Vinyl chloride resin composition, vinyl chloride resin molded article, and laminate
By adding an appropriate amount of lactone-based compounds and plasticizer to the vinyl chloride resin composition, the problem of odor odor in the molded body of vinyl chloride resin is solved, and the odor suppression and the improvement of low-temperature tensile elongation are achieved. It is suitable for automobiles Decorative materials.
Patent Information
- Application Number
- CN202380022986.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-05
AI Technical Summary
Vinyl chloride resin molded bodies have odor problems in car interior materials, which affects the comfort of the occupants.
The vinyl chloride resin molded body formed by adding a lactone-based compound with a content of 0.005 parts by mass or more and 15 parts by mass or less to the vinyl chloride resin composition is combined with an appropriate amount of plasticizer to suppress the generation of odor.
It effectively inhibits the odor of vinyl chloride resin molded bodies and improves its low-temperature tensile elongation, making it suitable for automotive instrument panels and other components.
Smart Images

Figure CN118900887A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a vinyl chloride resin composition, a vinyl chloride resin molded body and a laminate. Background Art
[0002] Vinyl chloride resin is generally used in a variety of applications because of its excellent properties such as cold resistance, heat resistance, and oil resistance.
[0003] Specifically, for example, in the formation of automobile interior parts such as automobile instrument panels and door trims, automobile interior materials such as skins formed of vinyl chloride resin molded bodies and laminates formed by lining the skins formed of vinyl chloride resin molded bodies with foamed bodies such as foamed polyurethane are used.
[0004] Furthermore, the vinyl chloride resin molded body constituting the surface of automobile interior parts such as automobile instrument panels can be produced by powder molding a vinyl chloride resin composition containing vinyl chloride resin, plasticizers, and additives such as pigments using a known molding method such as powder slush molding (for example, refer to Patent Document 1).
[0005] Specifically, for example, in Patent Document 1, a skin composed of a vinyl chloride resin molded body is produced by powder slush molding a vinyl chloride resin composition containing vinyl chloride resin particles, a trimellitate plasticizer, and additives such as a pigment composed of a mixture of phthalocyanine blue, titanium oxide, and carbon.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent document 1: Japanese Patent Application Laid-Open No. 8-291243. Summary of the invention
[0009] Problem that the invention aims to solve
[0010] Here, when a vinyl chloride resin molded article is used as an automobile interior material such as a surface skin of an automobile instrument panel, there is a problem that odor is generated from the vinyl chloride resin molded article, causing discomfort to the occupants of the automobile. Therefore, it is required to suppress the generation of odor from the vinyl chloride resin molded article.
[0011] Therefore, an object of the present invention is to provide a vinyl chloride resin composition capable of forming a vinyl chloride resin molded article in which the generation of odor is suppressed.
[0012] Another object of the present invention is to provide a vinyl chloride resin molded body in which generation of odor is suppressed.
[0013] Furthermore, an object of the present invention is to provide a laminate having the vinyl chloride resin molded article and in which the generation of odor is suppressed.
[0014] Solutions for solving problems
[0015] The present inventors have conducted intensive research for the purpose of solving the above-mentioned problems. The present inventors have found that if a vinyl chloride resin composition to which a lactone compound having a cis-isomer content of a predetermined value or more is added in a predetermined amount relative to the vinyl chloride resin is molded, a vinyl chloride resin molded body with suppressed odor generation can be obtained, thereby completing the present invention.
[0016] That is, the object of the present invention is to advantageously solve the above-mentioned problems. [1] The vinyl chloride resin composition of the present invention is characterized by comprising a vinyl chloride resin, a plasticizer and a lactone compound represented by the following formula (I):
[0017] [Chemical formula 1]
[0018]
[0019] In formula (I), R 1 ~R 4 Each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, a thiol group or a hydrocarbon group which may have a substituent, and the content of the lactone compound is 0.005 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the vinyl chloride resin. When a vinyl chloride resin composition comprising a vinyl chloride resin, a plasticizer and a lactone compound having the above-specified structure is used, and the content of the lactone compound is within a specified range, a vinyl chloride resin molded body with suppressed odor generation can be formed.
[0020] Here, [2] the vinyl chloride resin composition described in [1] is preferably the above R 1 If R in the above formula (I) is used 1 A lactone compound which is a hydrocarbon group can further suppress the generation of odor from the formed vinyl chloride resin molded article.
[0021] [3] The vinyl chloride resin composition described in [2] above preferably constitutes the R 1 The number of carbon atoms of the hydrocarbon group is 1 or more and 20 or less. If R in the above formula (I) is 1 When the number of carbon atoms of the hydrocarbon group is 1 or more and 20 or less, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed.
[0022] [4] The vinyl chloride resin composition described in [2] or [3] above preferably constitutes the above R 1 The hydrocarbon group is a chain hydrocarbon group. If R in the above formula (I) 1 If the hydrocarbon group is a chain hydrocarbon group, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed.
[0023] [5] The vinyl chloride resin composition described in any one of [2] to [4] above preferably constitutes the R 1 The hydrocarbon group is an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms. 1 If the hydrocarbon group is the alkyl group or alkenyl group specified above, the generation of odor from the formed vinyl chloride resin molded product can be further suppressed.
