Ni-Cr alloy member comprising laminated molded body, method for producing Ni-Cr alloy member, and product produced using Ni-Cr alloy member

By optimizing the content of Cr and Mo and the heat treatment conditions of Ni-Cr alloys, and using the laminated molding method to manufacture Ni-Cr alloy members, the problem of insufficient oxidation resistance and corrosion resistance in high-temperature corrosion environments is solved, and the mechanical characteristics are significantly improved and corrosion resistance.

CN118900924APending Publication Date: 2024-11-05PROTERIAL LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380027242.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-08
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing Ni-Cr alloy members lack oxidation resistance and corrosion resistance in high-temperature corrosion environments, especially in an environment above 600°C, and the surface oxide film is uneven, resulting in a decrease in corrosion resistance.

Method used

The laminated molding body is produced by a laminated molding method of laser beam or electron beam using Ni-Cr alloy containing Cr: 25% or more and 49% or less and Mo: 0% to 10% or less, and a laminated molding method of laser beam or electron beam, and is between 300°C and 1350°C. Heat treatment is performed to suppress the precipitation of the BCC phase, and a uniform Cr oxide film is formed to improve oxidation resistance and corrosion resistance.

Benefits of technology

It achieves a significant improvement in oxidation resistance and corrosion resistance at high temperatures, while improving mechanical characteristics such as endurance and hardness, which are suitable for applications in high-temperature corrosion environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900924A_ABST
    Figure CN118900924A_ABST
Patent Text Reader

Abstract

Provided is a Ni-Cr alloy member having improved corrosion resistance and oxidation resistance at high temperatures, and also having excellent mechanical characteristics. The solution is a Ni-Cr alloy member containing, in mass ratio, 25% to 49% of Cr, more than 0% and 10% or less of Mo, and Ni and unavoidable impurities as the remainder, the Ni-Cr alloy member is a Ni-Cr alloy member comprising a laminated molded body having a face-centered cubic structure (FCC phase) as a main component and having a body-centered cubic structure (BCC phase) phase fraction of less than 2.5%. Here, the size of the phase having the body-centered cubic structure is less than 10 [mu] m. In addition, the laminated molded body contains crystal grains having a plurality of columnar unit structures, and there is a dislocation accumulation portion between the plurality of adjacent columnar unit structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a Ni-Cr alloy component including a stacked molded body, a method for manufacturing the Ni-Cr alloy component, and a product using the Ni-Cr alloy component. Background Art

[0002] Components or parts used in chemical equipment, semiconductor manufacturing processes, etc. require corrosion resistance that can withstand corrosive environments. Stainless steel is generally used in such environments, but Ni-based alloys are selected for parts that are particularly susceptible to high corrosive environments.

[0003] In addition, the design of the components or parts becomes complicated, and it is required to give them complex shapes that are difficult to produce even in die forging or machining. In recent years, additive manufacturing has been increasingly used in the production of components with complex shapes.

[0004] As a method for making a component of a complex shape used in the above-mentioned corrosive environment, an additive manufacturing method (AM) of a corrosion-resistant alloy based on Ni is disclosed in Patent Document 1. A heat source is repeatedly supplied to the raw material powder to melt and solidify the raw material powder (hereinafter referred to as melting and solidification), thereby obtaining an additively manufactured body of a three-dimensional shape. According to the additive manufacturing method, even if it is a complex shape, a three-dimensional product can be obtained in a net shape or a near net shape. The following situation is shown: by applying an additive manufacturing method (hereinafter referred to as stacking molding), grains having a plurality of columnar unit structures are formed in the grains in the Ni-based alloy, and Mo segregation is formed between the columnar unit structures, thereby obtaining a high-strength metal stacked molded body (hereinafter referred to as a stacked molded body or simply a molded body). In addition, as disclosed in Patent Document 2, the term "additive manufacturing" is regarded as an industry standard term as specified in the American Society for Testing and Materials (ASTM) F2792.

[0005] The stacked molding can obtain a three-dimensional product through a net shape or a near net shape, and can obtain excellent properties of both strength and corrosion resistance by applying it to corrosion-resistant alloys. However, the stacked molding shown in Patent Document 1 has room for improvement in terms of high-temperature oxidation resistance, for example, when exposed to an environment above 600°C. For example, in a jet engine or a rocket engine, a combustion furnace exposed to flames in an incinerator, etc., it is desired to further improve the high-temperature oxidation resistance.

[0006] In the past, in such an environment, a molten forging material containing a Ni-Cr alloy with a high Cr content (Patent Document 3) that forms a more stable surface oxide film was used. However, in a Ni-Cr alloy with a high Cr content, the stability of the BCC phase (Body centered cubic structure) relative to the FCC phase (Face centered cubic structure) as the parent phase also increases, and sometimes separates into a two-phase structure during smelting. In the molten material, the amount of BCC phase generated as a precipitated phase tends to increase, and the Cr concentration forming the surface oxide film becomes uneven, so the corrosion resistance decreases and becomes a problem.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2020-179766

[0010] Patent Document 2: Japanese Patent Publication No. 2016-502596

[0011] Patent Document 3: Japanese Patent Application Publication No. 2008-291281 Summary of the invention

[0012] Problems to be solved by the invention

[0013] Based on the above, the object of the present invention is to provide a Ni-Cr alloy component including a stacked molded body, which has improved corrosion resistance and oxidation resistance at high temperatures and excellent mechanical properties, a method for manufacturing a Ni-Cr alloy component, and a product using the Ni-Cr alloy component.

