Potassium fluotantalate powder, method for producing tantalum powder through sodium reduction of potassium fluotantalate powder, tantalum powder obtained through method and application of tantalum powder

By using alkaline earth metal halide salt to flow and heating the potassium fluorotantalate powder and inert gas in sodium reducing potassium fluorotantalate method, the problems of low specific capacity, large leakage current and low breakdown voltage are solved, and the tantalum powder is realized Higher electrical properties and higher yields reduce oxygen content and reaction vessel corrosion.

CN118900825APending Publication Date: 2024-11-05NINGXIA ORIENT TANTALUM INDUSTRY CO LTD

Patent Information

Application Number
CN202480001175.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing sodium reducing potassium fluorotantalate method for preparing tantalum powder has problems such as low specific capacitance, large leakage current and low breakdown voltage. The process is mature but it is difficult to further improve performance, especially the reduction of tantalate and its countercapacitance are not involved. Effects of performance.

Method used

In the sodium reduction potassium fluorotantalate method, the potassium fluorotantalate powder of alkaline earth metal halide salt is added as raw material, and the diluted salt is heated and melted by inert gas flow, and potassium fluorotantalate and sodium metal are added multiple times for reduction. ,控制温度和搅拌条件,进一步进行老化和处理以提高钽粉的性能。

Benefits of technology

It significantly improves the specific capacitance, breakdown voltage and leakage current performance of tantalum powder, and at the same time improves the yield of tantalum powder, reduces the oxygen content, enhances the electrical performance, and extends the life of the reaction vessel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900825A_ABST
    Figure CN118900825A_ABST
Patent Text Reader

Abstract

The invention relates to potassium fluotantalate powder, a method for producing tantalum powder through sodium reduction of the powder, the tantalum powder obtained through the method and application of the tantalum powder. The potassium fluotantalate powder is used as a raw material in the production of tantalum powder by a sodium-reduced potassium fluotantalate process, the powder comprising 5-1000 ppm (preferably 50-800 ppm, more preferably 100-850 ppm, more preferably 100-500 ppm, more preferably 50-150 ppm and / or 300-500 ppm) of an alkaline earth metal haloid selected from the group consisting of haloid of magnesium and / or haloid of calcium, such as magnesium chloride, and the balance of potassium fluotantalate. The invention also relates to a method for producing tantalum powder through sodium reduction of the powder, the tantalum powder obtained through the method and application of the tantalum powder in a capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of smelting rare metal functional materials, and in particular relates to tantalum powder for making high-voltage and high-reliability capacitors and a manufacturing method thereof. Background Art

[0002] Tantalum electrolytic capacitors (hereinafter referred to as tantalum capacitors) have the advantages of high capacity, small size, strong self-healing ability, and high reliability. They are widely used in high-end technical fields such as communications, computers, automotive electronics, medical equipment, radar, aerospace, and automatic control devices. Tantalum powder is the key material for making tantalum capacitors. Only by using tantalum powder for capacitors with high specific capacitance and low leakage current can tantalum capacitors with smaller size and better reliability be produced. Therefore, only by continuously developing tantalum powder for capacitors with higher specific capacitance, higher breakdown voltage and / or lower leakage current can the tantalum capacitors produced continue to meet the requirements of electronic devices and electronic circuits for the miniaturization and high reliability of tantalum capacitors.

[0003] At present, the main methods for industrial preparation of capacitor-grade tantalum powder are sodium reduction potassium fluorotantalate method, magnesium reduction tantalum oxide method, etc. The magnesium reduction tantalum oxide method is expected to produce tantalum powder for capacitors with improved specific capacity and pressure resistance due to the change of the state of the reactants. However, due to the immature process, magnesium reduction of tantalum powder has the problems of low production efficiency and high cost, which limits its promotion and application. Although the sodium reduction potassium fluorotantalate method for preparing tantalum powder has the problems of low specific capacity, large leakage current and low breakdown voltage under relatively high voltage enabling conditions, the sodium reduction potassium fluorotantalate method has achieved large-scale production due to its mature process and relatively low production cost. In addition, the sodium reduction potassium fluorotantalate method can easily prepare high specific capacity tantalum powder. At present, sodium reduction tantalum powder accounts for more than 80% of the tantalum powder market for capacitors. It is of great significance to scientifically improve the sodium reduction potassium fluorotantalate process and improve the performance of sodium reduction tantalum powder.

[0004] In order to improve the quality of sodium reduced tantalum powder, many studies have been conducted in the industry.

[0005] US4684399A discloses a method for producing tantalum powder by reducing potassium fluorotantalate with sodium. Potassium fluorotantalate and metallic sodium are continuously or semi-continuously added to a molten diluent for multiple times for stirring and reduction to obtain tantalum powder. US4149876A proposes a method for producing tantalum powder by adding liquid sodium to a molten salt bath of molten potassium fluorotantalate and diluent. The method is to rapidly inject sodium at a relatively low temperature to raise the material temperature, use a large diluent ratio, force cooling, carry out a reduction reaction at a relatively low temperature, and maintain a constant temperature during the grain growth period, thereby producing tantalum powder with fine and uniform particle size.