[0024] [6] The vinyl chloride resin composition described in any one of [2] to [5] above preferably constitutes the R 1 The hydrocarbon group is an alkenyl group having 2 or more and 10 or less carbon atoms. 1 If the hydrocarbon group is the alkenyl group specified above, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed.
[0025] [7] The vinyl chloride resin composition described in any one of [1] to [6] is preferably 2 ~R 4 If R in the above formula (I) 2 ~R 4 If all of them are hydrogen atoms, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed.
[0026] [8] In the vinyl chloride resin composition according to any one of [1] to [7], the lactone compound preferably contains jasmine lactone. When jasmine lactone is used as the lactone compound, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed.
[0027] Furthermore, [9] the vinyl chloride resin composition described in any one of [1] to [8] above preferably contains the plasticizer in an amount of 50 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the vinyl chloride resin. If the amount of the plasticizer relative to the vinyl chloride resin is within the above-specified range, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed and the tensile elongation of the vinyl chloride resin molded article at low temperatures (hereinafter sometimes referred to as "low-temperature tensile elongation") can be sufficiently high.
[0028]
[10] The vinyl chloride resin composition described in any one of [1] to [9] is preferably used for powder molding. When the vinyl chloride resin composition is used for powder molding, a vinyl chloride resin molded body that can be preferably used as an automobile interior material such as an automobile instrument panel skin can be easily obtained.
[0029]
[11] The vinyl chloride resin composition described in any one of [1] to
[10] is preferably used for powder slush molding. If the vinyl chloride resin composition is used for powder slush molding, it is easier to obtain a vinyl chloride resin molded body that can be used well as an automobile interior material such as a car instrument panel skin.
[0030] Furthermore, the present invention aims to advantageously solve the above-mentioned problems.
[12] The vinyl chloride resin molded article of the present invention is characterized in that it is molded from the vinyl chloride resin composition described in any one of [1] to
[11] above. The vinyl chloride resin molded article molded from the vinyl chloride resin composition thus suppresses the generation of odor.
[0031]
[13] The vinyl chloride resin molded article described in
[12] is preferably used as a surface skin of an automobile instrument panel. The vinyl chloride resin molded article of the present invention can be preferably used as a surface skin of an automobile instrument panel in which odor generation is suppressed.
[0032] Furthermore, the present invention aims to advantageously solve the above-mentioned problems.
[14] The laminate of the present invention is characterized in that it comprises a foamed polyurethane molded body and a vinyl chloride resin molded body as described in
[12] or
[13] . The laminate comprising the foamed polyurethane molded body and the vinyl chloride resin molded body suppresses the generation of odor.
[0033]
[15] The laminate described in
[14] is preferably used for automobile instrument panels. When the laminate of the present invention is used for automobile instrument panels, it is possible to produce an automobile instrument panel in which odor generation from the surface is suppressed.
[0034] Effects of the Invention
[0035] According to the present invention, there can be provided a vinyl chloride resin composition capable of forming a vinyl chloride resin molded article in which generation of odor is suppressed.
[0036] Furthermore, according to the present invention, it is possible to provide a vinyl chloride resin molded body in which generation of odor is suppressed.
[0037] Furthermore, according to the present invention, it is possible to provide a laminate having the vinyl chloride resin molded article and in which the generation of odor is suppressed. DETAILED DESCRIPTION
[0038] Hereinafter, embodiments of the present invention will be described in detail.
[0039] The vinyl chloride resin composition of the present invention can be used, for example, to form the vinyl chloride resin molded body of the present invention. Furthermore, the vinyl chloride resin molded body formed using the vinyl chloride resin composition of the present invention can be preferably used as an automobile interior material such as a surface skin of automobile interior parts such as automobile instrument panels and door trims.
[0040] The vinyl chloride resin molded article of the present invention can be used, for example, to form a laminate of the present invention. Furthermore, the laminate formed using the vinyl chloride resin molded article of the present invention can be preferably used as an automobile interior material used, for example, when manufacturing automobile interior parts such as automobile instrument panels and door trims.
[0041] (Vinyl chloride resin composition)
[0042] The vinyl chloride resin composition of the present invention is characterized by comprising (a) a vinyl chloride resin, (b) a plasticizer and (c) a lactone compound having a predetermined structure (hereinafter sometimes referred to as "(c) lactone compound"), wherein the content of the (c) lactone compound is within a predetermined range.
[0043] Furthermore, the vinyl chloride resin composition of the present invention may arbitrarily contain additives other than the above-mentioned (a) vinyl chloride resin, (b) plasticizer and (c) lactone compound.
[0044] Moreover, the vinyl chloride resin composition of the present invention contains at least the above-mentioned (a) vinyl chloride resin, (b) plasticizer and (c) lactone compound, and the content of (c) lactone compound is within a prescribed range, so that a vinyl chloride resin molded body with suppressed odor generation can be formed.
[0045] Therefore, by using the vinyl chloride resin composition of the present invention, it is possible to obtain a vinyl chloride resin molded article suitable as an automobile interior material such as an automobile instrument panel skin and a door trim skin in which odor generation is suppressed.
[0046] Furthermore, a vinyl chloride resin molded article formed using the vinyl chloride resin composition of the present invention is also excellent in low-temperature tensile elongation.