[0014] Technical means of solving problems

[0015] The present invention is a Ni-Cr alloy component, which contains, by mass ratio, Cr: 25% or more and 49% or less, Mo: more than 0% and 10% or less, and Ni and inevitable impurities as the remainder, and the Ni-Cr alloy component is a stacked molded body comprising a face-centered cubic structure (FCC phase) as the main component and a phase fraction of a phase (BCC phase) having a body-centered cubic structure of less than 2.5%.

[0016] In this case, it is preferred that the size of the phase having a body-centered cubic structure contained in the stacked shaped body is less than 10 μm.

[0017] In addition, it is preferred that the stacked structure includes crystal grains having a plurality of columnar unit structures, and that dislocation accumulation portions exist between adjacent ones of the plurality of columnar unit structures.

[0018] In addition, it is preferred that the matrix phase including the crystal grains includes a Ni-based phase, and that no segregation of Cr is contained in the matrix phase.

[0019] In addition, it is preferred that the Vickers hardness of the stacked shaped body be 240 HV or more.

[0020] In addition, it is preferred that the laminated shaped body has a bearing strength of 400 MPa or more.

[0021] The present invention is a product using the Ni-Cr alloy member.

[0022] The present invention is a method for manufacturing a Ni-Cr alloy component including a stacked molded body, which has a stacked molding step of obtaining a stacked molded body including a Ni-Cr alloy by stacked molding using a laser beam or an electron beam, wherein the Ni-Cr alloy contains, by mass ratio, Cr: more than 25% and less than 49%, Mo: more than 0% and less than 10%, and Ni and unavoidable impurities as the remainder, and during melting and solidification accompanying the stacked molding, by rapidly cooling in a temperature range exceeding 300°C and less than the solidification point, the precipitation amount of a phase having a body-centered cubic structure relative to a phase having a face-centered cubic structure is less than 2.5% in terms of phase fraction.

[0023] In addition, the stacked shaped body may be heat-treated at 1000° C. to 1350° C. In this case, the heat treatment is preferably performed for 0.5 hours to 3 hours.

[0024] Effects of the Invention

[0025] According to the present invention, a Ni-Cr alloy component including a stacked shaped body having excellent corrosion resistance and oxidation resistance at high temperatures and also excellent mechanical properties, a method for manufacturing the Ni-Cr alloy component, and a product using the Ni-Cr alloy component can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] [ Figure 1 ] (a) is an image of the stacked structure A observed by scanning electron microscopy (SEM). (b) is an SEM image showing individual crystal grains by magnifying it, and (c) is an SEM image showing a columnar unit structure by further magnifying it.

[0027] [ Figure 2 ] (a) is an image of the stacked structure A observed by scanning transmission electron microscopy (STEM). (b) is an enlarged view of part b, and (c) is an enlarged view of part c.

[0028] [ Figure 3 ](a) shows a reflected electron image of the stacked structure A after solution treatment based on SEM, and (b) shows a composition mapping diagram of Cr of the stacked structure A after solution treatment observed using SEM and EDX.

[0029] [ Figure 4 ](a) shows a reflected electron image of a forged body based on SEM, and (b) shows a composition mapping diagram of Cr after solution treatment of the forged body observed using SEM and EDX.

[0030] [ Figure 5 ](a) is a phase diagram showing the distribution of FCC phase and BCC phase obtained by electron backscattering diffraction (EBSD) of the stacked molded body A, (b) is a phase diagram showing the distribution of FCC phase and BCC phase obtained by EBSD of the stacked molded body A after solution treatment, (c) is a phase diagram showing the distribution of FCC phase and BCC phase obtained by EBSD of the forged body.

[0031] [ Figure 6 ](a) is the intensity spectrum of the stacked body A obtained by X-ray diffraction (XRD), (b) is the intensity spectrum of the stacked body A after solution treatment obtained by XRD, and (c) is the intensity spectrum of the forged body obtained by XRD.

[0032] [ Figure 7 ](a) is an optical microscope image showing the appearance of the stacked molded body A after being immersed in a 2% hydrochloric acid aqueous solution (boiling), and (b) is an optical microscope image showing the appearance of the forged body after being immersed in a 2% hydrochloric acid aqueous solution (boiling). DETAILED DESCRIPTION

[0033] Hereinafter, the Ni-Cr alloy component including the stacked shape of the present invention will be described with reference to the accompanying drawings. First, the alloy composition and the stacked shape will be described, and it will be described that the stacked shape of the present embodiment can improve the corrosion resistance by suppressing the precipitation of the BCC phase that produces the segregation of Cr. In addition, it will be described that the stacked shape according to the present embodiment can obtain high endurance compared with the Ni-Cr alloy component of the same composition that has been forged and rolled. In addition, in this specification, the % indicating the content of the metal element refers to the mass %. In addition, the numerical range represented by "to" refers to the numerical value recorded before and after the "to" as the lower limit and upper limit. In addition, these upper limits and lower limits can be combined arbitrarily.