[0006] CN1069564C discloses a reduction process in which phosphorus, boron, nitrogen, oxygen, and silicon are added as additives to refine tantalum powder during the reduction process. The use of refiners can significantly increase the specific volume of tantalum powder reduced by sodium. There are also patents that propose the use of iodides or sulfates in the reduction process to improve the performance of tantalum powder.

[0007] JP4828016B2 discloses a method for producing tantalum powder by reducing potassium fluorotantalate with metallic sodium. The method comprises adding a small amount of potassium fluorotantalate to a molten diluent, then adding metallic sodium for reduction, and then adding a small amount of potassium fluorotantalate for sodium reduction. The process is repeated to achieve the reaction of potassium fluorotantalate at a low concentration. The amount of diluent salt is 40-1000 times that of potassium fluorotantalate, thereby achieving the purpose of increasing the specific capacitance of the tantalum powder. The specific capacitance of the tantalum powder produced by the method is 80000-250000 μFV / g.

[0008] CN201693181U discloses a method for achieving the reaction of dispersed metallic sodium and molten potassium tantalate by means of a sodium distributor provided at the end of a sodium injection tube; Chinese patent CN116100040A discloses a method for reducing potassium tantalate by jetting metallic sodium to disperse the metallic sodium, and the method produces a tantalum powder product with uniform particle size distribution and uniform particle shape distribution.

[0009] In order to improve the pressure resistance of tantalum powder produced by the sodium reduction potassium fluorotantalate method, other methods include increasing the sintering temperature and extending the sintering time of subsequent treatments. However, increasing the sintering temperature and extending the sintering time will inevitably reduce the specific capacitance.

[0010] Without being bound by general theories, the inventors have found after extensive research that there are studies on the process of reducing potassium tantalate with sodium, which involve the state, temperature, and concentration of potassium tantalate (using diluent salts such as potassium chloride, sodium chloride, and potassium fluoride to disperse potassium tantalate); involving alkali metal halides as diluent salts; involving the use of additives such as compounds containing phosphorus, boron, nitrogen, oxygen, silicon, iodine, and sulfur to refine tantalum powder during the reduction process; involving the temperature of injected metallic sodium and its fluidity, involving the stirring and mixing during the reduction process, and involving equipment for optimizing the reduction process. However, there are studies on the process of reducing potassium tantalate with sodium, which do not involve the reduction of tantalate in the sodium reduction potassium tantalate system, and even almost no attention has been paid to the generation and influence of tantalate in the prior art. In fact, oxygen is inevitably present in the sodium reduction molten salt system. Since tantalum has a strong affinity for oxygen, tantalate is easily formed in the sodium reduction system, and the tantalum in tantalate is difficult to be reduced by metallic sodium. If tantalate is allowed to enter the tantalum powder, the oxygen content of the tantalum powder will increase and the leakage current will increase. On the other hand, most of the tantalate formed in the sodium reduction system exists in the form of extremely fine particles, which are removed as harmful components during the water pickling process, resulting in a lower yield in the tantalum powder production process. Summary of the invention

[0011] According to one aspect of the present invention, a potassium fluorotantalate powder used as a raw material in the production of tantalum powder by a sodium reduction potassium fluorotantalate method is provided, wherein the potassium fluorotantalate powder contains 5-1000 ppm of an alkaline earth metal halogen salt and the remainder of potassium fluorotantalate. The potassium fluorotantalate powder is used as a raw material for the sodium reduction method to produce tantalum powder.

[0012] Halogenates are also called halides. In this application, "alkaline earth metal halides" and "alkaline earth metal halogen salts" can be used interchangeably, both referring to compounds containing alkaline earth metals (such as magnesium and / or calcium) and halogens, such as magnesium chloride. The "potassium fluorotantalate powder" mentioned below contains 5-1000ppm, preferably more than 50ppm, more preferably 100-850ppm, more preferably 100-500ppm, most preferably 50-150ppm and / or 300-500ppm of alkaline earth metal halogen salts, and the remainder of potassium fluorotantalate, unless otherwise specified. Since this amount is relatively small and does not significantly affect the macroscopic material of potassium fluorotantalate powder, the potassium fluorotantalate powder containing the said amount of alkaline earth metal halogen salts is still referred to as "potassium fluorotantalate powder" below and in the claims, unless otherwise specified. Therefore, "potassium fluorotantalate powder" is not used interchangeably herein with "potassium fluorotantalate," the latter of which refers to potassium fluorotantalate (K2TaF7) that does not contain alkaline earth metal halides, unless otherwise indicated.

[0013] According to another aspect of the present invention, a method for preparing tantalum powder by reducing potassium fluorotantalate with sodium is provided, the method comprising using the potassium fluorotantalate powder as a raw material.