[0047] In addition, for example, from the viewpoint of easily obtaining a vinyl chloride resin molded body that can be favorably used as an automobile interior material using the vinyl chloride resin composition of the present invention, the vinyl chloride resin composition of the present invention is preferably used for powder molding, and more preferably for powder slush molding.
[0048] <(a) Vinyl chloride resin>
[0049] As the (a) vinyl chloride resin, a granular vinyl chloride resin is generally used. Moreover, as the (a) vinyl chloride resin, for example, one or two or more vinyl chloride resin particles can be contained, and one or two or more vinyl chloride resin microparticles can be further contained. The (a) vinyl chloride resin preferably contains at least vinyl chloride resin particles, and more preferably contains vinyl chloride resin particles and vinyl chloride resin microparticles.
[0050] Furthermore, the (a) vinyl chloride resin can be produced by any conventionally known production method such as suspension polymerization, emulsion polymerization, solution polymerization, or bulk polymerization.
[0051] In the present specification, “resin particles” refer to particles having a particle size of 30 μm or more, and “resin fine particles” refer to particles having a particle size of less than 30 μm.
[0052] In addition, as (a) vinyl chloride resin, in addition to homopolymers formed from vinyl chloride monomer units, vinyl chloride copolymers preferably containing 50% by mass or more, more preferably containing 70% by mass or more of vinyl chloride monomer units can also be cited. Moreover, as specific examples of monomers (comonomers) that can constitute vinyl chloride copolymers and can be copolymerized with vinyl chloride monomers, for example, monomers described in International Publication No. 2016 / 098344 can be used. In addition, these components can be used alone or in combination of two or more in any ratio.
[0053] <<Vinyl chloride resin pellets>>
[0054] In a vinyl chloride resin composition, the vinyl chloride resin particles generally function as a base resin (substrate). In addition, the vinyl chloride resin particles are preferably produced by a suspension polymerization method.
[0055] [Average degree of polymerization]
[0056] Moreover, the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is preferably 800 or more, more preferably 900 or more, preferably 5000 or less, more preferably 3000 or less, and further preferably 2800 or less. If the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is above the above lower limit, the physical strength of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be sufficiently highly ensured and, for example, tensile properties, especially tensile elongation, can be improved. Moreover, the vinyl chloride resin molded body with good tensile elongation can be preferably used as, for example, an automobile interior material such as the surface of an automobile instrument panel that does not scatter fragments but cracks as designed when an airbag is inflated and deployed, and has excellent ductility. On the other hand, if the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is below the above upper limit, the solubility of the vinyl chloride resin composition can be improved.
[0057] In the present invention, the "average degree of polymerization" can be measured in accordance with JIS K6720-2.
[0058] [Average particle size]
[0059] In addition, the average particle size of the vinyl chloride resin particles is usually 30 μm or more, preferably 50 μm or more, more preferably 100 μm or more, preferably 500 μm or less, more preferably 200 μm or less. If the average particle size of the vinyl chloride resin particles is above the above lower limit, the powder fluidity of the vinyl chloride resin composition can be improved. On the other hand, if the average particle size of the vinyl chloride resin particles is below the above upper limit, the solubility of the vinyl chloride resin composition can be improved, and the surface smoothness of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be improved.
[0060] In the present invention, the "average particle size" can be measured as a volume average particle size by a laser diffraction method in accordance with JIS Z8825.
[0061] [Content ratio]
[0062] Moreover, the content of the vinyl chloride resin particles in the (a) vinyl chloride resin is preferably 70% by mass or more, more preferably 80% by mass or more, and can be 100% by mass, preferably 95% by mass or less, and more preferably 90% by mass or less. If the content of the vinyl chloride resin particles in the (a) vinyl chloride resin is above the above lower limit, the physical strength of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be fully ensured and the tensile elongation can be improved. In addition, if the content of the vinyl chloride resin particles in the (a) vinyl chloride resin is below the above upper limit, the powder fluidity of the vinyl chloride resin composition can be improved.
[0063] <<Vinyl chloride resin particles>>
[0064] In a vinyl chloride resin composition, vinyl chloride resin fine particles generally function as a release agent (powder flowability improver). In addition, the vinyl chloride resin fine particles are preferably produced by an emulsion polymerization method.
[0065] [Average degree of polymerization]
[0066] Furthermore, the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles is preferably 500 or more, more preferably 700 or more, preferably 2600 or less, more preferably 2400 or less. If the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles as the release agent is at least the above lower limit, the powder flowability of the vinyl chloride resin composition can be improved and the tensile elongation of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be improved. On the other hand, if the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles is at most the above upper limit, the solubility of the vinyl chloride resin composition can be improved and the surface smoothness of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be improved.
[0067] [Average particle size]
[0068] In addition, the average particle size of the vinyl chloride resin microparticles is usually less than 30 μm, preferably less than 10 μm, more preferably less than 5 μm, preferably more than 0.1 μm, more preferably more than 1 μm. If the average particle size of the vinyl chloride resin microparticles is greater than the above lower limit, for example, the size of the microparticles as a release agent will not be too small, and the powder fluidity of the vinyl chloride resin composition can be improved. On the other hand, if the average particle size of the vinyl chloride resin microparticles is less than the above upper limit, the solubility of the vinyl chloride resin composition can be improved, and the surface smoothness of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be improved.
