium carbamate compound, an ammonium carbonate compound or an ammonium bicarbonate compound, the ratio of the amount of the ammonium carbamate compound, the ammonium carbonate compound or the ammonium bicarbonate compound to the amount of the metal salt is preferably 0.01 to 1 times, more preferably 0.05 to 0.6 times.

[0150] Specific examples of carboxylic acids as complexing agents include caproic acid, caprylic acid, pelargonic acid, 2-ethylhexanoic acid, capric acid, neodecanoic acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, palmitoleic acid, oleic acid, linoleic acid, and linolenic acid. Among them, the carboxylic acid is preferably a carboxylic acid having 8 to 20 carbon atoms, and more preferably a carboxylic acid having 10 to 16 carbon atoms.

[0151] In the metal complex ink, the content of the metal complex is preferably 10 to 90% by mass, more preferably 10 to 40% by mass, relative to the total mass of the metal complex ink. If the content of the metal complex is 10% by mass or more, the surface resistivity is further reduced. If the content of the metal complex is 90% by mass or less, the ejection stability of the metal complex ink is further improved.

[0152] -Solvents-

[0153] The metal complex ink preferably contains a solvent. The solvent is not particularly limited as long as it can dissolve the components contained in the metal complex ink, such as the metal complex.

[0154] The boiling point of the solvent is preferably 30 to 300°C, more preferably 50 to 200°C, and even more preferably 80 to 180°C from the viewpoint of ease of production.

[0155] The solvent is preferably contained in the metal complex ink so that the concentration of the metal ions relative to the metal complex (the amount of the metal present as free ions relative to 1 g of the metal complex) is 0.01 to 3.6 mmol / g, and more preferably 0.05 to 2 mmol / g. When the concentration of the metal ions is within the above range, the metal complex ink has excellent fluidity and exhibits excellent conductivity.

[0156] Examples of the solvent include hydrocarbons, cyclic hydrocarbons, aromatic hydrocarbons, carbamates, olefins, amides, ethers, esters, alcohols, thiols, thioethers, phosphines, and water. The metal complex ink may contain only one type of solvent or two or more types of solvents.

[0157] The hydrocarbon is preferably a linear or branched hydrocarbon having a carbon number of 6 to 20. Specific examples of the hydrocarbon include pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, octadecane, nonadecane and eicosane.

[0158] The cyclic hydrocarbon is preferably a cyclic hydrocarbon having a carbon number of 6 to 20. Specific examples of the cyclic hydrocarbon include cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, and decalin.

[0159] Specific examples of the aromatic hydrocarbons include benzene, toluene, xylene, trimethylbenzene, and tetralin.

[0160] The ether may be any of a linear ether, a branched ether, and a cyclic ether. Specific examples of the ether include diethyl ether, dipropyl ether, dibutyl ether, methyl tert-butyl ether, tetrahydrofuran, tetrahydropyran, dihydropyran, and 1,4-dioxane.

[0161] The alcohol may be any of a primary alcohol, a secondary alcohol and a tertiary alcohol.

[0162] Specific examples of the alcohol include ethanol, 1-propanol, 2-propanol, 1-methoxy-2-propanol, 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 1-hexanol, 2-hexanol, 3-hexanol, 1-octanol, 2-octanol, 3-octanol, tetrahydrofurfuryl alcohol, cyclopentanol, terpineol, decanol, isodecanol, lauryl alcohol, isolauryl alcohol, myristyl alcohol, isomyristyl alcohol, cetyl alcohol, isocetyl alcohol, stearyl alcohol, isostearyl alcohol, oleyl alcohol, isooleyl alcohol, linolyl alcohol, isolinoleyl alcohol, palmityl alcohol, isopalmityl alcohol, eicosanol, and isoeicosanol.

[0163] Specific examples of ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.

[0164] Specific examples of the esters include methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, methoxybutyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate and 3-methoxybutyl acetate.

[0165] -reducing agent-

[0166] The metal complex ink may contain a reducing agent. If the metal complex ink contains a reducing agent, the reduction of the metal complex to the metal is promoted.

[0167] Specific examples of the reducing agent include metal borohydride salts, aluminum hydride salts, amines, alcohols, organic acids, reducing sugars, sugar alcohols, sodium sulfite, hydrazine compounds, dextrin, hydroquinone, hydroxylamine, ethylene glycol, glutathione, and oxime compounds.

[0168] The reducing agent may also be an oxime compound described in JP-A-2014-516463. Specific examples of the oxime compound include acetone oxime, cyclohexanone oxime, 2-butanone oxime, 2,3-butanedione monoxime, dimethylglyoxime, methylacetoacetate monoxime, methylacetonate monoxime, benzaldehyde oxime, 1-indanone oxime, 2-adamantanone oxime, 2-methylbenzamide oxime, 3-methylbenzamide oxime, 4-methylbenzamide oxime, 3-aminobenzamide oxime, 4-aminobenzamide oxime, acetophenone oxime, benzamide oxime, and pinacolone oxime.

