Composition
By using a combination of metal compound cocatalyst and oxygen atom chelating agent in the manufacture of LDM products, the gel problem caused by catalyst residue is solved, ensuring the stability of dielectric properties and the reliability of the process.
Patent Information
- Application Number
- CN202380028528.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-05
AI Technical Summary
In the manufacture of Low Dielectric Macromonomers (LDM) products, the use of metal compounds as catalysts or cocatalysts leads to gel production, and the prior art is difficult to completely and reliably remove catalyst residues, affecting dielectric properties.
Using metal or semi-metal compounds as cocatalysts and using chelating agents with one or two oxygen atoms in the compositions to optimize the harmless and dielectric properties of the catalyst residues, through specific composition ratios and reaction conditions Inhibit gel production.
It effectively suppresses the generation of gel in the manufacturing of LDM products with required dielectric characteristics, and ensures that catalyst residue does not affect the dielectric constant and dielectric loss, improving the reliability of the process and product performance.
Smart Images

Figure BDA0005048948750000141 
Figure BDA0005048948750000142 
Figure BDA0005048948750000151
Abstract
Description
Technical Field
[0001] The present invention relates to compositions and methods of making the same. Background Art
[0002] As communication frequencies develop towards high frequency bands above the gigahertz band, the demand for insulating materials with low dielectric properties has also increased. This is because it is known that transmission loss is roughly equal to the sum of conductor loss and dielectric loss proportional to the dielectric loss tangent. However, existing materials such as epoxy resins have difficulty in achieving sufficiently low dielectric constants and dielectric losses. Therefore, a new monomer called LDM (Low Dielectric Macromonomers) was explored as a raw material.
[0003] For example, Patent Document 1 discloses, as one type of LDM, a curable composition comprising a predetermined olefin-aromatic vinyl compound-aromatic polyene copolymer and a predetermined additional resin, which can further reduce the dielectric constant and dielectric loss.
[0004] As described in Patent Document 1, when synthesizing LDM products, compounds containing metals or semimetals such as zirconium, hafnium, aluminum, and boron are used as catalysts or promoters. Such catalysts and promoters are usually not removed and remain in the final product.
[0005] On the other hand, it is known that if aluminum residues are present in an olefin polymerization solution, fish eyes will be generated in the obtained film. Therefore, an aluminum scavenger is included to suppress the generation of fish eyes (Patent Document 2).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2021 / 112088
[0009] Patent Document 2: Japanese Patent Application Publication No. 2000-001577 Summary of the invention
[0010] Problems to be solved by the invention
[0011] When manufacturing LDM products, if a conventional metal compound is used as a catalyst or a co-catalyst, there is a problem that a gel is generated when the composition obtained in a state containing the catalyst residue is exposed to the atmosphere. However, even if a conventional metal scavenger is used to address this problem, there is still the next problem that the dielectric constant and dielectric loss are adversely affected.
[0012] In addition, there is a problem that the process of removing the catalyst and promoter residues is complicated and difficult to remove completely and reliably.
[0013] Therefore, the conventional technology has a new problem that it is difficult to suppress the generation of gel in the production of LDM products that require dielectric properties.
[0014] Means for solving problems
[0015] In order to solve the above-mentioned problems, the present invention can provide the following aspects.
[0016] Method 1.
[0017] The composition is characterized in that it comprises:
[0018] (A) a curable hydrocarbon resin;
[0019] (C) a co-catalyst which is a metal compound or a semi-metal compound; and
[0020] (D) a chelating agent having one or two oxygen atoms in one molecule,
[0021] The amount of the component (D) is 2 mol or more per 1 mol of the component (C) contained in the composition.
[0022] Method 2.
[0023] The composition according to embodiment 1, wherein the component (A) comprises an olefin-aromatic vinyl compound-aromatic polyene copolymer.
[0024] Method 3.
[0025] The composition according to embodiment 2, wherein the component (A) satisfies the following conditions (1) to (4).
[0026] (1) The number average molecular weight of the copolymer is 500 to 100,000.
[0027] (2) The aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass to 70% by mass.
[0028] (3) The aromatic polyene monomer unit is one or more selected from polyenes having a carbon number of 5 to 20 and having a plurality of vinyl and / or vinylidene groups in the molecule, and the content of the vinyl and / or vinylidene groups derived from the aromatic polyene monomer unit is 1.5 to less than 20 in terms of number average molecular weight.
[0029] (4) The olefin monomer units are one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units and aromatic polyene monomer units is 100% by mass.
[0030] Method 4.
[0031] The composition according to any one of aspects 1 to 3, further comprising (B) a resin component containing one or more selected from the group consisting of thermoplastic hydrocarbon elastomers and thermoplastic conjugated diene polymers.
[0032] Method 5.
[0033] The composition according to any one of aspects 1 to 4, wherein the amount of the component (D) is 0.5 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the component (A).
[0034] Method 6.
[0035] The composition according to any one of Embodiments 1 to 5, further comprising (E) a catalyst, wherein the catalyst is a metal compound or a semi-metal compound.
[0036] Method 7.
[0037] The composition according to Embodiment 6, wherein the amount of the component (D) is 100 mol or more per 1 mol of the component (E) contained in the composition.
[0038] Method 8.
[0039] The composition according to any one of Embodiments 1 to 7, wherein the component (D) does not contain a nitrogen atom in the molecule.
[0040] Method 9.
[0041] The composition according to any one of Embodiments 1 to 8, wherein the component (D) contains one or more selected from the group consisting of 4-tert-butylcatechol and acetylacetone.
[0042] Method 10.
[0043] A cured product, which is a cured product of the composition according to any one of Embodiments 1 to 9.
[0044] Method 11.
[0045] A laminate comprising a metal foil and a layer containing the composition according to any one of aspects 1 to 9.
[0046] Method 12.
[0047] A single-layer CCL, a multi-layer CCL, a single-layer FCCL or a multi-layer FCCL substrate, comprising the cured body described in embodiment 10.
[0048] Method 13.
[0049] A solution comprising the composition according to any one of aspects 1 to 9 and a solvent for dissolving the composition.
[0050] Effects of the Invention
[0051] The composition according to the present invention exhibits an effect of suppressing the generation of gel in the production process of LDM products requiring dielectric properties. DETAILED DESCRIPTION
[0052] In this specification, the concept of sheet also includes film. In addition, in this specification, even if it is recorded as film, it also includes the concept of sheet. In this specification, the so-called composition includes the concept of varnish. That is, the composition, especially the liquid composition in the composition, is recorded as varnish. The order of each process included in the method disclosed in this specification can also be freely changed in time series as long as it can exert its effect. Unless otherwise specified, the numerical range in this specification includes its lower limit and upper limit.
[0053] First, the composition of the present invention is characterized in that it contains: a metal compound or a semi-metal compound as a co-catalyst as a (C) component; and a chelating agent having one or two oxygen atoms in one molecule as a (D) component at a predetermined ratio. The amount of the (D) component relative to 1 mol of the (C) component contained in the composition is 2 mol or more, preferably 2 mol or more and 10 mol or less, and more preferably 2 mol or more and 7 mol or less. If the amount of the (D) component relative to 1 mol of the (C) component contained in the composition is less than 2 mol, the following problems may occur: gelation occurs when the composition is exposed to the atmosphere; or the viscosity increases when water is added.