[0069] [Content ratio]
[0070] Furthermore, the content of the vinyl chloride resin microparticles in the (a) vinyl chloride resin may be 0% by mass, preferably 5% by mass or more, more preferably 10% by mass or more, preferably 30% by mass or less, more preferably 20% by mass or less. If the content of the vinyl chloride resin microparticles in the (a) vinyl chloride resin is greater than the above lower limit, the powder fluidity of the vinyl chloride resin composition can be improved. On the other hand, if the content of the vinyl chloride resin microparticles in the (a) vinyl chloride resin is less than the above upper limit, the physical strength of the vinyl chloride resin molded body formed using the vinyl chloride resin composition can be improved.
[0071] <(b) Plasticizer>
[0072] The (b) plasticizer is a component that can impart sufficient flexibility to a vinyl chloride resin molded article formed using the vinyl chloride resin composition. For example, by using the (b) plasticizer in the vinyl chloride resin composition, the formed vinyl chloride resin molded article can exhibit excellent low-temperature tensile elongation.
[0073] In addition, it is speculated that (b) the plasticizer will become one of the causes of odor generated from the vinyl chloride resin molded product, but it is considered that by using (b) the plasticizer and the (c) lactone compound described later in the vinyl chloride resin composition, the formed vinyl chloride resin molded product can exhibit excellent low-temperature tensile elongation and also suppress the generation of odor.
[0074] <<Content>>
[0075] The content of the (b) plasticizer in the vinyl chloride resin composition is more preferably 50 parts by mass or more, further preferably 60 parts by mass or more, further preferably 70 parts by mass or more, and further preferably 80 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 180 parts by mass or less, further preferably 150 parts by mass or less, further preferably 120 parts by mass or less, and further preferably 100 parts by mass or less.
[0076] If the content of the (b) plasticizer in the vinyl chloride resin composition is not less than the above lower limit, the generation of odor from the formed vinyl chloride resin molded body can be sufficiently suppressed and the low-temperature tensile elongation of the vinyl chloride resin molded body can be further improved. On the other hand, if the content of the (b) plasticizer in the vinyl chloride resin composition is not more than the above upper limit, the low-temperature tensile elongation of the formed vinyl chloride resin molded body can be sufficiently highly ensured and the generation of odor from the vinyl chloride resin molded body can be further suppressed.
[0077] <<Type>>
[0078] As the (b) plasticizer, for example, the primary plasticizer and auxiliary plasticizer described in International Publication No. 2016 / 098344 can be used. These components may be used alone or in combination of two or more at any ratio.
[0079] Among the above plasticizers, from the viewpoint of further improving the low-temperature tensile elongation of the formed vinyl chloride resin molded body, it is preferred to use at least a primary plasticizer as the (b) plasticizer, and it is more preferred to use a primary plasticizer and an auxiliary plasticizer in combination. Specifically, it is preferred to use at least a trimellitic acid ester as the (b) plasticizer, and it is more preferred to use a trimellitic acid ester and an epoxidized vegetable oil in combination.
[0080] <<(b1) Trimellitate esters>>
[0081] The (b1) trimellitic acid ester which can be contained in the (b) plasticizer is preferably an ester compound of trimellitic acid and a monohydric alcohol.
[0082] Specific examples of the monohydric alcohol include, but are not limited to, aliphatic alcohols such as 1-hexanol, 1-heptanol, 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, and 1-dodecanol. As the monohydric alcohol, aliphatic alcohols having 6 to 18 carbon atoms are particularly preferred.
[0083] As the trimellitic acid ester (b1), a triester in which substantially all the carboxyl groups of trimellitic acid are esterified with the monohydric alcohol is particularly preferred. The alcohol residues in the triester may be derived from the same alcohol or from different alcohols.
[0084] The trimellitic acid ester (b1) may be composed of a single compound or a mixture of different compounds.
[0085] Specific examples of preferred (b1) trimellitic acid esters are tri-n-hexyl trimellitate, tri-n-heptyl trimellitate, tri-n-octyl trimellitate, tri(2-ethylhexyl) trimellitate, tri-n-nonyl trimellitate, tri-n-decyl trimellitate, tri-isodecyl trimellitate, tri-n-undecyl trimellitate, tri-n-dodecyl trimellitate, tri-n-alkyl trimellitate (esters having two or more alkyl groups with different carbon numbers [wherein the carbon numbers are 6 to 18] in the molecule), tri-n-alkyl trimellitate (esters having two or more alkyl groups with different carbon numbers [wherein the carbon numbers are 6 to 18] in the molecule), and mixtures thereof.
[0086] The content of the trimellitic acid ester (b1) in the (b) plasticizer is not particularly limited, but is preferably 75% by mass or more, more preferably 88% by mass or more, and even more preferably 94% by mass or more, and is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less. If the content of the trimellitic acid ester (b1) in the (b) plasticizer is within the above-specified range, the low-temperature tensile elongation of the formed vinyl chloride resin molded article can be further improved.