[0169] The reducing agent contained in the metal complex ink may be one kind or two or more kinds.

[0170] The content of the reducing agent in the metal complex ink is not particularly limited, but is preferably 0.1 to 20% by mass, more preferably 0.3 to 10% by mass, and even more preferably 1 to 5% by mass, based on the total mass of the metal complex ink.

[0171] -Resin-

[0172] The metal complex ink may contain a resin. If the metal complex ink contains a resin, the adhesion of the metal complex ink to the substrate is improved.

[0173] Examples of the resin include polyester, polyethylene, polypropylene, polyacetal, polyolefin, polycarbonate, polyamide, fluororesin, silicone resin, ethyl cellulose, hydroxyethyl cellulose, rosin, acrylic resin, polyvinyl chloride, polysulfone, polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl resin, polyacrylonitrile, polysulfide, polyamideimide, polyether, polyarylate, polyetheretherketone, polyurethane, epoxy resin, vinyl ester resin, phenolic resin, melamine resin and urea resin.

[0174] The resin contained in the metal complex ink may be one kind or two or more kinds.

[0175] -additive-

[0176] The metal complex ink may further contain inorganic salts, organic salts, inorganic oxides such as silicon dioxide, surface conditioners, wetting agents, crosslinking agents, antioxidants, rust inhibitors, heat stabilizers, surfactants, plasticizers, curing agents, thickeners, and silane coupling agents, etc., within the range that does not impair the coating properties or electromagnetic wave shielding properties. In the metal complex ink, the total content of the additives is preferably 20% by mass or less relative to the total mass of the metal complex ink.

[0177] -Physical properties of metal complex inks-

[0178] The viscosity of the metal complex ink is preferably 1 to 100 mPa·s, more preferably 2 to 50 mPa·s, and even more preferably 3 to 30 mPa·s.

[0179] The viscosity of the metal complex ink is a value measured using a viscometer at 25° C. The viscosity is measured using, for example, a VISCOMETER TV-22 type viscometer (manufactured by TOKI SANGYO CO., LTD.).

[0180] The surface tension of the metal complex ink is not particularly limited, but is preferably 20 to 45 mN / m, more preferably 25 to 35 mN / m.

[0181] The surface tension is a value measured using a surface tensiometer at 25° C. The surface tension is measured using, for example, DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).

[0182] (Metallic Salt Ink)

[0183] The metal salt ink is, for example, a conductive ink in which a metal salt is dissolved in a solvent.

[0184] -Metal Salts-

[0185] Examples of the metal constituting the metal salt include silver, copper, gold, aluminum, magnesium, tungsten, molybdenum, zinc, nickel, iron, platinum, tin, copper, and lead. Among them, from the viewpoint of conductivity, the metal constituting the metal salt preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium, and copper, more preferably includes at least one of silver and copper, and further preferably includes silver.

[0186] The content of the metal contained in the metal salt ink is preferably 1 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 20% by mass, based on the total mass of the metal salt ink, in terms of metal element.

[0187] In the metal salt ink, the content of the metal salt is preferably 10 to 90% by mass, more preferably 10 to 60% by mass, relative to the total mass of the metal salt ink. If the content of the metal salt is 10% by mass or more, the surface resistivity is further reduced. If the content of the metal salt is 90% by mass or less, the ejection stability is further improved when the metal salt ink is ejected from the nozzle.

[0188] Examples of the metal salt include benzoates, halides, carbonates, citrates, iodates, nitrites, nitrates, acetates, phosphates, sulfates, sulfides, trifluoroacetates, and carboxylates of metals. Two or more salts may be used in combination.

[0189] From the viewpoint of conductivity and storage stability, the metal salt is preferably a metal carboxylate.

[0190] The carboxylic acid forming the metal carboxylate is preferably at least one selected from the group consisting of formic acid and carboxylic acids having 1 to 30 carbon atoms, more preferably a carboxylic acid having 8 to 20 carbon atoms, and further preferably a fatty acid having 8 to 20 carbon atoms. The fatty acid may be linear or branched and may have a substituent.

[0191] Specific examples of the straight-chain fatty acids include acetic acid, propionic acid, butyric acid, valeric acid, pentanoic acid, hexanoic acid, heptanoic acid, behenic acid, oleic acid, octanoic acid, nonanoic acid, decanoic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, and undecanoic acid.

[0192] Specific examples of the branched fatty acid include isobutyric acid, isovaleric acid, ethylhexanoic acid, neodecanoic acid, pivalic acid, 2-methylvaleric acid, 3-methylvaleric acid, 4-methylvaleric acid, 2,2-dimethylbutyric acid, 2,3-dimethylbutyric acid, 3,3-dimethylbutyric acid, and 2-ethylbutyric acid.

[0193] Specific examples of the carboxylic acid having a substituent include hexafluoroacetylacetonic acid, hydroangelic acid, 3-hydroxybutyric acid, 2-methyl-3-hydroxybutyric acid, 3-methoxybutyric acid, acetone dicarboxylic acid, 3-hydroxyglutaric acid, 2-methyl-3-hydroxyglutaric acid, and 2,2,4,4-hydroxyglutaric acid.