[0054] The component (C) is a co-catalyst that can be used in a catalytic amount in the polymerization of the component (A), i.e., the curable hydrocarbon resin (hereinafter sometimes simply referred to as "resin"). The component (C) may contain, for example, one or more of any aluminum compound or boron compound.
[0055] As examples of aluminum compounds, organic aluminum compounds can be cited. As organic aluminum compounds, for example, methylaluminoxane (also called methylalumoxane or MAO), modified methylaluminoxane (also called modified MAO, MMAO), solid polymethylaluminoxane (also called SMAO), etc. can be cited. These are commercially available from Tosoh Corporation as trade names TMAO-312, TMAO-211, TMAO-212, MMAO-3A, TMAO-341, and solid MAO. In addition, alkyl aluminum compounds such as triisobutyl aluminum and triethyl aluminum can also be cited.
[0056] Examples of the boron compound include organic boron compounds, such as boric acid, boric acid esters, boron trifluoride alkyl ethers, and boron trifluoride phenol.
[0057] Examples of the component (C) (and the component (E) described below) include those described in European Patent Application Publication No. 0872492A2, Japanese Patent Application Publication No. 11-130808, Japanese Patent Application Publication No. 9-309925, International Publication No. 00 / 20426, European Patent Application Publication No. 0985689A2, and Japanese Patent Application Publication No. 6-184179.
[0058] The amount of component (C) is preferably in the range of 0.01 to 10 parts by mass, more preferably in the range of 0.1 to 1 part by mass, relative to 100 parts by mass of component (A). It should be noted that in this specification, when component (A) is included, component (A) and component (B) are sometimes collectively referred to as a "polymerization system".
[0059] (D) component is a chelating agent having one or two oxygen atoms in one molecule, preferably containing no nitrogen atom in the molecule. If there are three or more oxygen atoms in each molecule, the problem of dielectric properties deterioration in the cured body of the composition will occur. (D) component coordinates with (C) component which becomes catalyst residue after playing the role of catalyst or co-catalyst, and plays a harmless effect. In addition, for (E) component described later, (D) component can also coordinate with it to play a harmless effect.
[0060] Although it is not intended to be bound by a particular theory, it is speculated that the chelating agent contains a plurality of groups having oxygen atoms (preferably hydroxyl groups, carbonyl groups, etc. that do not have nitrogen atoms), thereby effectively coordinating with the (C) component dissolved in the polymerization system and being fully detoxified. In addition, the (D) component preferably does not have an ester structure in the molecule.
[0061] Relative to 100 parts by mass of component (A), the amount of component (D) is preferably 0.5 parts by mass or more, more preferably 0.6 parts by mass or more, more preferably 0.5 parts by mass or more or 0.6 parts by mass or more and 10 parts by mass or less, and further preferably 0.6 parts by mass or more and 7 parts by mass or less. When the amount of component (D) is within the preferred range, the following effects can be obtained: the catalyst residue can be fully rendered harmless and the dielectric properties of the composition are not easily adversely affected. When the amount of component (D) is within the preferred range, the following effects can be obtained: the chelating agent is fully diffused in the resin component, and it is easy to suppress the generation of gel when exposed to the atmosphere, and it is also easy to suppress the viscosity increase when water is added.
[0062] (A) component can be any curable hydrocarbon resin, having a functional group that can be (heat) cured in the presence of heat or a free radical polymerization initiator. Through the presence of (A) component, the cured body of the present composition can meet the heat resistance required as an electrical insulating material. As a functional group, if it is a functional group that can be cured by heat or free radicals, it is not limited, preferably one or more of the group consisting of vinyl, vinylidene, and allyl. For example, as such a (A) component, it can be a multifunctional vinyl aromatic copolymer obtained by a cationic polymerization reaction described in International Publication No. 2018 / 181842 and No. 2017 / 115813, or a polyphenylene ether resin with a functional group, such as SA-9000 of SABIC, OPE-2St of Mitsubishi Gas Chemical, or a polyether (ketone) with a functional group, or a polymer or copolymer with a 1,2-polybutadiene structure, such as the trade name "Ricon" of CrayValley. In addition, materials such as olefin-aromatic vinyl compound-aromatic polyene copolymers obtained by single-site coordination polymerization can be cited. They can be one or a composition comprising multiple types. As component (A), it is most preferred to include a multifunctional vinyl aromatic copolymer or an olefin-aromatic vinyl compound-aromatic polyene copolymer whose constituents are substantially carbon atoms and hydrogen atoms.
[0063] The composition according to a preferred embodiment of the present invention comprises, as component (A), an olefin-aromatic vinyl compound-aromatic polyene copolymer (hereinafter sometimes referred to as "copolymer"). The copolymer is characterized in that it is obtained by copolymerizing monomers of olefin, aromatic vinyl compound and aromatic polyene through a single-site coordination polymerization reaction promoted by component (C).
[0064] The so-called olefin monomer is one or more selected from alpha olefins with a carbon number of 2 or more and 20 or less and cyclic olefins with a carbon number of 5 or more and 20 or less, and refers to a compound that is substantially free of oxygen, nitrogen, and halogen and is composed of carbon and hydrogen. As alpha olefins with a carbon number of 2 or more and 20 or less, for example, ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, 3,5,5-trimethyl-1-hexene, etc. can be exemplified. As cyclic olefins with a carbon number of 5 or more and 20 or less, norbornene and cyclopentene can be exemplified. As olefins, it is preferred to use a combination of alpha olefins other than ethylene and cyclic olefins, or ethylene alone. When the mass ratio of ethylene alone or the alpha olefin component / ethylene component other than the ethylene contained is preferably less than 1 / 7, and more preferably less than 1 / 10, it is preferred that the peel strength of the obtained solidified body and copper foil and copper wiring can be improved. The content of the α-olefin monomer component other than ethylene in the copolymer is more preferably 6% by mass or less, and most preferably 4% by mass or less, or the olefin is ethylene alone. The glass transition temperature of the cured product of the copolymer described below can be adjusted by the type and content of the olefin.
[0065] When the total of olefin monomer units, aromatic vinyl compound monomer units and aromatic polyene monomer units is set to 100% by mass, the content of olefin monomer units in this copolymer is preferably 20% by mass or more, more preferably 25% by mass or more, and most preferably 30% by mass or more. When the content of olefin monomer units is 20% by mass or more, the toughness (elongation) and impact resistance of the finally obtained solidified body are improved, and the rupture of the solidified body in the midway of curing and the rupture of the solidified body in the thermal cycle test are not easy to occur. In this copolymer, the content of olefin monomer units is preferably 90% by mass or less.
[0066] The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and examples thereof include styrene, p-methylstyrene, p-isobutylstyrene, various vinylnaphthalenes, and various vinylanthracenes.