[0087] In addition, the content of (b1) trimellitic acid ester in the vinyl chloride resin composition is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, further preferably 65 parts by mass or more, further preferably 75 parts by mass or more, preferably 199 parts by mass or less, more preferably 179 parts by mass or less, further preferably 148 parts by mass or less, further preferably 118 parts by mass or less, and further preferably 98 parts by mass or less. If the content of (b1) trimellitic acid ester in the vinyl chloride resin composition is within the above-specified range, the low-temperature tensile elongation of the formed vinyl chloride resin molded body can be further improved. In addition, if the content of (b1) trimellitic acid ester in the vinyl chloride resin composition is below the above-mentioned upper limit, the generation of odor from the vinyl chloride resin molded body can be further suppressed.
[0088] <<(b2) Epoxidized vegetable oil>>
[0089] Examples of the epoxidized vegetable oil (b2) that may be included in the (b) plasticizer include epoxidized soybean oil and epoxidized linseed oil. In particular, epoxidized soybean oil is preferably used from the viewpoint of further improving the low-temperature tensile elongation of the resulting vinyl chloride resin molded article.
[0090] The content of the epoxidized vegetable oil (b2) in the plasticizer (b) is not particularly limited, but is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 25% by mass or less, more preferably 12% by mass or less, and even more preferably 6% by mass or less. If the content of the epoxidized vegetable oil (b2) in the plasticizer (b) is within the above-specified range, the low-temperature tensile elongation of the formed vinyl chloride resin molded article can be further improved.
[0091] In addition, the content of the epoxidized vegetable oil (b2) in the vinyl chloride resin composition is not particularly limited, but is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the above-mentioned (a) vinyl chloride resin. If the content of the epoxidized vegetable oil (b2) in the vinyl chloride resin composition is within the above-specified range, the low-temperature tensile elongation of the formed vinyl chloride resin molded article can be further improved.
[0092] <Lactone compounds>
[0093] The (c) lactone compound in the vinyl chloride resin composition is a component that can suppress the generation of odor from the formed vinyl chloride resin molded product. In addition, it is presumed that the cause of the odor generation is the components contained in the vinyl chloride resin composition for forming the vinyl chloride resin molded product (for example, the above-mentioned (a) vinyl chloride resin, (b) plasticizer, and additives described later, etc.).
[0094] Here, the (c) lactone compound is a compound represented by the following formula (I).
[0095] [Chemical formula 2]
[0096]
[0097] In formula (I), R 1 ~R 4 Each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, a thiol group, or a hydrocarbon group which may have a substituent.
[0098] As a component of R 1 ~R 4 The halogen atom includes a fluorine atom, a chlorine atom and the like.
[0099] As a component of R 1 ~R 4The (unsubstituted) hydrocarbon group may be a cyclic hydrocarbon group such as an aromatic hydrocarbon group, or a chain hydrocarbon group, and is preferably a chain hydrocarbon group from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded product. Furthermore, the chain hydrocarbon group may be a straight chain or a branched chain, and is preferably a straight chain from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded product.
[0100] Here, the above-mentioned hydrocarbon group may be an unsaturated hydrocarbon group having an unsaturated bond (carbon-carbon double bond, carbon-carbon triple bond) or a saturated hydrocarbon group having no unsaturated bond. From the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded product, an unsaturated hydrocarbon group is preferred.
[0101] In addition, the number of carbon atoms in the above-mentioned hydrocarbon group may be 1 or more, and from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded product, it is preferably 2 or more, more preferably 3 or more, further preferably 4 or more, further preferably 5 or more, preferably 20 or less, more preferably 10 or less, further preferably 8 or less, further preferably 6 or less, and particularly preferably 5.
[0102] In being able to constitute R 1 ~R 4 When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include a halogen atom (chlorine atom, fluorine atom, etc.), a hydroxyl group, an amino group, a thiol group, etc. In addition, the hydrocarbon group may have only one of these substituents, or may have two or more of these substituents. 1 It may have one substituent or may have two or more substituents.
[0103] In addition, from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded article, R 1 ~R 4 The hydrocarbon group is preferably a hydrocarbon group having no substituent.
[0104] Furthermore, from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded article, R 1 ~R 4 The hydrocarbon group is preferably an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms.
[0105] As a component of R 1 ~R 4More preferred specific examples of the hydrocarbon group include, from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded article, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, 2-methylbutyl, 1-methylbutyl, n-hexyl, isohexyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, n-heptyl, isoheptyl, n-octyl, isooctyl, 2-ethylhexyl, nonyl, decyl and the like. Alkyl groups having 1 to 10 atoms; alkenyl groups having 2 to 10 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl (allyl), 2-butenyl, 3-butenyl, isobutenyl, 4-pentenyl, 3-pentenyl, trans-2-pentenyl, cis-2-pentenyl, 1-pentenyl, 3-methyl-2-pentenyl, 5-hexenyl, 3-hexenyl, 2-hexenyl, heptenyl, octenyl, nonenyl and decenyl.
[0106] From the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded article, as a 1 ~R 4 The hydrocarbon group is more preferably an alkenyl group having 2 or more and 10 or less carbon atoms. The alkenyl group preferably has 3 or more carbon atoms, more preferably 4 or more carbon atoms, more preferably 5 or more carbon atoms, preferably 8 or less carbon atoms, more preferably 6 or less carbon atoms, and particularly preferably 5 carbon atoms. 1 ~R 4 The alkenyl group of the hydrocarbon group is particularly preferably a pentenyl group such as 4-pentenyl, 3-pentenyl, trans-2-pentenyl, cis-2-pentenyl, and 1-pentenyl.