[0194] The metal salt may be a commercially available product or may be a metal salt produced by a known method. The silver salt may be produced, for example, by the following method.

[0195] First, a silver compound (e.g., silver acetate) serving as a silver supply source and an equal amount of formic acid or a fatty acid having 1 to 30 carbon atoms to a molar equivalent of the silver compound are added to an organic solvent such as ethanol. The mixture is stirred for a predetermined time using an ultrasonic stirrer, and the resulting precipitate is washed with ethanol and decanted. All of these steps can be performed at room temperature (25° C.). The mixing ratio of the silver compound to formic acid or a fatty acid having 1 to 30 carbon atoms is preferably 1:2 to 2:1, more preferably 1:1, in terms of molar ratio.

[0196] -Other ingredients-

[0197] The metal salt ink may contain a solvent, a reducing agent, a resin, and an additive. Preferred embodiments of the solvent, the reducing agent, the resin, and the additive are the same as those that may be contained in the metal complex ink.

[0198] -Physical properties of metal salt inks-

[0199] The viscosity of the metal salt ink is preferably 1 to 100 mPa·s, more preferably 2 to 50 mPa·s, and even more preferably 3 to 30 mPa·s.

[0200] The viscosity of the metal salt ink is a value measured using a viscometer at 25° C. The viscosity is measured using, for example, a VISCOMETER TV-22 type viscometer (manufactured by TOKI SANGYO CO., LTD.).

[0201] The surface tension of the metal salt ink is not particularly limited, but is preferably 20 to 45 mN / m, more preferably 25 to 35 mN / m.

[0202] The surface tension is a value measured using a surface tensiometer at 25° C. The surface tension is measured using, for example, DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).

[0203] <Degassing process>

[0204] The degassing step is a step of degassing the conductive ink contained in the ink container, thereby obtaining a degassed conductive ink.

[0205] The conductive ink before the degassing step is contained in an ink container. The ink container is not particularly limited, and examples thereof include well-known ink containers such as an ink pack and an ink cartridge.

[0206] The degassed conductive ink may be contained in the ink container that contained the ink before degassed, or may be contained in an ink container different from the ink container that contained the conductive ink before degassed.

[0207] The conductive ink before the degassing step may be the prepared conductive ink as it is, or may be a conductive ink obtained by oxygenating the prepared conductive ink.

[0208] (Degassing method)

[0209] The degassing method in the degassing process is not particularly limited. For example, the following method can be cited: a degassing mechanism having a gas-permeable hollow fiber bundle is set between an ink container that contains the conductive ink and a nozzle that ejects ink of an inkjet head set in an inkjet recording device to allow the conductive ink to flow.

[0210] An example of a hollow fiber bundle is a bundle of a plurality of hollow fibers. By reducing the outer surface of the hollow fibers constituting the hollow fiber bundle to a reduced pressure of 0.1 to 0.8 atmospheres, dissolved oxygen in the conductive ink passing through the hollow fiber bundle can be removed.

[0211] As another example of the degassing method, the following method can be cited: conductive ink is supplied to a sub-tank (sub tunk) provided in the ink supply path from the ink container to the inkjet head, and the sub-tank is depressurized by a pump connected to the sub-tank to remove dissolved oxygen in the conductive ink supplied to the sub-tank.

[0212] The degree of decompression in the sub-tank can be appropriately selected, but is preferably set to 0.1 to 0.8 atmospheres. The degassed conductive ink is preferably stored in an appropriate amount in the sub-tank and transported to the nozzle that ejects the ink. As a specific example of an apparatus that can be used in the degassing process, the apparatus described in Japanese Patent Publication No. 2000-141687 can be cited.

[0213] From the viewpoint of improving degassing efficiency, the temperature of the conductive ink during the degassing step is preferably 20° C. or higher, more preferably 25° C. or higher, and even more preferably 30° C. or higher.

[0214] From the viewpoint of ink stability, the upper limit of the temperature of the conductive ink during the degassing step is preferably 80° C. or lower, and more preferably 60° C. or lower.

[0215] (Dissolved oxygen content)

[0216] From the viewpoint of suppressing the reduction of metal components in the conductive ink and thus improving the storage stability of the conductive ink, the dissolved oxygen amount A in the conductive ink before the degassing process contained in the ink container is preferably 15 mg / L or more, more preferably 20 mg / L or more, and further preferably 25 mg / L or more.

[0217] From the viewpoint that dissolved oxygen can be easily removed in the degassing step and discharge stability of the conductive ink is more excellent, the dissolved oxygen amount A is preferably 45 mg / L or less, more preferably 40 mg / L or less, and even more preferably 30 mg / L or less.

[0218] From the viewpoint of ink stability in the inkjet recording apparatus, the amount of dissolved oxygen B in the degassed conductive ink after the degassing step is preferably 0.05 mg / L or more, more preferably 0.1 mg / L or more, and even more preferably 0.5 mg / L or more.