[0014] It is generally believed in the prior art that the introduction of alkaline earth metal halogen salts should be avoided in the process of sodium reduction of potassium fluorotantalate, because alkaline earth metal halogen salts may be reduced to alkaline earth metals by sodium, and alkaline earth metals corrode the currently commonly used metal reduction containers seriously. However, the inventor unexpectedly found that in the method of the present invention, since the potassium fluorotantalate powder as a raw material contains a small amount of alkaline earth metal halogen salts, the alkaline earth metal halogen salts are reduced to alkaline earth metals by metallic sodium, and the alkaline earth metals further reduce harmful tantalates. Since the reduction of alkaline earth metal halogen salts by metallic sodium in the sodium reduction potassium fluorotantalate system is a weak equilibrium, but alkali metals such as metallic magnesium have a strong affinity for oxygen, the generated metallic magnesium is promptly converted into magnesium oxide, and loses the ability to corrode the sodium reduction potassium fluorotantalate container, so the corrosion of the reaction container for reducing potassium fluorotantalate is greatly reduced. Therefore, the addition of alkaline earth metal halogen salts in the process of sodium reduction of potassium fluorotantalate will not corrode the reaction container, nor will it affect its life.

[0015] According to another aspect of the present invention, there is provided a method for preparing tantalum powder for capacitors by sodium reduction of potassium fluorotantalate, comprising the following steps:

[0016] (1) providing potassium fluorotantalate powder, a diluent salt (preferably selected from alkali metal halides), and liquid metallic sodium as raw materials, wherein the potassium fluorotantalate powder contains 5-1000 ppm of alkaline earth metal halide,

[0017] (2) placing the diluted salt into a reduction container, evacuating the container, and then introducing an inert gas such as argon, and then heating the diluted salt in the reduction container until it melts while the inert gas is kept flowing (at a flow rate of 20-100 liters / minute),

[0018] (3) adding a portion of potassium fluorotantalate powder to a reduction container, monitoring the temperature to ensure that the mixture of potassium fluorotantalate powder and diluent salt is melted, and then adding liquid metallic sodium to reduce the portion of potassium fluorotantalate, repeating the process multiple times until all the potassium fluorotantalate powder and metallic sodium raw materials are used up.

[0019] (4) After the reduction is completed, the tantalum powder is aged.

[0020] (5) Then, the tantalum powder is separated.

[0021] Optionally, after step (5), the method further comprises the following steps:

[0022] (6) The tantalum powder is subjected to salt bath heat treatment and / or agglomeration heat treatment, the metal magnesium chips are subjected to oxygen reduction treatment, and further pickling, purification and drying are performed to obtain a tantalum powder product.

[0023] In step (1), the diluent salt is selected from the alkali metal halogen salts commonly mentioned in the prior art. There is no restriction on the ratio of potassium fluorotantalate and the diluent salt, and the ratio commonly used in the prior art can be adopted. Preferably, the diluent salt may also be mixed with a tantalum powder refiner, and the tantalum powder refiner is selected from one or more compounds containing sulfur, phosphorus, boron, nitrogen, oxygen, silicon, iodine, etc. As an alternative, high-purity nitrogen gas can be introduced, which can also act as a refiner. The amount of metallic sodium is in excess of the theoretical amount for completely reducing potassium fluorotantalate, for example, an excess of 1-3%, preferably an excess of 1.5-2.5%. Preferably, the metallic sodium is preheated to more than 150°C, for example, 180°C-500°C, more preferably 200-350°C, more preferably 200-260°C, more preferably 190°C-240°C, for example 210°C.

[0024] The melting point of sodium is 97.78 degrees. Even if solid sodium is added, it will melt into liquid quickly in the furnace. Therefore, the prior art pays little attention to the temperature of the metal sodium itself, but only focuses on the sodium injection temperature (that is, the temperature of the reduction container or furnace when sodium is added). Although some people may have studied the effect of increasing the sodium injection temperature, this means that the temperature in the furnace needs to be increased as a whole, which brings a greater heat load to the materials made of the reduction container and the furnace, which is not conducive to its service life. Moreover, increasing the temperature in the furnace also means greater energy consumption. The prior art may also have studied improving the fluidity of the liquid metal sodium by increasing the temperature of the liquid metal sodium itself, but since the fluidity of the liquid sodium almost tends to be stable as the temperature increases to above 120°C, the metal sodium with a temperature of about 120°C or less is generally added. The inventor unexpectedly found through a large amount of research that by further increasing the temperature of the liquid metal sodium, not only the good fluidity of the liquid sodium is maintained, but also the temperature of the reduction reaction point is accurately increased without increasing the power of the heating furnace, the morphology of the tantalum powder is improved, and finally the electrical properties of the tantalum powder, such as breakdown voltage and leakage current, are improved.