[0034] [Alloy composition]

[0035] The stacked molded body includes a Ni-Cr alloy having the largest Ni content and the second largest Cr content in terms of mass ratio. That is, the stacked molded body is a Ni-Cr alloy component. In the Ni-Cr alloy component in the present embodiment, Ni and Cr are referred to as main constituent elements. Among the main constituent elements, Cr is preferably contained in a range of 25% or more and 49% or less. In addition, the content of Ni is determined as the remainder relative to Cr and other elements.

[0036] The present invention is not limited to an alloy composition as long as the Ni—Cr alloy member contains Cr. For example, an example of a composition suitable for a component of a semiconductor manufacturing device used in a severe corrosive environment is described below.

[0037] (Chromium Cr: 25% or more and 49% or less)

[0038] Cr has the effect of improving corrosion resistance to halogen gases such as HCl, Cl2, HF, F2, NF3, ClF3 and HBr used in semiconductor manufacturing equipment. In particular, when the components of the semiconductor manufacturing equipment are temporarily exposed to the outside air when open, moisture from the atmosphere is adsorbed on the metal surface. If the adsorbed moisture is hydrated with the halogen process gas, electrochemical corrosion will occur. For hydrated acids, Cr exerts its corrosion resistance especially in the area with relatively low concentration. In addition, by containing a larger amount of Cr, it can also be resistant to high-temperature oxidation required by combustion furnaces, etc. In order to manifest these characteristics, Cr needs to contain more than 25%, more preferably more than 30%, but if it contains more than 49% (i.e. more than half), it is easy to produce the precipitation of BCC phase with the same crystal structure as pure Cr, making it difficult to maintain the uniformity of Cr concentration required for the manifestation of high-temperature oxidation resistance. Therefore, it is preferred to set its content to more than 25% and less than 49%, more preferably to more than 30% and less than 49%.

[0039] Furthermore, in the present alloy, Mo may be added as a main constituent element.

[0040] (Molybdenum Mo: more than 0% and less than 10%)

[0041] Since Mo is contained in the same way as Cr, it has the effect of improving corrosion resistance to halogen gases such as HCl, Cl2, HF, F2, NF3, ClF3 and HBr. However, if Mo is added excessively in the case of a large amount of Cr, coarse intermetallic compounds (P phase, μ phase, σ phase, etc.) are easily generated, resulting in adverse effects such as reduced corrosion resistance or reduced ductility caused by the formation of Mo-deficient areas. Therefore, the content of Mo should be set to more than 0% and less than 10%. In order to cope with a large amount of Cr, the upper limit of the preferred Mo amount is 8%, and more preferably 5%. In addition, in order to clearly improve corrosion resistance, the lower limit of the preferred Mo amount is 0.5%, and more preferably 1.0%.

[0042] (Other elements)

[0043] The Ni-Cr alloy component in the stacked molding of the present embodiment is basically composed of Cr: 25% or more and 49% or less, Mo: more than 0% and 10% or less, and Ni and inevitable impurities as the remainder. The Ni-Cr alloy component of the present embodiment sometimes contains Cr, Mo and Ni. In addition, in addition to the main constituent elements, other arbitrary elements may be contained as needed. The arbitrary elements are described below.

[0044] (Tantalum Ta: 2.5% or less)

[0045] Ta has the effect of improving the corrosion resistance to reducing acids or oxidizing acids, and the corrosion resistance to pitting and crevice corrosion. Therefore, Ta may be contained in an amount of 2.5% or less, preferably in a range of 1.0% to 2.5% or less, as required.

[0046] (Tungsten W: less than 5%)

[0047] W has the same effect as Mo in improving the corrosion resistance to reducing acids. In addition, W can also increase the melting point, thereby increasing the viscosity of the melt, making it easier to control the particle size when manufacturing powder. Therefore, it is possible to suppress the generation of fine powder (particle size less than 5 μm) that makes stacking modeling difficult. Therefore, it is contained in a range of 5% or less, preferably 2% or more and 5% or less, as required.

[0048] The following may be contained: less than 7.00% Fe, less than 2.50% Co, less than 0.04% N, less than 0.50% Mn, less than 0.01% Mg, less than 0.20% Si, less than 0.50% Al, less than 0.50% Ti, less than 0.25% Cu, less than 0.30% V, less than 0.05% B, less than 0.20% Zr, less than 0.10% O, etc.

[0049] As other inevitable impurities, C forms carbides with Cr near the grain boundary, increasing the deterioration of corrosion resistance, so it is preferably suppressed to less than 0.05%. In addition, S or P segregates at the grain boundary and becomes the cause of high temperature cracking, so it is preferably suppressed to less than 0.01%.

[0050] The content of these inevitable impurities is preferably as low as possible and may be 0%.

[0051] [Raw material alloy powder]

[0052] In order to shape the stacked molding body of the present embodiment, a raw alloy powder having the above composition is prepared. The chemical composition of the raw alloy powder is basically the same as that of the stacked molding body, but in the case where the stacked molding body includes an oxide film having excellent corrosion resistance on the surface, the oxygen content of the stacked molding body may be higher than that of the raw alloy powder. The oxide film will be described later.

[0053] The chemical composition of the raw alloy powder and the stacked molded body can be measured by fluorescent X-ray analysis or high-frequency inductively coupled plasma (ICP) analysis. In addition, the content of C, S, N, and O can be determined by gas analysis using a combustion method.