[0219] From the viewpoint of more excellent discharge stability of the conductive ink, the dissolved oxygen amount B is preferably 12 mg / L or less, more preferably 10 mg / L or less, further preferably 8 mg / L or less, and particularly preferably 6 mg / L or less.

[0220] In the present invention, the value of subtracting the dissolved oxygen amount B from the dissolved oxygen amount A (dissolved oxygen amount A-dissolved oxygen amount B) is greater than 15 mg / L. From the viewpoint of a more excellent effect of the present invention, it is preferably 16 mg / L or more, more preferably 18 mg / L or more, and further preferably 20 mg / L or more.

[0221] From the viewpoint of degassing treatment rate, the value obtained by subtracting the dissolved oxygen amount B from the dissolved oxygen amount A is preferably 40 mg / L or less, more preferably 35 mg / L or less, and even more preferably 30 mg / L or less.

[0222] The amount of dissolved oxygen in the conductive ink of the present invention can be measured by gas chromatography. The specific method for measuring the amount of dissolved oxygen in the conductive ink is described in the Examples section below.

[0223] Although the details of the reason are not yet clear, the inventors have discovered that when the molar concentration Mb (unit: mmol / L) of dissolved oxygen in the degassed conductive ink after the degassing process and the molar concentration Mm (unit: mmol / L) of the metal in the conductive ink satisfy a prescribed relationship, the ink ejection stability and the ink stability within the nozzle are better.

[0224] Specifically, the ratio (Mm / Mb) of the molar concentration Mm (unit: mmol / L) to the molar concentration Mb (unit: mmol / L) is preferably 1600 or more, more preferably 1700 or more, and even more preferably 2500 or more. When Mm / Mb is 1600 or more, the ejection stability of the ink is more excellent.

[0225] Furthermore, Mm / Mb is preferably 110000 or less, more preferably 100000 or less, and further preferably 90000 or less. When Mm / Mb is 110000 or less, even if the degassed conductive ink is stored in the inkjet head, changes in physical properties such as coloration of the conductive ink can be suppressed (i.e., the ink has excellent stability in the inkjet head).

[0226] Here, the molar concentration Mb is obtained by converting the above-mentioned dissolved oxygen amount B (unit: mg / L) into a molar concentration (unit: mmol / L).

[0227] The molar concentration Mm is calculated from a value obtained by converting the metal contained in the conductive ink (specifically, the metal constituting the metal complex, the metal salt, and the metal particles) into metal elements.

[0228] The molar concentration Mm is preferably 100 to 2500 mmol / L, more preferably 300 to 2000 mmol / L, and further preferably 600 to 1600 mmol / L.

[0229] The molar concentration Mb is preferably 0.0001 to 3 mmol / L, more preferably 0.005 to 2 mmol / L, and even more preferably 0.01 to 1 mmol / L.

[0230] <Conductive layer forming step>

[0231] The conductive layer forming step is a step of forming a conductive layer by discharging degassed conductive ink from a nozzle using an inkjet recording method and applying the ink to a substrate.

[0232] (Inkjet recording method)

[0233] The inkjet recording method can be any one of a charge control method that utilizes electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that utilizes the vibration pressure of a piezoelectric element, an acoustic wave inkjet method that converts an electrical signal into a sound beam and irradiates the ink and ejects the ink using radiation pressure, and a thermal induction inkjet (Bubble Jet (registered trademark)) method that heats the ink to form bubbles and utilizes the generated pressure.

[0234] As an inkjet recording method, the method described in Japanese Patent Application Laid-Open No. 54-059936 can be particularly effectively used, in which the ink undergoes a sudden volume change due to thermal energy and the ink is ejected from the nozzle by the force generated by the state change.

[0235] In addition, regarding the inkjet recording method, the method described in paragraphs 0093 to 0105 of Japanese Patent Application Laid-Open No. 2003-306623 can also be referred to.

[0236] The inkjet head used for the inkjet recording method is not particularly limited, and examples thereof include: a shuttle scan method using a short-sized serial head to record while scanning the head along the width direction of the substrate, and a linear method using a linear head with recording elements arranged in an entire area corresponding to one side of the substrate.

[0237] The amount of droplets of the conductive ink ejected from the nozzles of the inkjet head is preferably 1 to 100 pL (picoliter), more preferably 2 to 80 pL, and even more preferably 2 to 20 pL.

[0238] (Base material)

[0239] The conductive ink ejected from the nozzle is applied to the substrate. The ejected conductive ink can be applied in a manner of contacting the substrate, and when other layers (for example, an insulating layer described later) are provided on the substrate, the conductive ink can be applied in a manner of contacting the other layers.