[0067] The content of the aromatic vinyl compound monomer unit included in this copolymer can be 0 mass % or more and 70 mass % or less, preferably 10 mass % or more and 60 mass % or less. When the content of the aromatic vinyl compound monomer unit is 70 mass % or less, the glass transition temperature of the cured product of the resin composition finally obtained is lower than near room temperature, and the toughness and elongation at low temperatures can be improved, so it is preferred. When the content of the aromatic vinyl compound monomer unit is 10 mass % or more, the following effects can be obtained: the aromaticity of this copolymer is improved, the affinity with flame retardants and fillers becomes good, the exudation of flame retardants can be avoided, and the filling property of fillers can be improved. In addition, when the content of the aromatic vinyl compound monomer unit is 10 mass % or more, a cured product with a high peel strength from copper foil and copper wiring can also be obtained.
[0068] As an aromatic polyene monomer, it can be a polyene with a carbon number of 5 or more and 20 or less having multiple vinyl and / or vinylidene groups in its molecule, preferably various divinylbenzenes at ortho, meta, and para positions or mixtures thereof, divinylnaphthalene, divinylanthracene, p-2-propylene styrene, p-3-butylene styrene, etc. having an aromatic vinyl structure and substantially free of oxygen, nitrogen, and halogen and composed of carbon and hydrogen. In addition, bifunctional aromatic vinyl compounds such as 1,2-bis(vinylphenyl)ethane (abbreviated as: BVPE) described in Japanese Patent Publication No. 2004-087639 can also be used. Among them, various divinylbenzenes at ortho, meta, and para positions, or mixtures thereof are preferably used, and a mixture of meta and para divinylbenzenes can be used most preferably. In this specification, these divinylbenzenes are sometimes collectively described as divinylbenzenes. When divinylbenzenes are used as aromatic polyenes, the curing efficiency is high and the curing is easy during the curing treatment, so it is preferred.
[0069] As each monomer of the above olefin, aromatic vinyl compound, aromatic polyene, it is also possible to include in addition: olefin containing polar groups such as oxygen atoms, nitrogen atoms, etc.; aromatic vinyl compounds containing oxygen atoms, nitrogen atoms, etc.; or aromatic polyene containing oxygen atoms, nitrogen atoms, etc. The total mass of these monomers containing polar groups is preferably less than 10% by mass of the total mass of this composition, more preferably less than 3% by mass, most preferably without the monomer containing polar groups. By making the ratio of the total mass of the monomer containing polar groups less than 10% by mass, the dielectric properties (low dielectric constant, low dielectric loss) of the cured body obtained by curing this composition can be improved.
[0070] Examples of the copolymer not containing an aromatic vinyl compound monomer unit (olefin-aromatic polyene copolymer) include ethylene-divinylbenzene copolymer, ethylene-propylene-divinylbenzene copolymer, ethylene-1-butene-divinylbenzene copolymer, ethylene-1-hexene-divinylbenzene copolymer, ethylene-1-octene-divinylbenzene copolymer, and the like.
[0071] Examples of the copolymer containing an aromatic vinyl compound monomer unit (olefin-aromatic vinyl compound-aromatic polyene copolymer) include ethylene-styrene-divinylbenzene copolymer, ethylene-propylene-styrene-divinylbenzene copolymer, ethylene-1-hexene-styrene-divinylbenzene copolymer, ethylene-1-octene-styrene-divinylbenzene copolymer, and the like.
[0072] The number average molecular weight (Mn) of the copolymer may be 500 to 100,000, preferably 500 to 50,000, more preferably 500 to 20,000, and more preferably 500 to 10,000. When Mn is 100,000 or less, a suitable viscosity for a varnish can be obtained, and the effect of improving the workability when using the composition can be obtained.
[0073] The weight average molecular weight (Mw) of the copolymer may preferably be 10,000 to 200,000, more preferably 20,000 to 200,000, and more preferably 20,000 to 150,000. Preferably, the value Mw / Mn obtained by dividing the weight average molecular weight by the number average molecular weight may be in the range of 2.0≤Mw / Mn≤13.0, more preferably 2.0≤Mw / Mn≤12.0, and more preferably 2.0≤Mw / Mn≤10.0.
[0074] The number average molecular weight and weight average molecular weight in this specification refer to values measured as molecular weights converted to standard polystyrene by high temperature gel permeation chromatography (HT-GPC). The measurement conditions of the HT-GPC method in this specification are as follows.
[0075] Measuring device: HLC-8321GPC / HT manufactured by Tosoh Corporation
[0076] Chromatographic column: TSKgel GMHHR-H(20)HT, 3 roots
[0077] Column temperature: 140°C
[0078] Detector: RI
[0079] Solvent: o-dichlorobenzene
[0080] Liquid delivery flow: 1.0ml / min
[0081] Sample concentration: 0.2wt / Vol%
[0082] Sample injection volume: 100 μL
[0083] In the present copolymer, the content of vinyl and / or vinylidene groups (preferably vinyl groups) derived from aromatic polyene units is 1.5 or more and less than 20, preferably 2 or more and less than 7, in terms of number average molecular weight. When the content of the vinyl and / or vinylidene groups is 1.5 or more, the crosslinking efficiency is high, and a cured product with a sufficient crosslinking density can be obtained. The vinyl content derived from aromatic polyene units (divinylbenzene units) in the copolymer in terms of number average molecular weight can be obtained by dividing the number average molecular weight (Mn) calculated by the GPC (gel permeation chromatography) method known to those skilled in the art by the standard polystyrene conversion and the crosslinking density by the number average molecular weight (Mn). 1 The vinyl content derived from the aromatic polyene unit obtained by H-NMR measurement is compared. 1 Comparison of the intensity of each peak area obtained by H-NMR measurement shows that the vinyl content derived from the aromatic polyene unit (divinylbenzene unit) in the copolymer is 3.2% by mass, and the number average molecular weight based on standard polystyrene conversion measured by GPC is 2100. The molecular weight of the vinyl derived from the aromatic polyene unit in the number average molecular weight is the product of these, i.e., 67.5, which is divided by the formula weight of the vinyl, 27, to obtain 2.5. That is, the vinyl content derived from the aromatic polyene unit in the copolymer in terms of number average molecular weight is 2.5. 1 The attribution of the peaks obtained by H-NMR measurement is known from the literature. 1 A method for determining the composition of a copolymer by comparing the peak areas obtained by H-NMR measurement is also known. In addition, in this specification, the content of divinylbenzene units in a copolymer is determined by the peak intensity (based on the peak intensity of the vinyl group derived from the divinylbenzene unit) of the divinylbenzene unit. 1 That is, based on the content of vinyl groups derived from divinylbenzene units, one vinyl group is regarded as one divinylbenzene unit derived from the copolymer, and the content of divinylbenzene units is determined.