[0025] Preferably, in step (1), the diluent salt and potassium tantalate are both in the form of powder. As mentioned above, the content of alkaline earth metal halogen salt (preferably calcium chloride and magnesium chloride, especially preferably magnesium chloride) in the potassium tantalate powder is, for example, 5-1000 ppm by weight, preferably more than 50 ppm, more preferably 100-850 ppm, more preferably 100-500 ppm, most preferably 50-150 ppm or 300-500 ppm. If the content of alkaline earth metal halogen salt in the potassium tantalate powder is too much, the alkaline earth metal obtained by reduction cannot be completely converted into oxides, and this part of the excess alkaline earth metal will corrode the reduction container and shorten the life of the reduction container. Therefore, from the perspective of extending the life of the reduction container, the upper limit of the alkaline earth metal halogen salt is preferably 1000 ppm.

[0026] Preferably, in step (2), the evacuation and introduction of an inert gas such as argon are repeated multiple times, for example, 2-3 times, to exhaust the air in the reduction container as much as possible, reduce the corrosion of the metal reduction container by air, and reduce the adverse effects of air on tantalum powder. In order to allow the water vapor and acidic gas released during the heating and melting process to be carried by the argon gas and discharged from the reduction container in time to reduce the adverse effects on the reduction, preferably, the inert gas flow rate is maintained at 20-100 liters / minute, which can better discharge water vapor and acidic gas. In order to ensure that it is completely melted and improve the viscosity of the diluted salt so that stirring is smoother, the diluted salt is preferably heated to a temperature exceeding its melting point by 80°C, preferably exceeding 150°C, and more preferably exceeding 200°C. Preferably, after being fully melted, it is also kept warm, for example, for 30 minutes. Preferably, the diluted salt is stirred after being heated to the target temperature so as to be fully mixed and keep the temperature uniform. There are no special requirements for the stirring conditions. Preferably, after the diluted salt is melted, it is continuously stirred, preferably until the aging is completed.

[0027] In step (3), potassium fluorotantalate powder is repeatedly added in multiple times (e.g., 3-20 times) in order to reduce the concentration of potassium fluorotantalate in the diluted salt. There is no restriction on the amount of potassium fluorotantalate powder added each time and the number of times it is added. However, after a lot of research, the inventors found that the specific amount of potassium fluorotantalate powder added each time is related to the target specific surface area of ​​the product tantalum powder. In the case where the proportion of potassium fluorotantalate in the potassium fluorotantalate powder in step (1) is fixed and a fixed amount of diluted salt has been added in step (2), if a tantalum powder with a larger specific surface area is to be prepared, the amount of potassium fluorotantalate powder added each time can be reduced so that potassium fluorotantalate is reduced at a lower concentration. If a tantalum powder with a smaller specific surface area is to be prepared, the amount of potassium fluorotantalate powder added each time is appropriately increased. In other words, the present invention achieves good control of the specific surface area of ​​tantalum powder. Of course, no matter how many times potassium fluorotantalate powder is added, when metallic sodium is added for the last time, all the remaining raw sodium is added to ensure that the potassium fluorotantalate is completely reduced. Preferably, in this step, the temperature in the reduction container is controlled to exceed the melting point of the mixture of the dilute salt and potassium fluorotantalate powder to ensure its melting, for example, 80°C-400°C above its melting point, preferably 250°C-350°C above its melting point. It is easy for a person skilled in the art to understand that the temperature at which the potassium fluorotantalate powder and the dilute salt are melted simultaneously may be different from the melting point of the dilute salt and the melting point of potassium fluorotantalate. When the ratio of the two is different, the "melting point" (also called the apparent melting point) when the mixture is completely melted is also different, but its apparent melting point can be found based on the phase diagram data. Preferably, the temperature is increased after each addition of potassium fluorotantalate powder. Preferably, in order to make the obtained tantalum powder more uniform, before the last addition of metallic sodium, the amount of high-temperature metallic sodium added each time is such that 70-95%, more preferably 70-85%, of the potassium fluorotantalate in the potassium fluorotantalate powder just added is reduced. Such an addition method can avoid the excessive metallic sodium in the reduction container from reacting with the potassium fluorotantalate added in the last time too early (i.e., when it is not melted).

[0028] In step (4), preferably, the tantalum powder is aged by continuing to heat and keep the tantalum powder warm after the reduction is completed. Preferably, the heating is continued for 0.5-5 hours, preferably 2-3 hours. Preferably, the temperature in the reaction vessel is controlled to be the temperature before adding the metallic sodium in step (3). In this step, the excess metallic sodium is carried away from the reduction vessel by the argon gas and separated from the tantalum powder.

[0029] Preferably, in step (3) and / or (4), an inert gas such as argon is always circulated in the reduction container. Preferably, in step (5), the reduction container is kept at a positive pressure until the mixed material is started to be taken out of the reduction container.