[0240] The material of the substrate is not particularly limited and can be selected according to the purpose. Specific examples of the material of the substrate include synthetic resins such as polyimide, polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephtalate, polyethylene naphthalate, polybutylene naphthalate, polycarbonate, polyurethane, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, acrylic resin, AS resin (acrylonitrile styrene resin), ABS resin (acrylonitrile-butadiene-styrene copolymer), triacetyl cellulose, polyamide, polyacetal, polyphenylene sulfide, polysulfone, epoxy resin, glass epoxy resin, melamine resin, phenolic resin, urea resin, alkyd resin, fluororesin, and polylactic acid; inorganic materials such as copper, steel, aluminum, silicon, soda glass, alkali-free glass, and indium tin oxide (ITO); and paper such as base paper, coated paper, coated paper, cast-coated paper, resin-coated paper, and synthetic paper. Furthermore, the substrate may be a single layer or may be two or more layers. When the substrate is two or more layers, two or more substrates made of different materials may be stacked.

[0241] The substrate is preferably in the form of a sheet or a film, and preferably has a thickness of 20 to 2000 μm.

[0242] The substrate may have an ink receptive layer, and the thickness of the ink receptive layer is preferably 1 to 20 μm. If the thickness of the ink receptive layer is 1 to 20 μm, the ink receptive layer can be more stably maintained. The ink receptive layer refers to a coating formed on the substrate to absorb ink and fix the ink.

[0243] Before applying the conductive ink to the substrate, the substrate may be pretreated. Examples of the pretreatment include ozone treatment, plasma treatment, corona treatment, primer treatment, and roughening treatment.

[0244] The substrate may be an electronic substrate. When an insulating layer and a conductive layer are arranged on the electronic substrate, the conductive layer functions as a so-called electromagnetic wave shield. Therefore, when an insulating layer and a conductive layer are arranged on the electronic substrate, the insulating layer and the conductive layer are preferably arranged in a manner that covers the electronic components that may be included in the electronic substrate.

[0245] Here, the insulating layer is formed using a known insulating ink, and the conductive layer is a conductive layer obtained by the method for producing a conductive layer of the present invention.

[0246] Examples of the electronic substrate include a flexible printed circuit board, a rigid printed circuit board, and a rigid-flexible circuit board.

[0247] The electronic substrate preferably includes a wiring substrate and electronic components arranged on the wiring substrate.

[0248] The wiring board refers to a wiring board in which wiring is implemented at least on a substrate or inside a substrate.

[0249] Examples of the substrate constituting the wiring board include a glass epoxy substrate, a ceramic substrate, a polyimide substrate, and a polyethylene terephthalate substrate. The substrate may have a single-layer structure or a multi-layer structure.

[0250] The wiring provided on the wiring substrate is preferably a copper wiring. For example, one end of the wiring is connected to an external power supply and the other end is connected to a terminal of an electronic component.

[0251] Examples of electronic components include semiconductor chips, capacitors, and transistors.

[0252] (Curing treatment)

[0253] The method for producing a conductive layer of the present invention may further include a curing treatment of curing the degassed conductive ink applied to the substrate by at least one of heating and light irradiation. Thus, the degassed conductive ink applied to the substrate is cured to form a conductive layer.

[0254] Only one of heating and light irradiation may be performed, or both of them may be performed.

[0255] The temperature during heating (firing temperature) is preferably 80° C. or higher, more preferably 100° C. or higher. From the viewpoint of reducing damage to the substrate, etc., the firing temperature is preferably 250° C. or lower, more preferably 200° C. or lower.

[0256] The heating time (firing time) is preferably 1 minute or longer. From the viewpoint of reducing damage to the substrate and the like, the firing temperature is preferably 120 minutes or shorter, more preferably 60 minutes or shorter.

[0257] Before applying the conductive ink to the substrate, the substrate may be preheated. In the present invention, such heating is also regarded as one form of the above-mentioned heating. The temperature of the substrate when applying the conductive ink is preferably 20 to 180°C, more preferably 40 to 150°C.

[0258] Specific examples of light used in light irradiation include ultraviolet rays and infrared rays.

[0259] The peak wavelength of ultraviolet rays is preferably 200 to 405 nm, more preferably 250 to 400 nm, and further preferably 260 to 400 nm.

[0260] The exposure amount during light irradiation is preferably 0.1 to 10000 J / cm 2 , more preferably 1 to 500 J / cm 2 .

[0261] In the present invention, the time from when the degassed conductive ink lands on the substrate to when heating or light irradiation starts is preferably within 1 second, more preferably within 0.8 seconds, and further preferably within 0.6 seconds. This promotes the reduction of the metal salt, metal complex, or metal particles contained in the conductive ink landed on the substrate to the metal (i.e., the reduction can be suppressed from being blocked by oxygen in the air), so that a conductive layer with better conductivity can be formed.

[0262] The conductive layer forming step may be repeated, thereby adjusting the thickness of the conductive layer.

[0263] The thickness of the conductive layer is preferably 0.1 to 100 μm, more preferably 1 to 50 μm. The thickness of the conductive layer is the arithmetic mean of the lengths of 10 points corresponding to the thickness of the conductive layer obtained by taking a cross-sectional image of the conductive layer using a scanning electron microscope and measuring the lengths of the 10 points.