[0084] <Curing polyether resin>
[0085] (A) component can include curable polyphenylene ether, curable polyether resins such as polyether. As such polyphenylene ether, commercially known polyphenylene ether can be used. The number average molecular weight of polyphenylene ether is arbitrary. Considering the molding processability of the composition, the number average molecular weight is preferably less than 10,000, and most preferably less than 5,000. The number average molecular weight is preferably more than 500, and most preferably more than 1,000. In addition, when added for the purpose of curing of the present composition, the molecular end is preferably modified, and / or preferably has multiple functional groups in one molecule. As functional groups, functional groups such as allyl, vinyl, and epoxy can be cited, and free radical polymerizable functional groups are most preferably free radical polymerizable functional groups, particularly preferably vinyl, and more preferably one or more of the group consisting of (meth) acrylic groups and aromatic vinyl groups. That is, in the present composition, bifunctional polyphenylene ethers whose molecular chains are modified by free radical polymerizable functional groups at both ends are particularly preferred. As such polyphenylene ether, Noryl (trademark) SA9000 of SABIC Company can be cited, and it is particularly preferred to use a bifunctional polyphenylene ether oligomer (OPE-2St) manufactured by Mitsubishi Gas Chemical Company. The amount of the polyphenylene ether used in the present composition is preferably 1 to 200 parts by mass, and more preferably 10 to 100 parts by mass, relative to 100 parts by mass of the copolymer. In addition, as a polyether-based resin, an aromatic polyether (ELPAC HC-F series) of JSR Company can also be used. The amount of polyether-based resins such as polyphenylene ether in the present composition is preferably 1 to 200 parts by mass, and more preferably 1 to 100 parts by mass, relative to 100 parts by mass of component (A).
[0086] <Curing aromatic polyene resin>
[0087] The curable aromatic polyene resin that component (A) may contain includes a divinylbenzene-based reactive multibranched copolymer (PDV) manufactured by NIPPON STEEL Chemical & Material Co., Ltd. Such PDV is described in, for example, the document "Synthesis of multifunctional aromatic vinyl copolymers and development of novel IPN-type low dielectric loss materials using the same" (Masanao Kawabe et al., Journal of Japan Institute of Electronics Packaging p125, Vol. 12 No. 2 (2009)). In addition, as aromatic polyene resins, aromatic polyene polymer resins having the above-mentioned aromatic polyene monomers as main constituent units may also be mentioned.
[0088] The present composition may further contain, as component (B), a resin component containing one or more selected from the group consisting of thermoplastic hydrocarbon elastomers and thermoplastic conjugated diene polymers. Component (B) is different from component (A) in definition and does not include component (A).
[0089] <Thermoplastic hydrocarbon elastomer>
[0090] The amount of thermoplastic hydrocarbon elastomer that component (B) may contain is preferably 1 to 500 parts by mass, more preferably 1 to 200 parts by mass, relative to 100 parts by mass of the copolymer. Suitable hydrocarbon elastomers include one or more elastomers selected from ethylene-based and propylene-based elastomers, conjugated diene polymers, aromatic vinyl compound-conjugated diene block copolymers or random copolymers, and their hydrogenates (hydrogenated products). The number average molecular weight of the hydrocarbon elastomer is 1,000 or more, more preferably 2,000 or more, and most preferably 30,000 or more. The number average molecular weight of the hydrocarbon elastomer is preferably 80,000 or less, more preferably 60,000 or less.
[0091] As the ethylene-based elastomer that may be included in the component (B), there may be mentioned ethylene-α-olefin copolymers such as ethylene-octene copolymers and ethylene-1-hexene copolymers, EPR, and EPDM. As the propylene-based elastomer, there may be mentioned propylene-α-olefin copolymers such as atactic polypropylene, polypropylene with low stereoregularity, and propylene-1-butene copolymers.
[0092] As the thermoplastic conjugated diene polymer that can be included as component (B), polybutadiene and 1,2-polybutadiene can be cited. As block copolymers or random copolymers of aromatic vinyl compounds-conjugated dienes, and their hydrogenated products (hydrogenated products), SBS, SIS, SEBS, SEPS, SEEPS, SEEBS, etc. can be exemplified. 1,2-polybutadiene that can be preferably used can be obtained from JSR products, for example, liquid polybutadiene: product names B-1000, 2000, 3000 can also be obtained from Nippon Soda Co., Ltd. In addition, as a copolymer containing a 1,2-polybutadiene structure that can be preferably used, "Ricon100" of TOTAL CRAY VALLEY can be exemplified. When one or more resins selected from these hydrocarbon elastomers are in a liquid state (having a viscosity of approximately 300,000 mPa·S or less) particularly at room temperature (25°C), their usage amount is preferably in the range of 1 to 30 parts by mass, particularly preferably in the range of 1 to 20 parts by mass, relative to 100 parts by mass of the copolymer, from the viewpoint of the handleability and molding processability (handleability as a thermoplastic resin) of the present composition in an uncured state.
[0093] The present composition may further contain any additional components exemplified below unless the effects thereof are impaired.
[0094] <Curing agent>
[0095] As a curing agent that can be used in the present composition, a known curing agent that can be used in the polymerization or curing of aromatic polyenes and aromatic vinyl compounds in the past can be used. Such curing agents can exemplify free radical polymerization initiators, cationic polymerization initiators, and anionic polymerization initiators, and free radical polymerization initiators can be preferably used. Preferably, organic peroxides (peroxides), azo polymerization initiators, etc. can be freely selected according to the purpose and conditions. The product catalog that records organic peroxides can be downloaded from the homepage of NOF Corporation, such as https: / / www.nof.co.jp / business / chemical / chemical-product01. In addition, organic peroxides are also recorded in the product catalogs of Fujifilm and Koho Pure Chemical Industries, Ltd. and Tokyo Chemical Industry Co., Ltd. Curing agents can be obtained from these companies. In addition, known photopolymerization initiators using light, ultraviolet rays, and radiation can also be used as curing agents. As a curing agent using a photopolymerization initiator, a photoradical polymerization initiator, a photocationic polymerization initiator, or a photoanionic polymerization initiator can be cited. Such a photopolymerization initiator can be obtained from Tokyo Chemical Industry Co., Ltd., for example. In addition, curing can also be performed by radiation or electron beam itself. In addition, crosslinking and curing can also be performed by thermal polymerization of the included raw materials without containing a curing agent.
[0096] The amount of the curing agent used is not particularly limited, and is generally preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the composition. The composition preferably does not include a curing agent or a solvent. When using a curing agent such as a peroxide (peroxide) or an azo polymerization initiator, the curing treatment is performed at an appropriate temperature and time in consideration of its half-life. The conditions in this case are optional depending on the curing agent, and generally, a temperature range of about 50°C to 200°C is suitable.