[0030] Preferably, separating the tantalum powder in step (5) includes: stopping stirring, then cooling to room temperature while introducing argon gas to maintain a positive pressure in the reduction reaction container to obtain a mixture containing halide and tantalum powder, taking out the mixture from the reduction container, separating and removing part of the by-products that do not wrap the tantalum powder, and further separating the by-products by water acid washing, washing, purifying and drying to obtain the final tantalum powder.

[0031] After step (5), the inventors calculated the yield of tantalum powder and found that the yield of tantalum powder was improved compared with the prior art.

[0032] Preferably, the method of the present invention further comprises step (6) after step (5): water washing and / or pickling, heat treatment such as high temperature and high vacuum heat treatment (or high temperature and high vacuum heat treatment after molten salt assisted sintering according to the invention of patent CN114210973B), oxygen reduction, pickling, and then separating the tantalum powder by filtering and drying, so as to obtain tantalum powder suitable for making high-reliability tantalum capacitors. These treatments are all known processes in the prior art. In other words, these treatments can adopt any process known in the prior art. For example, the high-temperature and high-vacuum heat treatment and passivation here can adopt the methods provided by patents CN201110039272.9, CN201120077798.1, CN201120077680.9, CN201120077305.4, etc., the oxygen reduction can adopt the methods provided by patents CN201420777210.7, CN201420777210.7, and the pickling can adopt the methods provided by patents CN201210548101.3, CN201280077499.5, CN201210548008.2, etc.

[0033] The present invention may also include adding N, P and / or B elements to the tantalum powder after step (5) and / or (6). Of course, raw materials containing these elements may also be used directly. These elements may also be added in the aforementioned high temperature and high vacuum heat treatment step. It is particularly preferred to add the P element. Adding the P element can increase the specific volume. As long as the total amount of P doping is controlled, the effect of increasing the specific volume is the same regardless of when it is added. These can be carried out in a conventional manner in the prior art and will not be described in detail.

[0034] The obtained tantalum powder product was pressed into blocks, sintered, and energized under high voltage conditions. The electrical properties of the energizing blocks were tested, and it was found that the energizing blocks had lower leakage current.

[0035] According to any aspect of the present invention, the obtained product tantalum powder has the advantages of low oxygen content, low leakage current, larger specific capacitance and / or higher breakdown voltage. Moreover, the yield of tantalum powder is higher than that of the prior art. In particular, the present invention has the advantage of making the product tantalum powder have low oxygen content.

[0036] The tantalum powder of the above product was pressed into blocks and sintered, and the electrical properties of the energy blocks were tested, and it was found that the energy blocks had lower leakage current. After energy was performed under the same conditions, the tantalum powder produced by the present invention had a larger specific capacitance, a higher breakdown voltage and / or a lower leakage current than the tantalum powder of the same grade for capacitors produced by other methods. Therefore, the leakage current of tantalum capacitors made of tantalum powder produced by the present invention was improved.

[0037] Without being bound by general theories, the inventors believe that the reasons for the excellent effects of the present invention are as follows: when potassium fluorotantalate powder containing a small amount of alkaline earth metal halogen salt is used for reduction to prepare tantalum powder, metallic sodium reduces the alkaline earth metal halogen salt while reducing potassium fluorotantalate, and the generated alkaline earth metal reduces tantalate, thereby reducing the oxygen content in the final tantalum powder. In this way, the leakage current of tantalum powder is reduced and the electrical performance is improved; moreover, tantalate is reduced to metallic tantalum and deposited on the surface of tantalum powder, thereby increasing the yield of tantalum powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The following drawings are provided for a better understanding of the present invention. These drawings are exemplary and are not intended to limit the scope of the present invention.

[0039] Figure 1 A scanning electron microscope photograph of tantalum powder obtained according to one embodiment of the present invention is given.

[0040] The figure illustrates that the obtained tantalum powder has a more uniform particle size, smoother particles, and a coarser sintering neck. DETAILED DESCRIPTION

[0041] In order to further illustrate the present invention, the preferred embodiments of the present invention are described below in conjunction with the examples, and it can be clearly seen that the objects, features and advantages of the present invention. However, these descriptions are only for further illustrating the features and advantages of the present invention, rather than for limiting the present invention. If the specific conditions are not specified in the examples, they are carried out under normal conditions. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0042] For the purpose of this specification, all numbers indicating the amount of ingredients, reaction conditions, etc. in the specification and claims should be understood as being modified by the term "about" in all cases, unless otherwise specified. Accordingly, the numerical parameters given in the following specification and the appended claims are approximate values, which may vary according to the desired properties that the present invention attempts to obtain, unless otherwise indicated. At least, and without intending to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be interpreted at least in accordance with the number of reported significant figures and in accordance with conventional rounding techniques.

[0043] The analysis of impurity content in tantalum powder is carried out according to Chinese standards GB / T15076.1~15076.15, and the physical properties are carried out according to the provisions of industry standard YS / T573-2015. The test of electrical properties in tantalum powder is carried out according to the provisions of Chinese standard GB / T3137 (using 30% sulfuric acid solution).