[0264] From the viewpoint of more excellent conductivity of the conductive layer, the volume resistivity of the conductive layer is preferably 6 μΩ·cm or less, more preferably 5 μΩ·cm or less, and further preferably 4 μΩ·cm or less.

[0265] The lower limit of the volume resistivity of the conductive layer is not particularly limited, and is, for example, 2 μΩ·cm.

[0266] The volume resistivity of the conductive layer can be measured by the method described in the Examples section described later.

[0267] From the viewpoint of more excellent conductivity of the conductive layer, the porosity of the conductive layer is preferably 24% or less, more preferably 23% or less, and further preferably 22% or less.

[0268] The lower limit of the porosity is not particularly limited, and is, for example, 0%.

[0269] The porosity of the conductive layer can be measured by the method described in the Examples section described later.

[0270] Example

[0271] Below, the present invention is further described in detail according to the examples. The materials, usage amounts, ratios, processing contents and processing procedures shown in the following examples can be appropriately changed without departing from the gist of the present invention. Therefore, the scope of the present invention should not be interpreted restrictively by the examples shown below.

[0272] [Preparation of Conductive Ink 1]

[0273] 570 g of silver neodecanoate was added to a 2000 mL three-necked flask. Then, 400.0 g of trimethylbenzene and 30.0 g of terpineol were added and stirred to obtain a solution containing a silver salt. The solution was filtered using a PTFE (polytetrafluoroethylene) membrane filter with a pore size of 0.45 μm to obtain a conductive ink 1. The content of metal contained in the conductive ink 1 ("metal amount" in Table 1) was 22% by mass in terms of metal element conversion relative to the total mass of the conductive ink 1.

[0274] After the conductive ink 1 was sealed in an ink pack made of an oxygen-impermeable material used in an inkjet recording apparatus described later, 10 μL of the conductive ink 1 was drawn with a syringe, and the dissolved oxygen content A (mg / L) of the conductive ink 1 at 25° C. was measured by gas chromatography (measurement device: GC390, manufactured by GL Sciences Inc.). The measurement results are shown in Table 1.

[0275] The ink pack is a multilayer film formed by laminating polyamide, aluminum alloy, polyethylene terephthalate and polyolefin in this order and heat-sealed into a bag shape in such a way that the polyolefin becomes the liquid contact part. The oxygen permeability of the ink pack is 0.5 cc / m 2 ·atm·24hrs or less, oxygen is substantially not transmitted.

[0276] [Preparation of Conductive Inks 2 to 6]

[0277] Conductive inks 2 to 6 were obtained by diluting conductive ink 1 with a mixed solvent of trimethylbenzene and terpineol (trimethylbenzene:terpineol=40:3 (mass ratio)) so that the metal content in the conductive ink became the value described in Table 1.

[0278] Conductive inks 2 to 6 were oxygenated or degassed so that the values ​​of dissolved oxygen content A (mg / L) were the values ​​shown in Table 1. Thereafter, each conductive ink was sealed in the above-mentioned ink pack, and the dissolved oxygen content A (mg / L) was measured by the same method as that of conductive ink 1. The measurement results are shown in Table 1.

[0279] [Example 1]

[0280] An inkjet recording apparatus X having a piezoelectric inkjet head (product name "Samba", manufactured by FUJIFILM DIMATIX Inc.) was prepared.

[0281] The ink supply system in the inkjet recording apparatus X is composed of an ink pack, a supply pipe, a degassing filter SEPAREL EF-G2 (manufactured by DIC Corporation), an ink supply tank just before the inkjet head, a degassing filter (SEPAREL EF-G2, manufactured by DIC Corporation), and the above-mentioned inkjet head. The ink pack containing the conductive ink 1 was used.

[0282] When the conductive ink 1 was supplied from the ink pack to the inkjet head, the degassing filter provided between the ink pack and the inkjet head was depressurized (degassing process) so that the dissolved oxygen content B (mg / L) of the conductive ink 1 became the value of Table 1. The temperature of the conductive ink 1 during the degassing process was 30°C.

[0283] Here, the dissolved oxygen amount B (mg / L) in Example 1 is the dissolved oxygen amount of the conductive ink 1 at 25° C. measured by gas chromatography (measurement device: GC390, manufactured by GL Sciences Inc.) by extracting 10 μL of the conductive ink 1 from the flow path on the inkjet head side downstream of the degassing filter with a syringe. The measurement results are shown in Table 1.

[0284] <Evaluation of discharge stability>

[0285] After the degassing step, the conductive ink having a dissolved oxygen content B was continuously ejected from the nozzle of the inkjet head toward a substrate (polyimide film, product name "Kapton", manufactured by DU PONT-TORAY CO., LTD.), and the ink ejection stability was evaluated.

[0286] Specifically, the amount of droplets ejected from the nozzles of the inkjet head was adjusted to 2.5 pL, and the conductive ink having a dissolved oxygen amount B was ejected continuously for 15 minutes under the conditions of 128 nozzles and 20 kHz.