[0107] In the above formula (I), R 1 ~R 4 There are no particular limitations on the above-mentioned groups as long as they each independently represent a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, a thiol group, or a hydrocarbon group which may have a substituent.
[0108] Furthermore, from the viewpoint of further suppressing the generation of odor from the formed vinyl chloride resin molded article, it is preferred that R 1 represents at least a hydrocarbon group, and preferably R 2 ~R 4 At least one of represents a hydrogen atom, and more preferably R 2 ~R 4 At least two of them represent hydrogen atoms, and more preferably R 2 ~R 4 Both represent hydrogen atoms.
[0109] As the lactone compound (c) represented by the above formula (I), it is particularly preferred to use R 1 represents cis-2-pentenyl, R 2 ~R 4The lactone compounds all represent hydrogen atoms, namely, jasmine lactone represented by the following formula (Ia).
[0110] [Chemical formula 3]
[0111]
[0112] The content of the lactone compound (c) in the vinyl chloride resin composition needs to be 0.005 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.06 parts by mass or more, further preferably 0.07 parts by mass or more, and further preferably 0.08 parts by mass or more, relative to 100 parts by mass of the above-mentioned (a) vinyl chloride resin, and needs to be 15 parts by mass or less, preferably 10 parts by mass or less, more preferably 5 parts by mass or less, further preferably 0.8 parts by mass or less, further preferably 0.5 parts by mass or less, and particularly preferably 0.1 parts by mass or less. If the content of the lactone compound (c) in the vinyl chloride resin composition is within the above-specified range, the generation of odor from the formed vinyl chloride resin molded body can be sufficiently suppressed. In addition, if the content of the lactone compound (c) in the vinyl chloride resin composition is within the above-specified range, the low-temperature tensile elongation of the formed vinyl chloride resin molded body can be sufficiently highly ensured.
[0113] The content of the lactone compound (c) in the vinyl chloride resin composition is preferably 0.005 parts by mass or more, more preferably 0.05 parts by mass or more, further preferably 0.06 parts by mass or more, further preferably 0.07 parts by mass or more, and further preferably 0.08 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, further preferably 5 parts by mass or less, further preferably 0.8 parts by mass or less, further preferably 0.5 parts by mass or less, and particularly preferably 0.1 parts by mass or less. If the content of the lactone compound (c) in the vinyl chloride resin composition is within the above-specified range, the generation of odor from the formed vinyl chloride resin molded article can be further suppressed and the low-temperature tensile elongation of the vinyl chloride resin molded article can be sufficiently high.
[0114] <Additives>
[0115] The vinyl chloride resin composition of the present invention may contain various additives in addition to the above-mentioned components. The additives are not particularly limited, and examples thereof include: lubricants; stabilizers such as perchloric acid-treated hydrotalcite, zeolite, β-diketone, fatty acid metal salts, etc.; release agents; other release agents other than the above-mentioned vinyl chloride resin particles; impact modifiers; perchloric acid compounds (sodium perchlorate, potassium perchlorate, etc.) other than perchloric acid-treated hydrotalcite; antioxidants; antifungal agents; flame retardants; antistatic agents; fillers; light stabilizers; foaming agents; pigments, etc.
[0116] Furthermore, as the additives that may be contained in the vinyl chloride resin composition of the present invention, for example, additives described in International Publication No. 2016 / 098344 may be used, and the preferred content thereof may also be the same as that described in International Publication No. 2016 / 098344.
[0117] <Method for preparing vinyl chloride resin composition>
[0118] The vinyl chloride resin composition of the present invention can be prepared by mixing the above-mentioned components.
[0119] Here, the mixing method of the above-mentioned (a) vinyl chloride resin, (b) plasticizer, (c) lactone compound and various additives further mixed as needed is not particularly limited, and for example, the following method can be mentioned: a method of mixing the components other than the release agent (including vinyl chloride resin particles) by dry mixing, and then adding the release agent and mixing. Here, a Henschel mixer is preferably used for dry mixing. In addition, the temperature during dry mixing is not particularly limited, but is preferably 50° C. or more, more preferably 70° C. or more, and preferably 200° C. or less.
[0120] <Application of vinyl chloride resin composition>
[0121] Furthermore, the obtained vinyl chloride resin composition is not particularly limited, but can be preferably used for powder molding, and can be more preferably used for powder slush molding.
[0122] (Vinyl chloride resin molded article)
[0123] The vinyl chloride resin molded article of the present invention is characterized in that it is obtained by molding the above-mentioned vinyl chloride resin composition by any method. Moreover, since the vinyl chloride resin molded article of the present invention is formed using the above-mentioned vinyl chloride resin composition, it usually contains at least (a) vinyl chloride resin, (b) plasticizer and a predetermined amount of (c) lactone compound, and the generation of odor can be suppressed. In addition, since the vinyl chloride resin molded article of the present invention is formed using the above-mentioned vinyl chloride resin composition, it is also excellent in low-temperature tensile elongation.
[0124] Therefore, the laminate formed by lining the polyurethane foam molded article with the vinyl chloride resin molded article of the present invention can be preferably used as an automobile interior material such as the surface of an automobile instrument panel because the generation of odor is suppressed.