[0097] <Single body>
[0098] The amount of monomer that this composition can contain is arbitrary, preferably 10 parts by mass or less relative to 100 parts by mass of the copolymer. It should be noted that this composition may be substantially free of monomer. When the monomer is 10 parts by mass or less, the uncured composition will not have a viscous nature, and the molding process as a thermoplastic resin becomes easy. In addition, when the content of the easily volatile monomer amount is below a certain amount, the odor will not be a problem in the uncured stage. In the case where a solvent is added to the composition and the product form is varnish-like, there is the following problem: when using, the monomer will disappear along with the evaporation of the solvent (solvent), and the substantial content of the monomer is easily reduced. In addition, when the product form is an uncured sheet, if a certain amount of monomer is included, it is not easy to cause a change in the monomer content during storage. The molecular weight of the monomer that can be preferably used in this composition is preferably less than 1000, and more preferably less than 500. The monomer that can be preferably used in the composition of the present invention is an aromatic vinyl compound monomer, an aromatic polyene monomer, and / or a polar monomer. As the monomer, it is preferably a monomer that can be polymerized by a free radical polymerization initiator, more preferably one or more of the group consisting of the aforementioned aromatic vinyl compound and aromatic polyene. In addition, BVPE (1,2-bis(vinylphenyl)ethane) recorded in Japanese Patent Publication No. 2003-212941 can also be preferably used. From the viewpoint of improving the mechanical strength (elastic modulus) of the cured body at high temperatures, the aromatic polyene is preferably 1 mass part or more and 30 mass parts or less relative to 100 mass parts of the copolymer. In addition, in order to impart the adhesion to other materials required as an insulating material or to increase the crosslinking density, a relatively small amount of polar monomers can be used. As the above-mentioned polar monomer, various maleimides, bismaleimides, maleic anhydride, glycidyl (meth) acrylate, triallyl isocyanurate, tri(meth) acrylate isocyanurate, trimethylolpropane tri(meth) acrylate, etc. can be cited. Usable maleimides and bismaleimides are described in, for example, International Publication No. 2016 / 114287 and Japanese Patent Application Publication No. 2008-291227, and can be purchased from, for example, Yamato Kasei Kogyo Co., Ltd. and Designer molecules Inc. From the viewpoints of solubility in organic solvents, high-frequency characteristics, high adhesion to conductors, prepreg formability, etc., these maleimide group-containing compounds are preferably bismaleimides.
[0099] As the bismaleimides, bismaleimides represented by the following formula (B-1) are preferred.
[0100] Formula (B-1)
[0101] [Chemical formula 1]
[0102]
[0103] In formula (B-1), R represents an alkylene group having 5 or more carbon atoms, and L represents a single bond or a divalent linking group. R and L may each independently have a substituent. In addition, the maleimide represented by formula (B-1) is preferably represented by the following formula (B-2).
[0104] Formula (B-2)
[0105] [Chemical formula 2]
[0106]
[0107] In formula (B-2), R' independently represents an alkylene group having 5 or more carbon atoms which may have a substituent, and A independently represents an alkylene group having 5 or more carbon atoms which may have a substituent or a divalent group having an aromatic ring which may have a substituent. n represents an integer of 1 to 10.
[0108] Examples of maleimides represented by formula (B-2) include compounds represented by the following formula (B-3): wherein n represents an integer of 1 to 10. Examples of compounds represented by formula (B-3) include BMI-1500 manufactured by Designer Molecules Inc. (n average value = 1.3).
[0109] Formula (B-3)
[0110] [Chemical formula 3]
[0111]
[0112] Bismaleimides can be used as polyaminobismaleimide compounds. Polyaminobismaleimide compounds are obtained, for example, by subjecting a compound having two maleimide groups at the end to a Michael addition reaction with an aromatic diamine compound having two primary amino groups in the molecule. In the case of wanting to obtain a high crosslinking efficiency with a small amount of addition, it is preferred to use a polar monomer having a multifunctional group of more than two functional groups, and examples thereof include bismaleimides, triallyl isocyanurate (TAIC), and trimethylolpropane tri(meth)acrylate. The amount of polar monomer that the composition may contain is in the range of 0.1 to 10 parts by mass, preferably in the range of 0.1 to 5 parts by mass, relative to 100 parts by mass of the copolymer. By using less than 10 parts by mass, the dielectric constant and dielectric loss tangent of the obtained cured body can be reduced.
[0113] The present composition may further comprise a catalyst, which is any metal compound or semi-metal compound, which can be used in a catalytic amount in the polymerization of the component (A) as the component (E). The component (E) is distinguished from the component (C) by definition by excluding the component (C). The component (E) may preferably comprise one or more of a zirconium compound or a hafnium compound.
[0114] Examples of the zirconium compound or hafnium compound include compounds represented by the following general formula (I).
[0115] [Chemical formula 4]
[0116]
[0117] M in the above formula is an element selected from zirconium or hafnium.
[0118] Cp1 and Cp2 are cyclopentadienyl groups having no substituent or cyclopentadienyl groups having one or two alkyl substituents having no cyclic structure (preferably having 1 to 3 carbon atoms). Cp1 and Cp2 may be the same or different from each other. In addition, one of Cp1 and Cp2 may be indenyl groups having no substituent or indenyl groups having one or two alkyl substituents having no cyclic structure (preferably having 1 to 3 carbon atoms).
[0119] Y is an element having a bond with Cp1 and Cp2 and selected from carbon, silicon, germanium or boron having a hydrogen atom or a substituent. The substituents (preferably alkyl groups or phenyl groups, etc.) may be different or the same and may have a cyclic structure (cyclohexyl structure, etc.).
[0120] Each X is independently selected from the group consisting of hydrogen, halogen, alkyl and aryl groups, or two Xs are bonded to form a diene group.
[0121] Examples of such zirconium compounds or hafnium compounds include dimethylmethylenebiscyclopentadienylzirconium dichloride, diphenylmethylenebiscyclopentadienylzirconium dichloride, dimethylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride, and diphenylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride.
[0122] The amount of the component (D) relative to 1 mol of the component (E) contained in the composition may be 100 mol or more, preferably 100 mol or more and 500 mol or less. In addition, the amount of the component (E) relative to 100 parts by mass of the component (A) may be in the range of 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass.
[0123] <Solvent (solvent)>
[0124] For this composition, an appropriate solvent can be added as needed. The solvent is used to adjust the viscosity and fluidity of the composition. As a solvent, a volatile solvent is preferred, for example, cyclohexane, toluene, ethylbenzene, acetone, isopropanol, etc. can be used. In addition, as far as its usage is concerned, from the perspective of the molding processability and operation of the composition before curing as a thermoplastic resin, it is preferably 10 parts by mass or less relative to 100 parts by mass of the copolymer. In addition, from the perspective of removal during and after curing, it is more preferred that no solvent is substantially used. Substantially no use means preferably 5 parts by mass or less, more preferably 1 part by mass or less, and most preferably 0 parts by mass. In addition, when used as a varnish, it is preferred to add an appropriate solvent to this composition. The solvent is used to adjust the viscosity and fluidity of the composition as a varnish. As a solvent, when the boiling point at atmospheric pressure is high, that is, when the volatility is low, the thickness of the film obtained by coating becomes uniform, so a solvent with a boiling point above a certain degree is preferred. The preferred boiling point is about 100°C or more at atmospheric pressure, preferably 130°C or more and 300°C or less. As a solvent suitable for such a varnish, toluene, xylene, mesitylene, ethylbenzene, limonene, ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, etc. can be used. In addition, the amount used is preferably in the range of 10 to 2000 parts by mass relative to 100 parts by mass of the present composition.
[0125] The present composition may further include one or more selected from fillers, flame retardants, and surface modifiers. The present composition may become the matrix of a cured body. During curing, in order to make the filling property of other materials excellent, the present composition may include one or more selected from these fillers, flame retardants, and surface modifiers. In this way, even after curing, the cured body is easy to show impact resistance and toughness.