[0287] After the ejection, nozzle detachment and defective nozzles were confirmed, and the ejection stability of the ink was evaluated according to the following evaluation criteria. If the evaluation criteria were 3 or more, it was a level with no practical problems. The evaluation results are shown in Table 1.

[0288] (Evaluation Criteria)

[0289] 5: No nozzle detachment and no defective nozzles

[0290] 4: Nozzle detachment, less than 3 defective nozzles

[0291] 3: Nozzle detachment, more than 3 and less than 5 defective nozzles

[0292] 2: Nozzle detachment, defective nozzles are more than 5 and less than 10

[0293] 1: Nozzle detachment, more than 10 defective nozzles

[0294] <Volume resistivity (electrical conductivity evaluation)>

[0295] After the above degassing step, a conductive ink having a dissolved oxygen content B was ejected from the nozzle of the inkjet head to print an image (size: 3 mm×20 mm) composed of the conductive ink on the surface of a substrate (polyimide film, product name "Kapton", manufactured by DU PONT-TORAY CO., LTD.). The obtained image was heated on a hot plate at 180° C. for 30 minutes to obtain a substrate with a conductive layer (thickness 1 μm) formed on the surface of the substrate (conductive layer forming step). In addition, the time from the point when the conductive ink landed on the substrate to the start of heating was within 1 second.

[0296] The resistance of the conductive layer was measured at room temperature (23°C) using a resistance meter (trade name "DT4222", manufactured by HIOKI EE Corporation), and the cross-sectional area of ​​the conductive layer was measured at room temperature (23°C) using a scanning electron microscope (product name S-4700, manufactured by HITACHI, LTD.), and the volume resistivity (μΩ·cm) was calculated based on the obtained value. The evaluation criteria are as follows: the lower the volume resistivity, the better the conductivity. If the evaluation criteria is 2, it is a level with no practical problems. The evaluation results are shown in Table 1.

[0297] (Evaluation Criteria)

[0298] 2: Volume resistivity is less than 4μΩ·cm

[0299] 1: Volume resistivity exceeds 4μΩ·cm

[0300] <Evaluation of storage stability>

[0301] The conductive ink before the degassing process (i.e., the conductive ink having the dissolved oxygen amount A as shown in Table 1) was sealed in the above-mentioned ink pack formed of the oxygen-impermeable material. The ink pack was stored in a thermostatic bath maintained at 45°C, 100 μL of the conductive ink was extracted from the spout of the ink pack with a syringe, diluted 10 times with trimethylbenzene, and the absorbance at a wavelength of 240 to 800 nm was measured and evaluated using an ultraviolet-visible-infrared spectrophotometer V-550 (manufactured by JASCO Corporation). The evaluation criteria are as follows. If the evaluation criteria are 2 or more, it is a level that has no practical problems. The evaluation results are shown in Table 1.

[0302] (Evaluation Criteria)

[0303] 4: The change in the maximum absorbance at a wavelength of 400-600 nm on the 45th day is less than 0.2

[0304] 3: No color change until the 30th day, but the change range Δ of the maximum absorbance at a wavelength of 400 to 600 nm on the 45th day is 0.2 or more

[0305] 2: There is no color change until the 29th day, but the change range Δ of the maximum absorbance at a wavelength of 400 to 600 nm on the 30th day is 0.2 or more

[0306] 1: The change range Δ of the maximum absorbance at wavelengths of 400 to 600 nm is greater than 0.2 before the 29th day

[0307] <Ink stability in the inkjet head (in-head stability)>

[0308] While the conductive ink supplied to the inkjet head of the inkjet recording device X (i.e., the conductive ink having the dissolved oxygen content B as the value described in Table 1) was maintained at 35°C, 100 μL of the conductive ink was extracted from the inkjet head side flow path downstream of the degassing filter once a day with a syringe, diluted 10 times with trimethylbenzene, and the absorbance at 240 to 800 nm was measured and evaluated with an ultraviolet visible infrared spectrophotometer V-550 (manufactured by JASCO Corporation). The evaluation criteria are as follows, and if the evaluation criteria is 2 or more, it is a level with no practical problems. The evaluation results are shown in Table 1.

[0309] (Evaluation Criteria)

[0310] 3: The change in the maximum absorbance at a wavelength of 400-600 nm on the 10th day is less than 0.2)

[0311] 2: There is no color change until the 9th day, but the change range Δ of the maximum absorbance at a wavelength of 400 to 600 nm on the 10th day is 0.2 or more

[0312] 1: The change range Δ of the maximum absorbance at wavelengths of 400-600 nm is greater than 0.2 before the 9th day

[0313] <Porosity>

[0314] The substrate with a conductive layer produced in the measurement of volume resistivity was cut in the thickness direction of the substrate with a conductive layer using a microtome (product name RM2255, manufactured by Leica) to obtain a cross section. A cross-sectional observation photograph of the obtained cross section was obtained using a scanning electron microscope (product name S-4700, manufactured by HITACHI LTD.).