[0044] Example 1

[0045] Potassium fluorotantalate powder containing 50 ppm of magnesium chloride, NaCl as a diluent, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180° C. for use.

[0046] Take 100kg of sodium chloride (NaCl) and put it into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon at a flow rate of 40 liters / minute. Heat it to 920℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate powder. After the temperature rises to 920℃, add 4.0kg of metallic sodium for reduction. Repeat the temperature increase and reduction 7 times. After adding potassium fluorotantalate for the 8th time, add 8.20kg of metallic sodium for reduction. After the reduction is completed, keep it at 920℃ for 180 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. Take out the mixture from the reduction container, separate and remove some by-products that do not wrap the tantalum powder, and further separate the by-products by water acid washing, wash, purify and dry to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder was analyzed, and the yield of the tantalum powder was calculated. The measured results are listed in Table 1.

[0047] Then, the tantalum powder was doped with 50 ppm P and heated at 1450 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 150V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0048] Example 2

[0049] Potassium tantalate powder containing 50 ppm of calcium chloride, NaCl as a diluent, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180° C. for use.

[0050] Take 100kg of sodium chloride (NaCl) and put it into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon at a flow rate of 40 liters / minute. Heat it to 920℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate powder. After the temperature rises to 920℃, add 4.0kg of metallic sodium for reduction. Repeat the temperature increase and reduction 7 times. After adding potassium fluorotantalate for the 8th time, add 8.20kg of metallic sodium for reduction. After the reduction is completed, keep it at 920℃ for 180 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. Take out the mixture from the reduction container, separate and remove some by-products that do not wrap the tantalum powder, and further separate the by-products by water acid washing, wash, purify and dry to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder was analyzed, and the yield of the tantalum powder was calculated. The measured results are listed in Table 1.

[0051] Then, the tantalum powder was doped with 50 ppm P and heated at 1450 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 150V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0052] Comparative Example 1

[0053] Powder consisting only of potassium fluorotantalate, NaCl as a diluent, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180° C. for use.

[0054] Take 100kg of sodium chloride (NaCl) and put it into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the process of evacuating and then filling it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow at a flow rate of 40 liters / minute. Heat it to 920℃ and start stirring. Keep it warm for 30 minutes. Then add 15kg of potassium fluorotantalate. After the temperature rises to 920℃, add 4.0kg of metallic sodium for reduction. Repeat the temperature increase and reduction 7 times. After adding potassium fluorotantalate for the 8th time, add 8.20kg of metallic sodium for reduction. After the reduction is completed, keep it warm at 920℃ for 180 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield of the tantalum powder is calculated. The measured results are listed in Table 1.

[0055] Then, the tantalum powder was doped with 50 ppm P and heated at 1450 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 150V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0056] Example 3

[0057] Potassium fluorotantalate powder containing 100 ppm of magnesium chloride, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 220° C. for use.

[0058] Take 50kg of potassium chloride (KCl) and 50kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow at a flow rate of 60 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 10kg of potassium tantalate fluorophosphate powder. After the temperature rises to 900℃, add 2.6kg of sodium metal for reduction. Repeat the temperature increase and reduction 14 times. After adding potassium tantalate fluorophosphate powder for the 15th time, add 8.20kg of sodium metal for reduction. After the reduction is completed, keep the tantalum powder at 900℃ for 120 minutes under the condition of argon circulation, then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield of the tantalum powder is calculated. The measured results are listed in Table 1.

[0059] Then, the tantalum powder was doped with 60 ppm P and heated at 1400 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 100V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0060] Example 4

[0061] Potassium fluorotantalate powder containing 850 ppm of magnesium chloride, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 220° C. for use.

[0062] Take 50kg of potassium chloride (KCl) and 50kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow at a flow rate of 60 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 10kg of potassium tantalate fluorophosphate powder. After the temperature rises to 900℃, add 2.6kg of sodium metal for reduction. Repeat the temperature increase and reduction 14 times. After adding potassium tantalate fluorophosphate powder for the 15th time, add 8.20kg of sodium metal for reduction. After the reduction is completed, keep the tantalum powder at 900℃ for 120 minutes under the condition of argon circulation, then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield of the tantalum powder is calculated. The measured results are listed in Table 1.

[0063] Then, the tantalum powder was doped with 60 ppm P and heated at 1400 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 100V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0064] Comparative Example 2

[0065] Powder composed of potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 220° C. for use.

[0066] Take 50kg of potassium chloride (KCl) and 50kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow at a flow rate of 60 liters / minute. Raise the temperature to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 10kg of potassium fluorotantalate. After the temperature rises to 900℃, add 2.6kg of metallic sodium for reduction; repeat the temperature increase and reduction 14 times. After adding potassium fluorotantalate for the 15th time, add 8.20kg of metallic sodium for reduction. After the reduction is completed, keep the tantalum powder at 900℃ for 120 minutes under the condition of argon circulation, then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield from reducing the input tantalum to obtaining the high-purity tantalum powder is calculated. The measured results are listed in Table 1.