[0054] The additive manufacturing method (referred to as the stacking modeling method in this specification) is a modeling method that obtains the desired shape by repeatedly melting and solidifying each powder, but if the particle size of the raw alloy powder is too small, the supply of the powder becomes unstable, so it is difficult to obtain a sound stacking modeling body. On the contrary, if the particle size of the raw alloy powder is too large, it contains powder that cannot be completely melted in a tiny heat source, so it is difficult to obtain a sound stacking modeling body. Therefore, the particle size of the raw alloy powder is used in the range of about 5μm to 500μm, but the particle size distribution obtained in the powder bed method is different from that obtained in the metal deposition method. In the powder bed method, the particle size d50 corresponding to the cumulative 50 volume% in the cumulative distribution curve obtained by the laser diffraction method, which shows the relationship between the particle size and the cumulative volume from the small particle size side, is preferably about 10μm to 100μm. In addition, in the metal deposition method, the particle size d50 is preferably about 30μm to 250μm.

[0055] The raw alloy powder can be produced by gas atomization, water atomization, disk atomization, plasma atomization, plasma rotating electrode atomization, etc. The raw alloy powder is preferably spherical, and the method with excellent productivity is preferred, so the raw alloy powder is preferably produced by gas atomization.

[0056] [Layered Style]

[0057] The stacking molding method for metal materials can be divided into a powder bed fusion method (PBF: Powder Bed Fusion) and a directed energy deposition method (DED: Directed Energy Deposition). The stacking molding body of the present embodiment can also be molded by either method.

[0058] The powder bed fusion bonding method (powder bed method) is a method of spreading metal powder and using a laser beam or electron beam as a heat source to melt and solidify the molded part. By spreading metal powder to form a solidified layer after melting and solidification, and repeating the above operation, the solidified layers are stacked to form a component of a specified shape. The powder bed method has the following laser beam heat source method and electron beam heat source method.

[0059] The laser beam heat source method is to irradiate the metal powder material with a laser beam to melt, solidify and stack the material. The known methods include powder laser melting (SLM) and powder laser sintering (SLS). The laser beam heat source method melts and solidifies in an inert environment such as argon or nitrogen.

[0060] The electron beam heat source method converts the kinetic energy of the metal powder into heat by irradiating the metal powder with electron beams in a high vacuum and causing it to collide, thereby melting the powder. The electron beam method melts and solidifies the powder in a vacuum. The electron beam heat source method is called the powder electron beam melting method (Selective Electron Beam Melting: SEBM) or simply the electron beam melting method (EBM).

[0061] The directional energy deposition method is also called a metal deposition method, in which metal powder is continuously sprayed in front of the direction in which the laser beam or electron beam is moved, and the supplied metal powder is irradiated with a laser beam or an electron beam to melt and solidify it to form a shape.

[0062] The powder bed method has the advantage of high shape accuracy of the stacked molded body, while the directional energy deposition method has the advantage of high-speed molding. In the powder bed method, SLM is a method of molding by using a fine laser beam to selectively melt, solidify and stack the solidified layers of a powder bed with a stacking thickness of tens of μm. Compared with other stacking molding methods, it has the characteristic of being able to mold precision parts. In the present embodiment, in the case of molding precision parts, SLM is preferably used. At this time, for example, the conditions of laser power below 1000W, scanning speed below 7000mm / s, scanning spacing 0.02mm~0.20mm, and layer thickness 0.01mm~0.2mm can be selected, and the energy density can be appropriately set for molding.

[0063] The scanning path of the laser beam or electron beam in the powder bed method and the directional energy deposition method is arbitrary. It can be scanned parallel to the X-axis direction and reciprocatingly, or it can be scanned parallel to the Y-axis direction and reciprocatingly. The stacked molding body is stacked in the Z-axis direction (usually the vertical direction), and its upper end surface is called the XY surface, and the side surfaces are called the Z surface.

[0064] In addition, in the stacked molded body, regarding the XY plane as the upper end surface and the Z plane as the side surface, it is preferred to perform scanning with a heat source such as a laser beam twice or more (for example, twice) in terms of improving dimensional accuracy or surface accuracy. In addition, in the second and subsequent scans, metal powder is not supplied and only scanning with a laser beam or the like is performed. The XY plane and the Z plane constitute the outer surface of the stacked molded body. The multiple scannings with a laser beam or the like can contribute to improving the corrosion resistance of the stacked molded body described later.

[0065] [Corrosion resistance and high temperature oxidation resistance]

[0066] As in the present embodiment, in a Ni-Cr alloy component including a stacked molded body containing a large amount of Cr, in order to manifest the corrosion resistance based on Cr, it is effective to have no deviation in the Cr concentration in the stacked molded body, that is, to uniformly disperse Cr without causing Cr segregation. Factors affecting the dispersion of Cr are roughly divided into solidification segregation generated during solidification and composition changes caused by solid phase transformation after solidification. Segregation can be said to be a phenomenon in which a specific element is distributed in a biased manner due to solidification and solid phase transformation. In this regard, in the stacked mold, macroscopic solidification segregation throughout the entire molten portion can be prevented by local melting caused by the tiny heat source and the accompanying local quenching. Specifically, when solidifying from the high temperature region (above 1400°C) during melting, the cooling process in the temperature region (intermediate temperature region) of about 1000°C to 300°C is not maintained and high-speed cooling is performed, thereby suppressing the generation of precipitates or segregation. That is, it is characterized by having "a process of rapidly cooling to a temperature range exceeding 300° C. and below the solidification point during melting and solidification accompanying the layered molding".