[0126] <Filling agent>
[0127] As the filler that this composition can contain, inorganic or organic fillers can be cited. These fillers are added in order to control the thermal expansion coefficient, control thermal conductivity, and realize low price, and their usage amount is arbitrary according to the purpose. This composition can especially contain a large amount of inorganic fillers, and relative to 100 parts by mass of copolymer, its usable amount can reach 2000 parts by mass at most. Especially when adding inorganic fillers, it is preferred to use known surface modifiers, such as silane coupling agents, etc. Especially in the case of one of the purposes of the present invention, i.e., with low dielectric constant, low dielectric loss excellent composition as the purpose, as inorganic fillers, preferably boron nitride (BN) and / or silicon dioxide, more preferably silicon dioxide. In silicon dioxide, preferably fused silica. From the viewpoint of low dielectric properties, if a large amount of addition is made, there is the possibility that the dielectric constant becomes especially high, so it is preferred to use a filler that is less than 500 parts by mass, more preferably less than 400 parts by mass relative to 100 parts by mass of copolymer. Furthermore, in order to improve and enhance low dielectric properties (low dielectric constant, low dielectric loss tangent), a hollow filler or a filler having a shape with many voids may be added.
[0128] In addition, organic fillers such as high molecular weight or ultra high molecular weight polyethylene can also be used to replace inorganic fillers. From the viewpoint of heat resistance, organic fillers are preferably self-crosslinked, preferably used in the state of particulate or powder. These organic fillers can suppress the increase of dielectric constant, dielectric loss tangent. Relative to 100 mass parts of copolymers, the usage amount of filler is most preferably more than 1 mass part and less than 400 mass parts.
[0129] On the other hand, by mixing and dispersing a high dielectric constant insulator filler having a dielectric constant of preferably 3 to 10,000, more preferably 5 to 10,000 at 1 GHz in the present composition, it is possible to produce an insulating solid body having a high dielectric constant insulating layer in which the increase of dielectric loss tangent (dielectric loss) is suppressed and the dielectric constant is preferably 3.1 to 20. By increasing the dielectric constant of the film formed by the insulating solid body, it is possible to achieve miniaturization of circuits and high capacitance of capacitors, which can contribute to miniaturization of high-frequency electrical components. High dielectric constant, low dielectric loss tangent insulating layers are suitable for capacitors, inductors for resonant circuits, filters, antennas and other uses. As the high dielectric constant insulator filler used in the present invention, inorganic fillers or metal particles subjected to insulation treatment can be cited. Specific examples are known high dielectric constant inorganic fillers such as barium titanate and strontium titanate, and other examples are specifically recorded in, for example, Japanese Patent Publication No. 2004-087639.
[0130] <Flame retardant>
[0131] As flame retardants that may be included in the present composition, from the viewpoint of maintaining a low dielectric constant and a low dielectric loss tangent, known organic phosphorus-based flame retardants such as phosphate esters or their condensates, known bromine-based flame retardants, and red phosphorus are used. Among phosphate esters, in particular, compounds having a plurality of xylene groups in the molecule are preferred from the viewpoint of flame retardancy and low dielectric loss tangent.
[0132] In addition, in addition to flame retardants, antimony compounds such as antimony trioxide, antimony tetroxide, antimony pentoxide, sodium antimonate, or nitrogen-containing compounds such as melamine, triallyl-1,3,5-triazine-2,3,4-(1H,3H,5H)-trione, 2,4,6-triallyloxy 1,3,5-triazine may be added as flame retardant aids. The total amount of these flame retardants and flame retardant aids is usually preferably 1 to 100 parts by mass relative to 100 parts by mass of the composition. In addition, 30 to 200 parts by mass of the aforementioned polyphenylene ether (PPE)-based resins with low dielectric constants and excellent flame retardancy may be added relative to 100 parts by mass of the flame retardant.
[0133] <Surface modifier>
[0134] In order to improve the adhesion with fillers, copper plates, and wiring, the present composition may further include various surface modifiers. The amount of the surface modifier used is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the present composition other than the surface modifier. As the surface modifier, various silane coupling agents, titanate coupling agents, etc. can be cited. Various silane coupling agents and titanate coupling agents can use one or more.
[0135] The present composition can also be made into a viscous liquid varnish according to its composition and mixing ratio. For example, by using a sufficient amount of solvent and / or by using a proper amount of liquid monomer, it can be made into a varnish. When used as a varnish, it is preferred to add a suitable solvent to the present composition. The solvent is used to adjust the viscosity and fluidity of the composition as a varnish. As a solvent, when the boiling point at atmospheric pressure is high, that is, when the volatility is low, it has the advantage that the thickness of the film obtained by coating becomes uniform, so a solvent with a boiling point above a certain degree is preferred. The preferred boiling point is about 100°C or more at atmospheric pressure, preferably 110°C or more and 300°C or less. As a solvent suitable for such a varnish, xylene, mesitylene, ethylbenzene, limonene, ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, etc. can be used. In addition, its usage amount is preferably in the range of 10 to 2000 parts by mass relative to 100 parts by mass of the present composition. Varnish-like compositions can also be made using a polymerization liquid containing the present copolymer obtained by polymerization. For example, the polymerization solution may be concentrated or the residual monomers may be removed. Alternatively, a solvent, other resin components, various additives, etc. may be added as necessary to adjust the component concentrations, solution viscosity, etc. for production.
[0136] The varnish can be applied or impregnated on a substrate, for example, and the solvent can be removed by drying, etc., thereby forming an uncured or semi-cured molded body. Usually, the molded body has a sheet, film, or tape form.
[0137] <Curing>
[0138] The curing of the present composition can be carried out by referring to the curing conditions (temperature, time, pressure) of the included curing agent and by known methods. When the curing agent used is a peroxide, the curing conditions can be determined by referring to the half-life temperature disclosed for each peroxide.
[0139] The composition can be used as various insulating materials for wiring (preferably for high-frequency signal wiring), such as covering layers, solder resists, buildup materials, interlayer insulating agents, bonding sheets, interlayer adhesives, and bump sheets for flip chip bonding machines. In addition, it can also be used as an electrical insulating layer or adhesive layer of a substrate or substrate such as a single-layer or multi-layer printed substrate, a flexible printed substrate, a CCL (copper clad laminate), or a FCCL (flexible copper clad laminate) substrate.
[0140] <Viscosity>
[0141] In this specification, the viscosity of the composition is obtained in accordance with JIS Z 8803:2011 when it is prepared as a 50 mass % toluene solution. The viscosity of the composition at 25°C is determined at a shear rate of 1 s -1 Under the condition of , it can be 100000 cP or less, preferably 10000 cP or less or 9000 cP or less, further preferably 8000 cP or less, more preferably 5000 cP or less. The lower limit of the viscosity is not particularly limited, for example, it can be 500 cP or more, preferably 1000 cP or more. By making the viscosity within such a range, the effect of improving the operability of the varnish can be obtained.