[0067] Then, the tantalum powder was doped with 60 ppm P and heated at 1400 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 100V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0068] Example 5

[0069] Potassium fluorotantalate powder containing 200 ppm magnesium chloride, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180° C. for use.

[0070] Take 100kg of potassium chloride (KCl) and 100kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow at a flow rate of 70 liters / minute. Raise the temperature to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 8kg of potassium tantalate fluorophosphate powder. After the temperature rises to 920℃, add 2.15kg of sodium metal for reduction. Repeat the temperature increase and reduction 9 times. After adding potassium tantalate fluorophosphate powder for the 10th time, add 5.0kg of sodium metal for reduction. After the reduction is completed, keep the temperature at 900℃ for 60 minutes under the condition of argon flow to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield of the tantalum powder is calculated. The measured results are listed in Table 1.

[0071] Then, the tantalum powder was doped with 100 ppm of P and heated at 1230 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 60V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0072] Comparative Example 3

[0073] Powder composed of potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 180° C. for standby use.

[0074] Take 100kg of potassium chloride (KCl) and 100kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow at a flow rate of 70 liters / minute. Raise the temperature to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 8kg of potassium tantalate fluorophosphate powder. After the temperature rises to 920℃, add 2.15kg of sodium metal for reduction. Repeat the temperature increase and reduction 9 times. After adding potassium tantalate fluorophosphate powder for the 10th time, add 5.0kg of sodium metal for reduction. After the reduction is completed, keep the temperature at 900℃ for 60 minutes under the condition of argon flow to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield from reducing the input tantalum to obtaining the high-purity tantalum powder is calculated. The measured results are listed in Table 1.

[0075] Then, the tantalum powder was doped with 100 ppm of P and heated at 1230 °C and below 5.0 × 10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature, and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements, the final tantalum powder obtained was made into an anode block, energized under 60V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements, and the measured results are listed in Table 2.

[0076] Example 7

[0077] Potassium fluorotantalate powder containing 300 ppm magnesium chloride, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 150° C. for use.

[0078] Take 100kg of potassium chloride (KCl) and 100kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Let argon flow in at a flow rate of 90 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 5kg of potassium tantalate fluorophosphate powder. After the temperature rises to 890℃, add 1.3kg of sodium metal for reduction. Repeat the temperature increase and reduction 11 times. After adding potassium tantalate fluorophosphate powder for the 12th time, add 3.8kg of sodium metal for reduction. After the reduction is completed, keep the temperature at 890℃ for 60 minutes under the condition of argon flow to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool it to room temperature. The mixture is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield of the tantalum powder is calculated. The measured results are listed in Table 1.

[0079] Then, the tantalum powder was doped with 150 ppm of P and heated at 1150°C and below 5.0×10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements. The final tantalum powder obtained was made into an anode block, energized under 28V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. The measured results are listed in Table 2.

[0080] Comparative Example 4

[0081] Powder composed of potassium fluorotantalate, KCl and KF as diluents, and metallic sodium are provided as raw materials. The metallic sodium is preheated to a high temperature of 150° C. for use.

[0082] Take 100kg of potassium chloride (KCl) and 100kg of potassium fluoride (KF) and put them into the reduction container. After evacuating the reduction container, fill it with argon to 0.10MPa. Repeat the evacuation and fill it with argon to 0.10MPa twice. Put the reduction container into a heating furnace and heat it. Pass argon gas at a flow rate of 90 liters / minute. Heat it to 900℃ and start stirring. Keep it warm for 30 minutes. Then add 8kg of potassium tantalate fluorophosphate powder. After the temperature rises to 890℃, add 1.3kg of sodium metal for reduction; repeat the temperature increase and reduction 11 times. After adding potassium tantalate fluorophosphate powder for the 12th time, add 3.8kg of sodium metal for reduction. After the reduction is completed, keep it at 890℃ for 60 minutes under the condition of argon circulation to age the tantalum powder. Then stop stirring, maintain the pressure of the reaction container at 0.10MPa, and cool the material to room temperature. The mixed material is taken out from the reduction container, and some by-products that do not cover the tantalum powder are separated and removed, and the by-products are further separated by water acid washing, washed, purified and dried to obtain high-purity tantalum powder. The oxygen content of the high-purity tantalum powder is analyzed, and the yield from reducing the input tantalum to obtaining the high-purity tantalum powder is calculated. The measured results are listed in Table 1.