[0067] Examples of precipitates that can be suppressed during the process include carbides and intermetallic compounds. In Ni-Cr alloys containing a large amount of Cr, it is required to suppress the formation of BCC phases caused by pure Cr. In particular, in Ni-Cr alloys with a Cr content exceeding 25 mass %, or even 30 mass %, the possibility of the formation of BCC phases after solidification becomes high. If the BCC phase is generated, an FCC phase with a small amount of Cr is generated around the BCC phase with a large amount of Cr, resulting in an uneven distribution in the Cr concentration. Here, in terms of suppressing the BCC phase, a stacking molding process with a high cooling rate in the intermediate temperature region where phase transformation may occur is effective. The absence of a Cr segregation portion can prevent the suppression of the BCC phase in the intermediate temperature region. According to this process feature, a Ni-Cr alloy with a BCC phase phase fraction of less than 2.5% (including 0) can be obtained even if the Cr content is 25 mass %, more preferably 30 mass % or more. The phase fraction of the BCC phase is preferably small. If it is less than 2.5%, it can be said that there is an inhibitory effect on the formation of the BCC phase. Regarding the method for confirming that the phase fraction is less than 2.5%, for example, it can be confirmed in the following manner: the phase diagram in the electron backscattering diffraction method (EBSD) is obtained to calculate that the detection ratio of the BCC phase is less than 2.5% of the total. In addition, it can also be confirmed by not observing (substantially not detecting) the diffraction peak caused by the BCC phase in the X-ray diffraction method (XRD). Alternatively, the phase fraction can be confirmed to be small by a peak intensity of less than 3% relative to the peak intensity of the FCC phase, and more preferably less than 2%. In addition, it can also be evaluated by showing that the area of ​​the diffraction spot of the BCC phase in the transmission electron microscopy method (Transmission Electron Microscopy: TEM) is less than 2.5%.

[0068] In a Ni-Cr alloy having a macroscopically uniform structure without deviation, it is believed that the detection ratio of the BCC phase is the same regardless of which cross section is cut, and therefore the phase fraction of the BCC phase is believed to be substantially the same regardless of the area ratio or the volume ratio.

[0069] In addition, the stacked shaped body of the present embodiment can improve corrosion resistance and high-temperature oxidation resistance by including a film containing an oxide (Cr2O3) containing Cr as a constituent element in the surface layer. The oxide film is formed from the surface of the stacked shaped body in a range of 1nm to 1000nm, preferably with a thickness of 1nm to 100nm. The thickness of the oxide film is more preferably 2nm to 20nm, and more preferably formed to a thickness of 3nm to 10nm. For example, a stacked shaped body of a Ni-Cr alloy containing 25% by mass or more, more preferably 30% by mass or more, of Cr forms a more stable surface oxide film, so in addition to corrosion resistance, high-temperature oxidation resistance in a high-temperature atmosphere including a combustion furnace is also excellent.

[0070] The oxide film of the present embodiment is preferably formed by oxidation treatment in a high temperature environment and a low oxygen atmosphere for a stacked molded body in which Cr is uniformly dispersed. The oxidation treatment can be performed during the stacking molding. The oxide film is a film formed on the outer surface of the stacked molded body, so the oxidation treatment performed during the stacking molding is performed when the outer surface is molded. Specifically, in the laser beam heat source type of the powder bed method, as described above, the stacking molding is performed in an inert atmosphere such as nitrogen and argon. If a trace amount of oxygen is contained in the inert gas, the oxidation treatment can be performed during the stacking molding method in which the raw alloy powder is melted and solidified.

[0071] The oxygen concentration in the oxidation treatment of the present embodiment is preferably in the range of 100 ppm to 21%, more preferably in the range of 100 ppm to 1%, and still more preferably in the range of 100 ppm to 2000 ppm. The oxygen concentration is determined on a volume basis.

[0072] The temperature in the oxidation treatment of the present embodiment is preferably in the range of 300°C to 1000°C, more preferably in the range of 400°C to 800°C, and still more preferably in the range of 500°C to 600°C.

[0073] In the above oxygen concentration range, oxidation treatment at a low oxygen concentration is preferred in order to obtain a dense oxide film. However, even if the oxygen concentration is 21%, for example, a dense oxide film can be formed if a low temperature of around 200° C. to 300° C. is selected.

[0074] [organize]

[0075] The stacked molded body of this embodiment has improved endurance and hardness compared to a forged body that is a material that has been forged and rolled, even if it is a Ni-Cr alloy having the same chemical composition, as shown in the examples described later. The stacked molded body with improved mechanical properties has a columnar unit structure generated in the stacked molding process. Dislocation accumulation portions are formed at the boundaries of the columnar unit structure, which function as a so-called dislocation pinning effect, thereby improving the mechanical properties.

[0076] Next, the mechanism by which the columnar unit structure formed in the stacked structure contributes to the improvement of mechanical properties will be described.