[0142] <Manufacturing method>
[0143] The composition containing the copolymer can be obtained by mixing the olefin monomer, the aromatic vinyl compound monomer and the aromatic polyene monomer in a suitable solvent to prepare a raw material solution, and subjecting the raw material solution to a single-site coordination polymerization reaction. In another embodiment, a process of polymerizing in a liquid monomer without using a solvent can also be adopted instead.
[0144] As the solvent that can be used, there can be mentioned saturated aliphatic or aromatic hydrocarbons such as pentane, hexane, heptane, cyclohexane, methylcyclohexane, benzene, toluene, ethylbenzene, xylene, mesitylene, limonene, chlorine-substituted benzene, chlorine-substituted toluene, dichloromethane, chloroform, or a single halogenated hydrocarbon or a mixed solvent. Preferably, a mixed alkane solvent, cyclohexane, toluene, ethylbenzene, etc. can be used as the solvent.
[0145] It should be noted that the copolymer can be produced even without using a chain transfer agent, but a chain transfer agent may be used to reduce the molecular weight. As such a chain transfer agent, a known chain transfer agent used together with a so-called single-site coordination polymerization catalyst may be used, for example, hydrogen, alkyl aluminums such as triisobutyl aluminum, 9-BBN described in Chung TC: Macromolecules, 26, 3467 (1993), etc.
[0146] The equipment capable of producing the present composition may be, for example, a single or multiple connected tank-type polymerization tank, a linear or annular single or multiple connected pipeline polymerization equipment, etc. The pipeline-shaped polymerization tank may have various known mixers such as a dynamic or static mixer, a static mixer with heat removal function, and various known coolers such as a cooler with a heat removal capillary. In addition, it may also have a batch prepolymerization tank. In addition, a gas phase polymerization process may also be adopted.
[0147] The polymerization temperature is preferably 0 to 200° C. When it is 0° C. or higher, the polymerization rate is fast, which is industrially advantageous. When it is 200° C. or lower, the effect of not decomposing the transition metal compound can be obtained. In addition, it is industrially preferably 30 to 160° C., and particularly preferably 50 to 160° C. The pressure during the polymerization is usually preferably 1 to 100 atmospheres, more preferably 1 to 30 atmospheres, and most preferably 1 to 10 atmospheres industrially.
[0148] When the copolymer is recovered from the reaction system after the polymerization is completed, any process can be used, and preferably, the steam stripping method and the crumb forming method, which are so-called methods for recovering raw rubber, can be used. In the laboratory, the method of precipitating the copolymer in a large amount of methanol, the so-called methanol precipitation method, is convenient. In addition, the copolymer can be removed from the polymerization solution by an evaporation method based on a rotary evaporator, a thin film evaporator, etc. without recovering the copolymer, and the solvent and the residual monomers can be removed in whole or in part, and diluted with a solvent, and can also be used as a varnish.
[0149] Example
[0150] [Table 1]
[0151]
[0152] [Table 2]
[0153] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Polymerization liquid Mass 100 100 100 100 100 100 Types of copolymer components P-1 P-1 P-1 P-1 P-2 P-3 Copolymer components in the polymerization solution Mass 18 18 18 1 8 16 17 The vinyl group of divinylbenzene in the copolymer Number average molecular weight 3.4 3.4 3.4 3.4 6.0 4.7 catalyst Mass 0.003 0.003 0.003 0.003 0.002 0.004 Catalyst Mass 0.081 0.081 0.081 0.081 0.082 0.079 Chelating agent 1 (TBC) Mass 0.216 Chelating agent 2 (Acac) Mass 0.432 0.216 0.108 0.192 0.204 Chelating agent 3 (AcacOEt) Mass Chelating agent 4 (TMEDA) Mass Chelating agent 5 (EDTA·4Na) Mass Chelating agent addition amount relative to copolymer ppm 12000 24000 12000 6000 12000 12000 (Mole number of chelating agent) / (Mole number of catalyst) 129.41 427.05 213.53 106.76 284.70 151.25 (Mole number of chelating agent) / (Mole number of co-catalyst) 2.552 8.423 4.211 2.106 3.698 4.078 Formation of gel when exposed to the atmosphere none none none none none none Viscosity increases due to the addition of water none none none none none none
[0154] [Table 3]
[0155]
[0156] [Table 4]
[0157] Example 1 Example 3 Example 5 Example 6 Comparative Example 1 Comparative Example 3 Comparative Example 7 Comparative Example 8 Copolymer components in LDM polymerization solution Mass 100 100 100 100 100 100 100 100 catalyst Mass 0.02 0.02 0.01 0.02 0.02 0.02 0.01 0.02 Catalyst Mass 0.45 0.45 0.455556 0.438889 0.45 0.45 0.455556 0.438889 Toluene Mass 60 60 60 60 60 60 60 60 Perhexyne 25B Mass 0.75 0.75 0.75 0.75 0.75 0.75 0.75 0.75 Chelating agent 1 (TBC) Mass 1.2 Chelating agent 2 (Acac) Mass 1.2 1.2 1.2 Chelating agent 3 (AcacOEt) Mass 1.2 Chelating agent 4 (TMEDA) Mass Chelating agent 5 (EDTA·4Na) Mass Chelating agent addition amount relative to copolymer ppm 12000 12000 12000 12000 12000 Storage modulus at 25℃ MPa 3.63 5.98 3.12 4.02 2.76 3.36 2.73 2.28 Dielectric constant 2.43 2.43 2.29 2.31 2.39 2.42 2.27 2.33 Dielectric loss tangent 0.0010 0.0010 0.0007 0.0007 0.0010 0.0014 0.0007 0.0007
[0158] In order to verify the generation of gel, an LDM polymerization solution was prepared according to the following steps. The production methods described in Japanese Patent Application Laid-Open No. 9-40709, International Publication No. 00 / 37517, Japanese Patent Application Laid-Open No. 2009-161743, and Japanese Patent Application Laid-Open No. 2010-280771 were used as references, dimethylmethylenebiscyclopentadienylzirconium dichloride was used as a catalyst, methylaluminoxane (MMAO-3A toluene solution manufactured by Tosoh Finechem Co., Ltd.) was used as a co-catalyst, cyclohexane was used as a solvent, styrene, divinylbenzene (a mixture of meta- and para-divinylbenzene), and ethylene were used as raw materials, and a 10L autoclave equipped with a stirrer and a heating and cooling jacket was used. The monomer amount, ratio, polymerization pressure, and polymerization temperature were appropriately changed to obtain copolymers of the compositions shown in Table 1. 1-Isopropanol was added to the obtained polymerization solution to obtain an LDM polymerization solution. Furthermore, the chelating agent shown in Tables 2 and 3 was introduced into the LDM polymerization liquid, and the mixture was stirred and subjected to the evaluation described later.
[0159] It should be noted that in Tables 2 and 3, the LDM polymer solution is set to 100 parts by mass, and the amount of the catalyst, co-catalyst and chelating agent added is expressed in terms of the added ratio. In addition, in Tables 2 and 3, when calculating the number of moles of MMAO, the molecular weight (58.02) is taken as the average. m (100.10) n , assuming m=n=1, the calculated value is 158.12.