[0125] <Method for forming a vinyl chloride resin molded article>
[0126] Here, when the vinyl chloride resin molded body is formed by powder slush molding, the metal mold temperature during powder slush molding is not particularly limited, but is preferably 200°C or more, more preferably 220°C or more, and preferably 300°C or less, more preferably 280°C or less.
[0127] Furthermore, when manufacturing a vinyl chloride resin molded body, there is no particular limitation, and for example, the following method can be used. That is, the vinyl chloride resin composition of the present invention is sprinkled into a metal mold in the above-mentioned temperature range, and left for a period of more than 5 seconds and less than 30 seconds, and then the remaining vinyl chloride resin composition is shaken off, and then left for a period of more than 30 seconds and less than 3 minutes at an arbitrary temperature. Thereafter, the metal mold is cooled to a temperature of more than 10°C and less than 60°C, and the obtained vinyl chloride resin molded body of the present invention is demolded from the metal mold. Then, a sheet-like molded body having a shape similar to that of the metal mold is obtained.
[0128] (Laminated body)
[0129] The laminate of the present invention comprises a foamed polyurethane molded body and the above-mentioned vinyl chloride resin molded body. In addition, the vinyl chloride resin molded body usually constitutes one surface of the laminate.
[0130] Furthermore, the laminate of the present invention can suppress the generation of odors because it has, for example, a vinyl chloride resin molded body formed using the vinyl chloride resin composition of the present invention. Therefore, the laminate of the present invention can be preferably used as an automobile interior material for forming automobile interior parts, particularly automobile instrument panels.
[0131] Here, the lamination method of the foamed polyurethane molded body and the vinyl chloride resin molded body is not particularly limited, and the following methods can be used, for example. That is, the following methods can be mentioned: (1) a method of laminating the foamed polyurethane molded body and the vinyl chloride resin molded body by using heat fusion, heat bonding, or a known adhesive or the like after preparing the foamed polyurethane molded body and the vinyl chloride resin molded body separately; (2) a method of directly forming the foamed polyurethane molded body on the vinyl chloride resin molded body by reacting isocyanates and polyols, etc., which are raw materials of the foamed polyurethane molded body, on the vinyl chloride resin molded body, polymerizing them, and foaming polyurethane by a known method. From the perspective of simplifying the process and the aspect of being easy to firmly bond the vinyl chloride resin molded body and the foamed polyurethane molded body when obtaining a laminated body of various shapes, the latter method (2) is particularly preferred.
[0132] Example
[0133] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.
[0134] Furthermore, the low-temperature tensile elongation and odor intensity of the vinyl chloride resin molded sheet were measured and evaluated by the following methods.
[0135] <Tensile elongation at low temperature>
[0136] The vinyl chloride resin molded sheet punched out using a No. 1 dumbbell cutter described in JIS K6251 was measured for tensile elongation at break (%) at a low temperature of -35°C at a tensile speed of 200 mm / min in accordance with JIS K7113. The larger the value of tensile elongation at break, the better the tensile elongation at low temperature (low-temperature tensile elongation) of the vinyl chloride resin molded sheet.
[0137] <Odor intensity>
[0138] The obtained vinyl chloride resin molded sheet was placed in a 1 L glass bottle, which was sealed with a lid and heated by standing in an oven at 80° C. for 2 hours.
[0139] After heating, the glass bottle was taken out and the lid was opened. Seven evaluation panelists smelled the air inside the bottle and evaluated the smell in 0.5-level intervals according to the following criteria, from 0 to 5, where stronger smells indicate higher levels.
[0140] Level 0: No odor
[0141] Level 1: Barely perceptible odor
[0142] Level 2: A faint odor that can be identified as an odor
[0143] Level 3: Odor that can be easily perceived
[0144] Level 4: Strong odor
[0145] Level 5: Strong odor
[0146] Among the levels of the judgment results of 7 people, the maximum value and the minimum value were removed, and the average value was taken, and the obtained value was used as the odor intensity.
[0147] (Example 1)
[0148] <Preparation of vinyl chloride resin composition>
[0149] The components shown in Table 1 except for the plasticizer and the vinyl chloride resin particles as a release agent were added to a Henschel mixer and mixed. Then, when the temperature of the mixture rose to 80°C, all of the above plasticizer was added to dry it (meaning that the plasticizer was absorbed by the vinyl chloride resin particles as the vinyl chloride resin, and the above mixture became dry). Then, when the temperature of the dried mixture was cooled to 70°C or less, the vinyl chloride resin particles as a release agent were added to prepare a vinyl chloride resin composition.
[0150] <Formation of vinyl chloride resin molded article>
[0151] A vinyl chloride resin molded sheet having a size of 150 mm×200 mm×1 mm was prepared as follows.
[0152] Specifically, the vinyl chloride resin composition obtained above is sprinkled into a textured metal mold heated to a temperature of 250°C, and after being left for an arbitrary time to melt, the remaining vinyl chloride resin composition is shaken off. Then, the textured metal mold sprinkled with the vinyl chloride resin composition is left to stand in an oven set at a temperature of 200°C, and the textured metal mold is cooled with cooling water when 60 seconds have passed since the standing. When the temperature of the metal mold is cooled to 40°C, the vinyl chloride resin molded sheet, which is a vinyl chloride resin molded body, is demolded from the metal mold.