[0077] As described above, in the present application, a layered molding method using a laser beam or an electron beam is used. Since a laser beam or an electron beam is used for melting and solidification, the solidification speed is extremely high, and a fine and columnar unit structure is generated in the grains due to rapid solidification. If the structure after solidification is observed, it is as follows Figure 1 (c) As a result, multiple columnar unit structures 3 are gathered to form grains. Moreover, due to the rapid solidification in the stacking molding process, dislocations (like stripes) are generated in the unit structure between adjacent unit structures 3 (unit boundaries). Regarding the dislocations in the unit structure, they want to become energetically stable and move to achieve dislocation bonding, but they are not reduced much during the rapid solidification in the stacking molding process and remain. Therefore, the dislocation density (dislocation density) in the unit structure is maintained at a high level. It is believed that the high dislocation density leads to improved mechanical properties of the stacked molded body.

[0078] Here, Figure 1It is a SEM image of a stacked molded body. The stacked molded body is shown in (a), and the shape of columnar grains 2 (hereinafter also referred to as columnar crystals 2) extending along the stacking direction 1 is shown in the molded body structure. As shown in (b), each columnar grain 2 is arranged and generated in the stacking direction 1. In this embodiment, the average particle size of the columnar grains 2 is 5μm to 150μm, preferably about 10μm to 50μm. In the further enlarged (c), the portion shown as a white area is the columnar unit boundary 4, and the area surrounded by the unit boundary is the columnar unit structure 3. The columnar unit boundary often has a short axis and a long axis, and the short axis direction is 200nm to 4000nm, preferably about 500nm to 2000nm. The long axis direction has a length of 4μm to 80μm, preferably about 5μm to 30μm. In addition, although not shown in the SEM image, there is also an image of a white area that looks like a circle in the SEM image. This is because the columnar unit structure 3 is cut in a section perpendicular to the paper surface, so the unit boundary looks circular. In addition, since the cross-section of the columnar unit structure 3 is not a perfect circle, the average diameter of the cross-section of the columnar unit structure 3 is calculated as the average diameter of the circle equivalent diameter. In the present embodiment, the average diameter of the circle equivalent diameter of the cross-section of the columnar unit structure 3 is less than 1000nm. In addition, adjacent columnar unit structures 3 are mostly arranged in the same direction, and multiple columnar unit structures 3 are generated in a single grain. There are tens to thousands of columnar unit structures 3 inside a grain. Among them, not all grains constituting the stacked molded body of the present embodiment necessarily have columnar unit structures 3. In addition, for the forged body, if the average grain size of the grains is generally tens to hundreds of μm, it can be seen that the stacked molded body has a fine structure.

[0079] Figure 2 (a) is from Figure 1 (c) is an image observed at the position indicated by the dotted line ab, and is a STEM image of a thin slice cut out by focused ion beam processing. In the figure, the image of selecting and enlarging the parts b and c is equivalent to Figure 2 (b) Figure 2 (c). Here, the black stripes 5 observed in the bright field image show dislocations caused by electron scattering due to the strain field. Here, the more black stripes 5 there are, the higher the dislocation density. Dislocations also exist inside the columnar unit structure 3, but a tendency for more dislocation accumulation is observed at the columnar unit boundary 4. In addition, although the dispersion of oxides was also observed in the STEM observation, no segregation of Cr was found. In addition, for other constituent elements such as Mo and Ni, no significant segregation, i.e. deviation, was found in the elemental analysis (energy-dispersive X-ray spectroscopy (EDS)) in the SEM.

[0080] Generally speaking, the dislocation density ρ in fully annealed metal materials is 10 9 m -2 ~10 11 m -2 In addition, it is known that the dislocation density ρ in a heavily processed metal material is 10 14 m -2 ~10 16 m -2 The stacked shaped body of this embodiment can achieve a dislocation density ρ of 10 without any strong processing. 14 m -2 More than 10 16 m -2 The dislocations dispersed in the structure and then accumulated and fixed at the columnar unit boundaries 4 and the like are considered to contribute to the improvement of the mechanical strength of the stacked structure.

[0081] [Mechanical properties]

[0082] As an index showing mechanical properties, proof stress, tensile strength, elongation, drawing, and Vickers hardness (HV) can be cited as examples.

[0083] The endurance of the stacked shaped body of the present embodiment shown above can be preferably 400 MPa or more, more preferably 500 MPa or more, and further preferably 600 MPa or more. Since the stacked shaped body of the present invention contains a large number of dislocations as described above, it can be considered that the strengthening based on the interaction of dislocations, i.e., processing strengthening, plays a role and improves the endurance.

[0084] In addition, regarding the tensile strength, the stacked shaped body of the present embodiment can show a value of preferably 600 MPa or more, more preferably 700 MPa or more, and further preferably 750 MPa or more.

[0085] The elongation is preferably 20% or more, more preferably 30% or more, and further preferably 40% or more.

[0086] In addition, the drawing depth can be shown to be preferably 30% or more, more preferably 40% or more, and still more preferably 50% or more.

[0087] The stacked shaped body of the present embodiment can show a value of preferably 220 HV or more, and more preferably 240 HV or more, in terms of Vickers hardness (HV 10).

[0088] Among the mechanical properties, the proof stress and tensile strength are indices for determining strength, and the elongation and drawing are indices for determining ductility. As the name suggests, the Vickers hardness (HV) is an index for determining hardness.

[0089] [Method for producing laminated structure]

[0090] Next, a preferred method for producing the laminated structure of the present application will be described.