[0160] The chelating agents used are as follows.
[0161] Chelating agent 1: TBC (4-tert-butylcatechol, molecular weight 165.2)
[0162] Chelating agent 2: Acac (acetylacetone, molecular weight 100.12)
[0163] Chelating agent 3: AcacOEt (ethyl acetoacetate, molecular weight 130.14)
[0164] Chelating agent 4: TMEDA (tetramethylethylenediamine, molecular weight 116.24)
[0165] Chelating agent 5: EDTA·4Na (tetrasodium ethylenediaminetetraacetate, molecular weight 380.17)
[0166] The obtained polymer (composition) was exposed to the air, and after 5 hours, the presence or absence of a gel was visually confirmed.
[0167] The viscosity of the resin solution containing the polymer obtained in each example and comparative example was measured in the following manner. The resin solution was concentrated using a rotary evaporator and diluted by adding toluene to a concentration of 50% by mass to prepare a measurement solution. The viscosity was measured using a rotational rheometer ("MCR302" manufactured by Anton Paar) at 25°C and a shear rate of 1 sec. -1 Furthermore, water was added to the polymer in an amount of 5000 ppm relative to the resin, and the viscosity was measured again in the same manner after 1 hour to confirm whether the viscosity increased by 50% or more, which was evaluated as "viscosity increase due to addition of water" in the table.
[0168] In addition, for the composition of some embodiments and comparative examples, the components in the LDM polymerization liquid were set to 100 parts by mass according to the formulation shown in Table 4, and a toluene solvent and a curing agent ("Perhexyne 25B" manufactured by NOF Corporation, 2,5-dimethyl-2,5-bis(tert-butylperoxide)-3-hexyne) were further added. Coordination polymerization was carried out in the same manner as above to obtain a polymer. The obtained polymer was evaluated as follows. The results are shown in Table 4.
[0169] <Measurement of storage modulus>
[0170] The dynamic viscoelasticity measuring device (TA Instruments, formerly Rheometrics RSA-G2) was used to measure the temperature in the range of -60°C to +300°C at a frequency of 1 Hz. The sample for measurement (3 mm × 40 mm) was cut out from a film with a thickness of about 0.1 to 0.3 mm and the storage modulus was determined at 25°C. The main measurement parameters related to the measurement are as follows.
[0171] Measuring frequency 1Hz
[0172] Heating rate: 3℃ / min
[0173] Sample measurement length 10mm
[0174] Strain 0.1%
[0175] <Measurement of dielectric constant and dielectric loss (dielectric loss tangent)>
[0176] Dielectric constant and dielectric loss tangent use a balanced disk resonator (made by Deutsche Technologies) to evaluate dielectric properties in the same way. For the dielectric property evaluation method using a balanced disk resonator, prepare two samples cut out from a sheet (3 cm in diameter and 0.2 to 0.6 mm in thickness), sandwich a copper foil between them, and place them in the resonator to measure the resonant frequency (f0) and unloaded Q value (Qu) of the peak appearing at 27 to 42 GHz. The dielectric constant is calculated based on f0 and the dielectric loss tangent (tanδc) is calculated based on Qu using the analysis software (Balanced type circular disk resonator (method) calculator) attached to the resonator. The measurement temperature is 23°C and the humidity is 50% RH.
[0177] As shown in Tables 2 and 3, Example 1 using chelating agent 1 having two oxygen atoms in the molecule and Examples 2 to 6 using chelating agent 2 did not produce gels, and did not show an increase in viscosity when water was added.
[0178] On the other hand, in Comparative Examples 1 and 7 to 8 in which no chelating agent was added, gel was generated and the viscosity increased when water was added.
[0179] Comparative Example 2 used the same chelating agent 1 as in Example 1, but the amount thereof was small, so a gel was produced and the viscosity increased when water was added, which was not suitable.
[0180] In Comparative Example 3, which uses Chelating Agent 3 having a large number of oxygen atoms in the molecule and an ester structure, the dielectric loss tangent is higher than that of the Example and is not suitable. Even a small difference in the dielectric loss tangent (a difference of the order of 0.0001) has a large impact, so even a slight decrease can be considered a significant effect.
[0181] Comparative Example 4 using the chelating agent 4 having no oxygen atom but nitrogen atom in the molecule produced a gel and increased viscosity when water was added, which was not suitable.
[0182] Comparative Example 5 using a chelating agent 5 having many oxygen atoms and nitrogen atoms in the molecule had poor solubility of the chelating agent, resulting in the formation of a gel, and the viscosity increased when water was added, which was not suitable.
[0183] Comparative Example 6 used the same chelating agent 2 as in Examples 2 to 4, but the amount thereof was small, so a gel was produced and the viscosity increased when water was added, which was not suitable.
Claims
1. A composition, characterized in that Include: (A) a curable hydrocarbon resin; (C) a co-catalyst which is a metal compound or a semi-metal compound; and (D) a chelating agent having one or two oxygen atoms in one molecule, The amount of the component (D) is 2 mol or more per 1 mol of the component (C) contained in the composition.
2. The composition according to claim 1, wherein The component (A) contains an olefin-aromatic vinyl compound-aromatic polyene copolymer.
3. The composition according to claim 2, wherein The component (A) satisfies the following conditions (1) to (4), (1) The number average molecular weight of the copolymer is 500 or more and 100,000 or less; (2) the aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% to 70% by mass; (3) the aromatic polyene monomer unit is one or more selected from polyenes having a plurality of vinyl and / or vinylidene groups in the molecule and having a carbon number of 5 to 20, and the content of vinyl and / or vinylidene groups derived from the aromatic polyene monomer unit is 1.5 to less than 20 in terms of number average molecular weight; (4) The olefin monomer units are one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units and aromatic polyene monomer units is 100% by mass. 4 . The composition according to claim 1 , further comprising (B) a resin component containing at least one selected from the group consisting of thermoplastic hydrocarbon elastomers and thermoplastic conjugated diene polymers.
5. The composition according to any one of claims 1 to 4, wherein The amount of the component (D) is 0.5 parts by mass or more and 10 parts by mass or less based on 100 parts by mass of the component (A). 6 . The composition according to claim 1 , further comprising (E) a catalyst, wherein the catalyst is a metal compound or a semi-metal compound.
7. The composition according to claim 6, wherein The amount of the component (D) is 100 mol or more per 1 mol of the component (E) contained in the composition.
8. The composition according to any one of claims 1 to 7, wherein The component (D) does not contain a nitrogen atom in its molecule.
9. The composition according to any one of claims 1 to 8, wherein (D) The component contains one or more selected from the group consisting of 4-tert-butylcatechol and acetylacetone. 10 . A cured product, which is a cured product of the composition according to claim 1 . 11 . A laminate comprising a metal foil and a layer containing the composition according to claim 1 .
12. A single-layer CCL, a multi-layer CCL, a single-layer FCCL or a multi-layer FCCL substrate, comprising the cured body according to claim 10.
13. A solution comprising the composition according to any one of claims 1 to 9 and a solvent for dissolving the composition.