[0153] Then, the odor intensity and low-temperature tensile elongation of the obtained vinyl chloride resin molded sheet (size: 150 mm×200 mm×1 mm) were measured and evaluated according to the above-mentioned methods.
[0154] (Examples 2 to 5, Comparative Examples 1 to 3)
[0155] A vinyl chloride resin composition and a vinyl chloride resin molded article were prepared in the same manner as in Example 1 except that the amount of jasmine lactone used as a lactone compound was changed as shown in Table 1. Then, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.
[0156] [Table 1]
[0157]
[0158] 1) Shin-Daiichi Vinyl Chloride Co., Ltd., product name "ZEST 1700ZI" (vinyl chloride resin particles obtained by suspension polymerization, average degree of polymerization 1700, average particle size 130 μm)
[0159] 2) Shin-Daiichi Vinyl Chloride Co., Ltd., product name "ZEST PQLTX" (produced by emulsion polymerization, average degree of polymerization: 800, average particle size: 1.8 μm)
[0160] 3) Kao Corporation, product name "Trimex T-08" (tri-2-ethylhexyl trimellitate)
[0161] 4) ADK CIZER O-130S manufactured by ADK Co., Ltd.
[0162] 5) Kyowa Chemical Industry Co., Ltd., product name: "ALCAMAIZER (registered trademark) 5"
[0163] 6) Made by Mizusawa Chemical Industry Co., Ltd., product name: "MIZUKALIZER DS"
[0164] 7) Made by Showa Denko K.K., product name "Karenz DK-1"
[0165] 8) Made by Sakai Chemical Industry Co., Ltd., product name: "SAKAI SZ2000"
[0166] 9) ADK Co., Ltd., product name: ADK STAB LS-12
[0167] 10) Made by Japan Zeon Co., Ltd., product name: "Jasmine lactone"
[0168] 11) Dainichi Seika Industries, Ltd., product name: DA P 4720BLACK
[0169] As can be seen from Table 1, the vinyl chloride resin molded sheets formed using the vinyl chloride resin compositions of Examples 1 to 5 comprising a vinyl chloride resin, a plasticizer and a lactone compound having a predetermined structure, wherein the content of the lactone compound is within a predetermined range, suppress the generation of odor.
[0170] On the other hand, it is found that the vinyl chloride resin molded sheet formed using the vinyl chloride resin composition of Comparative Example 1 which does not contain the lactone compound having a predetermined structure cannot suppress the generation of odor.
[0171] Furthermore, it is understood that the vinyl chloride resin molded sheet formed using the vinyl chloride resin composition of Comparative Example 2, in which the content of the lactone compound having a predetermined structure does not satisfy the predetermined range, cannot sufficiently suppress the generation of odor.
[0172] Furthermore, it is found that the vinyl chloride resin molded sheet formed using the vinyl chloride resin composition of Comparative Example 3 in which the content of the lactone compound having a predetermined structure exceeds the predetermined range cannot sufficiently suppress the generation of odor.
[0173] Industrial Applicability
[0174] According to the present invention, there can be provided a vinyl chloride resin composition capable of forming a vinyl chloride resin molded article in which generation of odor is suppressed.
[0175] Furthermore, according to the present invention, it is possible to provide a vinyl chloride resin molded body in which generation of odor is suppressed.
[0176] Furthermore, according to the present invention, it is possible to provide a laminate having the vinyl chloride resin molded article and in which the generation of odor is suppressed.
Claims
1. A vinyl chloride resin composition, comprising: Vinyl chloride resin; Plasticizers; and A lactone compound represented by the following formula (I): In formula (I), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, a thiol group or a hydrocarbon group which may have a substituent, The content of the lactone compound is 0.005 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the vinyl chloride resin.
2. The vinyl chloride resin composition according to claim 1, in, The R 1 It represents a hydrocarbon group.
3. The vinyl chloride resin composition according to claim 2, in, The R 1 The hydrocarbon group has 1 to 20 carbon atoms.
4. The vinyl chloride resin composition according to claim 2, in, The R 1 The hydrocarbon group is a chain hydrocarbon group.
5. The vinyl chloride resin composition according to claim 2, in, The R 1 The hydrocarbon group is an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms.
6. The vinyl chloride resin composition according to claim 2, in, The R 1 The hydrocarbon group is an alkenyl group having 2 or more and 10 or less carbon atoms.
7. The vinyl chloride resin composition according to claim 1, in, The R 2 ~R 4 Both represent hydrogen atoms.
8. The vinyl chloride resin composition according to claim 1, in, The lactone compound contains jasmine lactone.
9. The vinyl chloride resin composition according to claim 1, in, The content of the plasticizer is 50 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the vinyl chloride resin.
10. The vinyl chloride resin composition according to claim 1, in, The vinyl chloride resin composition is used for powder molding.
11. The vinyl chloride resin composition according to claim 1, in, The vinyl chloride resin composition is used for powder slush molding. 12 . A vinyl chloride resin molded article obtained by molding the vinyl chloride resin composition according to claim 1 .
13. The vinyl chloride resin molded article according to claim 12, in, The vinyl chloride resin molded body is used for the surface skin of automobile instrument panels. 14 . A laminate comprising a foamed polyurethane molded product and the vinyl chloride resin molded product according to claim 12 .
15. The laminate according to claim 14, in, The laminate is used for automobile instrument panels.