[0083] Then, the tantalum powder was doped with 150 ppm of P and heated at 1150°C and below 5.0×10 -3 Pa, high temperature and high vacuum heat treatment was performed for 1.0 hour, and then oxygen reduction and acid washing were performed to obtain the final tantalum powder. According to the anode block mass, pressing density, anode block sintering temperature and sintering time specified in Table 1, and other conditions were in accordance with the aforementioned GB / T3137 requirements. The final tantalum powder obtained was made into an anode block, energized under 28V conditions, and then the electrical properties were tested in accordance with the aforementioned GB / T3137 requirements. The measured results are listed in Table 2.

[0084] Table 1 Analysis results of impurity yield of high purity tantalum powder

[0085]

[0086]

[0087] Table 2 Analysis results of electrical properties of finished tantalum powder

[0088]

[0089]

[0090] It can be seen from Table 1 that the preparation of tantalum powder by the present invention improves the yield of tantalum powder and reduces the oxygen content of tantalum powder, which is conducive to obtaining a low leakage current product after subsequent treatment.

[0091] It can be seen from Table 2 that the tantalum powder prepared by the present invention has a higher breakdown voltage and a lower leakage current, and the electrical properties of the tantalum powder are improved.

Claims

1. Potassium fluorotantalate powder used as a raw material in the production of tantalum powder by the sodium reduction potassium fluorotantalate method, the powder containing 5-1000ppm (preferably 50-1000ppm, more preferably 100-850ppm, more preferably 100-500ppm, more preferably 50-150ppm and / or 300-500ppm) of an alkaline earth metal halogen salt and the remainder of potassium fluorotantalate, wherein the alkaline earth metal halogen salt is selected from a halogen salt of magnesium and / or a halogen salt of calcium, such as magnesium chloride.

2. A method for producing tantalum powder by sodium reduction of potassium fluorotantalate, characterized in that The tantalum powder as claimed in claim 1 is used as a raw material.

3. A method for preparing tantalum powder for capacitors by sodium reduction of potassium fluorotantalate, comprising the following steps: (1) providing potassium fluorotantalate powder, a diluent salt (preferably selected from alkali metal halides), and liquid metallic sodium as raw materials, wherein the potassium fluorotantalate powder contains 5-1000 ppm of alkaline earth metal halide, (2) placing the diluted salt into a reduction container, evacuating the container, and then introducing an inert gas such as argon, and then heating the diluted salt in the reduction container until it melts while the inert gas is kept flowing (at a flow rate of 20-100 liters / minute), (3) adding a portion of potassium fluorotantalate powder to a reduction container, monitoring the temperature to ensure that the mixture of potassium fluorotantalate powder and diluent salt is melted, and then adding liquid metallic sodium to reduce the portion of potassium fluorotantalate, repeating the process multiple times (e.g., 3-10 times) until all the potassium fluorotantalate powder and metallic sodium raw materials are used up. (4) After the reduction is completed, the tantalum powder is aged, and (5) Then, the tantalum powder is separated.

4. The method according to claim 3, further comprising step (6) after step (5): The tantalum powder is subjected to salt bath heat treatment and / or agglomeration heat treatment, the metal magnesium chips are subjected to oxygen reduction treatment and further pickled, purified and dried to obtain the product tantalum powder.

5. The method according to claim 3 or 4, wherein in step (1), the sodium metal is preheated to more than 150°C, such as 180°C-500°C, more preferably 200-350°C, more preferably 200-260°C, more preferably 190°C-240°C, such as 210°C.

6. The method according to any one of claims 3 to 5, wherein in step (1), the amount of metallic sodium is in excess of the theoretical amount required for complete reduction of potassium fluorotantalate, for example, 1-3% in excess, preferably 1.5-2.5% in excess.

7. The method according to any one of claims 3 to 6, wherein in step (2) the molten diluent salt is stirred, preferably heated to a temperature exceeding its melting point by 80°C, preferably exceeding 150°C, more preferably exceeding 200°C.

8. A method according to any one of claims 3 to 7, wherein melting of the mixture of dilute salt and potassium fluorotantalate powder is ensured by controlling the temperature in the reduction vessel to exceed the melting point of the mixture, e.g. 80°C to 400°C, preferably 250°C to 350°C.

9. The method according to any one of claims 3 to 8, wherein before the last addition of metallic sodium, the amount of metallic sodium added each time is such that 70-95%, more preferably 70-85%, of the potassium fluorotantalate in the potassium fluorotantalate powder just added is reduced.

10. Tantalum powder produced by using the potassium fluorotantalate powder according to claim 1 or by the method according to any one of claims 2 to 9, and use thereof in capacitors.

Citation Information

Patent Citations

  • Thermal treatment method of tantalum powder

    CN102120258A

  • Stirring water-washing method and device for producing tantalum powder by reducing potassium fluotantalate via metallic sodium

    CN102990076A

  • Method for purifying tantalum powder

    CN102994780A

  • Target powder purification method and device

    CN105051223A

  • Technology for making tantalum powder

    CN1069564C

Cited By

  • Preparation method of pure tantalum standard sample for trace element analysis

    CN120028120A

  • Preparation method of pure tantalum standard sample for trace element analysis

    CN120028120B