[0315] The threshold of the obtained cross-sectional observation photograph was adjusted using image software (manufactured by Adobe Systems, Inc., "Adobe Photoshop"), and the white area where the conductive material (metal) existed and the black area where the pores existed were binarized in the conductive layer. The ratio of the area of ​​the black area to the total area of ​​the white area and the black area was calculated and used as the porosity (%). The values ​​of the porosity (%) are shown in Table 1. The smaller the porosity, the better the conductivity of the conductive layer.

[0316] [Examples 2 to 7]

[0317] The degassing process of the conductive ink was carried out in the same manner as in Example 1, except that an ink pack containing the conductive ink described in Table 1 was used and the decompression conditions were adjusted so that the dissolved oxygen amount B (mg / L) of the conductive ink after the degassing process became the value of Table 1. The dissolved oxygen amount B (mg / L) of each conductive ink after the degassing process is shown in Table 1.

[0318] Then, the above-mentioned various evaluations were performed in the same procedure as in Example 1. Table 1 shows the evaluation results.

[0319] [Comparative Example 1]

[0320] The above-mentioned various evaluations were performed in the same manner as in Example 1, except that the degassing step was not performed. Table 1 shows the evaluation results.

[0321] In Comparative Example 1, the degassing step was not performed, but the value of the dissolved oxygen amount in the conductive ink supplied to the inkjet head is shown in the column of dissolved oxygen amount B in Table 1 for convenience.

[0322] [Table 1]

[0323]

[0324] In Table 1, "AB" represents a value obtained by subtracting the dissolved oxygen amount B from the dissolved oxygen amount A.

[0325] In Table 1, the “metal amount” refers to a value (mass %) in which the metal contained in the conductive ink is converted into a metal element relative to the total mass of the conductive ink.

[0326] Mm / Mb represents the ratio of the molar concentration Mm (unit: mmol / L) of the metal in the conductive ink before the degassing process to the molar concentration Mb (unit: mmol / L) of the dissolved oxygen in the degassed conductive ink after the degassing process, and the calculation method of Mm and Mb is as described above. However, in Comparative Example 1, since the degassing process was not performed, the value equivalent to the molar concentration Mb was calculated using the conductive ink supplied to the inkjet head.

[0327] As shown in Table 1, it is shown that when the value (AB) of the dissolved oxygen amount B in the degassed conductive ink after the degassing process minus the dissolved oxygen amount A in the conductive ink before the degassing process is greater than 15 mg / L, a conductive layer having excellent ink storage stability and ejection stability and excellent conductivity can be formed (Example).

[0328] Furthermore, the comparison of Examples 1 to 7 shows that when the value of Mm / Mb is within the range of 1700 to 100000 (Examples 2 to 5 and 7), both the stability within the nozzle and the discharge stability are more excellent.

Claims

1. A method for manufacturing a conductive layer, comprising the following steps: A degassing step of degassing the conductive ink contained in the ink container; and The conductive layer forming step uses an inkjet recording method to eject degassed conductive ink from a nozzle and apply it to the substrate to form a conductive layer. The conductive ink comprises at least one material selected from the group consisting of metal salts, metal complexes and metal particles. When the amount of dissolved oxygen in the conductive ink before the degassing step is defined as dissolved oxygen amount A and the amount of dissolved oxygen in the degassed conductive ink after the degassing step is defined as dissolved oxygen amount B, a value obtained by subtracting the amount of dissolved oxygen B from the amount of dissolved oxygen A is greater than 15 mg / L.

2. The method for manufacturing a conductive layer according to claim 1, wherein: The dissolved oxygen amount B is less than 10 mg / L.

3. The method for manufacturing a conductive layer according to claim 1 or 2, wherein: The metal constituting the metal salt, the metal complex, and the metal particles includes at least one of silver and copper.

4. The method for manufacturing a conductive layer according to claim 1 or 2, wherein: The conductive ink includes at least one of the metal salt and the metal complex.

5. The method for manufacturing a conductive layer according to claim 1 or 2, wherein: When the molar concentration of the metal in the conductive ink is defined as Mm and the molar concentration of dissolved oxygen in the degassed conductive ink after the degassing step is defined as Mb, the value of Mm / Mb is 1700 to 100000, Wherein, the units of the Mm and the Mb are both mmol / L.

6. The method for manufacturing a conductive layer according to claim 1 or 2, wherein: The conductive layer forming step includes a curing process in which the degassed conductive ink applied to the substrate is cured by at least one of heating and light irradiation. The time from when the degassed ink lands on the substrate to when the heating or light irradiation starts is within 1 second.

7. The method for manufacturing a conductive layer according to claim 1 or 2, wherein: The temperature of the conductive ink during the degassing step is 30° C. or higher.

Citation Information

Patent Citations

  • Ink jet recorder and ink tank therefor

    JP2000141687A

  • Aqueous ink

    JP2003306623A

  • Silver ink composition

    JP2014516463A

  • Bonding composition

    WO2014057633A1

  • Ink-jet printing based conductive circuit printing process

    CN107148154A