[0091] The manufacturing method has a step of obtaining a laminated molded body containing a Ni-Cr alloy by laminated molding using a laser beam or an electron beam, wherein the Ni-Cr alloy contains 25% to 49% Cr, more than 0% to 10% Mo, and the remainder Ni and inevitable impurities by mass ratio. Here, melting and solidification are repeated in the laminated molding, and in particular, the solidification process is not maintained in the intermediate temperature region of more than 300°C and less than the solidification point, and is rapidly cooled, thereby preventing Cr segregation, thereby eliminating the region where the BCC phase is easy to precipitate. As a result, macroscopic segregation of Cr is not caused, and precipitation of the BCC phase during cooling can be suppressed. As a result, oxidation resistance at high temperatures is improved. Accordingly, as a laminated molding method, it is preferred to use a laser melting method (selective laser melting method (SLM: Selective Laser Melting)) that does not require preheating exceeding 300°C. In addition, even an electron beam laminated molding method (electron beam melting method (EBM: Electron Beam Melting)) can be used without preheating exceeding 300°C.

[0092] In addition, a grain having a plurality of columnar unit structures 3 is formed, and dislocations can be accumulated inside the grain and between a plurality of adjacent columnar unit structures 3. Thus, the mechanical properties can be improved. These are the basic concepts of this manufacturing method. Moreover, the mechanical properties of the stacked molded body can be appropriately adjusted by subjecting the stacked molded body to the following heat treatment and / or aging treatment.

[0093] In the present application, the dislocations are left in the columnar unit boundaries 4 existing in the grains, thereby improving the mechanical properties of the stacked structure based on the above mechanism. Therefore, when specifically expecting to improve the mechanical properties, it is ideal not to use a high temperature and long time heat treatment that completely eliminates the dislocations.

[0094] In addition, the following heat treatment is performed arbitrarily and is not a necessary process. As described later, the stacked molded body ("molded body A" in the embodiment described later) in the molded state (as built) without heat treatment or aging treatment also has a resistance of more than 400 MPa and a Vickers hardness of more than 220 HV, which exceeds the mechanical properties of the forged body. Therefore, the values ​​of other mechanical properties (tensile strength, elongation and stretch) of the stacked molded body in the molded state are also necessary to be sufficient, and it is also preferred to use the stacked molded body in the molded state.

[0095] (Heat Treatment)

[0096] On the other hand, the stacked molded body can be subjected to heat treatment, and the mechanical properties, such as hardness, can be adjusted as shown in the embodiments described later. In the Ni-Cr alloy of the present application, since the amount of Cr added is as much as 25% or more, it is necessary to set the heat treatment conditions at a relatively high temperature in consideration of the eutectic reaction between Ni and Cr. The heat treatment is carried out in the atmosphere at a temperature of 1000°C or more and 1350°C or less, preferably 1000°C or more and 1300°C or less, and more preferably 1100°C or more and 1250°C or less. The heat treatment can be maintained in the temperature range for 10 minutes or more and 10 hours or less, preferably 0.5 hours or more and 3 hours or less, depending on the size of the stacked molded body.

[0097] By setting the heat treatment conditions within the range, the strain of the stacked molded body can be obtained. The strain removal of the stacked molded body helps to improve the shape accuracy of the stacked molded body. On the other hand, if the heat treatment temperature is set to exceed 1350°C, there is a concern that the grains will coarsen or local melting will occur, thereby reducing the endurance or strength. Therefore, the upper limit of the heat treatment temperature is set to 1350°C, preferably 1300°C, and more preferably 1250°C. Heat treatment under this condition is sometimes called solution treatment. The reason is that by performing heat treatment within the range, the alloy components of the material are dissolved into the parent phase.

[0098] The lower limit of the heat treatment temperature is 1000°C, preferably 1100°C. If it is 1000°C or higher, the homogenization of the structure can be achieved without the precipitation of the BCC phase that is stable at low temperatures. Although heat treatment can be performed at less than 1000°C, especially in a composition with a large amount of Cr, if it is maintained at 500°C to 800°C for a long time, in addition to the formation of the BCC phase, there is also a concern that the corrosion resistance will deteriorate due to the formation of Cr carbides, so it is necessary to avoid long-term maintenance.

[0099] In addition, the heat treatment time must be appropriately set based on the heat treatment temperature. For example, when the heat treatment temperature is set to a range of 1200°C to 1300°C, the holding time can be set to 10 minutes to 20 minutes. When the heat treatment temperature is set to a range of 1100°C to 1200°C, the holding time can be set to 20 minutes to 40 minutes. When the heat treatment temperature is set to a range of 1000°C to 1100°C, the holding time can be set to 30 minutes to 2 hours. In addition, in order to prevent the precipitation of BCC in the low temperature part, the cooling after the heat treatment is preferably performed by air cooling (cooling), gas cooling, oil cooling, water bath, etc., and for example, cooling is performed at a cooling rate of 600°C / hour (10°C per minute) or more.

[0100] [use]

[0101] The stacked molded body of this embodiment can be used for any purpose. Even in the stacked molded state, it can be used for high-strength and high-corrosion-resistant purposes, and mechanical properties corresponding to the purpose can be obtained by whether or not heat treatment is performed.

[0102] As an example of a use requiring oxidation resistance at high temperatures, parts constituting combustion furnaces and burners, incinerator parts, jet engines, and rocket engine parts, etc., which are exposed to combustion flames containing sulfides, chlorides, etc., can be cited. In addition, by effectively utilizing the corrosion resistance to mixed acids containing fluoric acid, sulfuric acid, phosphoric acid, and oxidizing acids, etc., which is manifested by high Cr concentrations, the stacked molding of this embodiment can also be applied to semiconductor manufacturing devices or chemical equipment, etc. It is particularly preferred to be applied to components that are in direct contact with these corrosive gases or liquids. In addition, the stacked molding of this embodiment is preferably applied to injection molding screws or cylinders, oil well excavation equipment, or valves or joints of chemical equipment where corrosive fluids flow, heat exchangers, pumps, turbine holes of generators, impellers of compressors, etc. In the present invention, these machines, machines, components, parts, etc. are collectively referred to as manufactured objects.

[0103] Example

[0104] Hereinafter, the present invention will be specifically described based on examples.

[0105] A raw alloy powder for additive manufacturing having the chemical composition shown in Table 1 was prepared. The raw alloy powder was prepared by preparing a melted raw material and melting it in a conventional high-frequency vacuum melting furnace to make a master alloy, and was made by gas atomization in an argon atmosphere. In addition, a powder with a particle size of 10 μm to 60 μm was classified from the atomized powder and provided for additive manufacturing. Regarding the d10, d50, and d90 of the classified powder, d10 was 18.9 μm, d50 was 33.2 μm, and d90 was 58.0 μm.

[0106] [Table 1]

[0107]

[0108] The laminated molding was performed under the following conditions to produce a laminated molded body A (30 mm×30 mm×5 mm) (hereinafter, the laminated molded body may be simply referred to as a molded body).

[0109] Layer modeling device: EOS M290 (SLM method)

[0110] Cascading modeling conditions:

[0111] Energy density: 20J / mm 3 ~200J / mm 3 Method setting

[0112] Energy density = laser power (W) / (scanning speed (mm / s) × scanning pitch (mm) × layer thickness (mm)).

[0113] In the embodiment, the laser power is 350W, the scanning speed is 900mm / s, the scanning interval is 0.11mm, and the layer thickness is 0.04mm, so the energy density is 88J / mm 3 .

[0114] Atmosphere: Ar (O2<0.10%)

[0115] The chemical composition of the molded body A was also analyzed. The results are shown in Table 1. The composition analysis of Mo and Cr was performed by ICP emission spectroscopy. The composition analysis of O (oxygen) was performed by infrared absorption.

[0116] Next, a shaped body A, a shaped body B obtained by heat-treating the shaped body A, and a forged body produced by forging and rolling with the same chemical composition as the shaped body A are prepared.

[0117] The heat treatment of the shaped body B was performed by keeping the body at 1200° C. for 30 minutes in a vacuum furnace and then introducing nitrogen gas for cooling.

[0118] Since solid solution is achieved by the heat treatment, the heat treatment of the molded body B is referred to as "solution heat treatment".

[0119] Next, the structures of the samples of the molded body A, the molded body B, and the forged body were observed, the phase fraction of the BCC phase was calculated, and the mechanical properties and corrosion resistance were measured.

[0120] [Microstructure]

[0121] The microstructures of the molded body A, the molded body B, and the forged body were observed using a scanning electron microscope (SEM: manufactured by JEOL, JSM7900F). Figure 1 , Figure 2 The microstructure of the molded body A is shown in FIG. Figure 3 The microstructure of the molded body B is shown in FIG. Figure 4 The microstructure of the forged body is shown in FIG.

[0122] like Figure 1 As shown in (a) and (b), the microstructure of the molded body as a whole includes columnar grains 2 with a width of several μm along the lamination direction 1 toward the long axis. Figure 1 As shown in (c), columnar unit structures 3 are observed inside the columnar crystal grains 2, and columnar unit boundaries 4 between adjacent columnar unit structures 3 are observed as bright portions (white portions) having a brightness higher than that of the surrounding portions in an electron microscope image (reflected electron image).

[0123] Next, for the purpose of evaluating the internal structure of the cell, a thin slice ( Figure 1 (c) shows the collection site) for observation. Figure 2 The black stripes 5 observed in the bright field images of (a)(b)(c) indicate dislocations caused by electron scattering due to the strain field. Here, the more black stripes 5 there are, the higher the dislocation density. Dislocations also exist inside the columnar unit structure 3, but a tendency for more dislocation accumulation is observed at the columnar unit boundary 4. In addition, the dispersion of oxides was also observed in the STEM observation, but no segregation, i.e., deviation, of the constituent elements including Cr was observed. For the dislocation density of the sample, the dislocation length is a measure of the dislocation length that can be observed in the STEM image (observation area: 4.32 μm 2 (1.44μm 2 The dislocation lengths observed in the samples were measured and the total length was calculated. The evaluation volume was calculated as “observation area × sample thickness (80 nm)”. The dislocation lengths were as high as 5.0 × 10 15 m -2 The value of .

[0124] On the other hand, in the molded body B which is obtained by heat-treating the molded body A, Figure 3 As observed in (a), even at the same magnification, the columnar unit structure disappears, and coarsely grown grains and spherical or lamellar precipitates 6 less than 10 μm are observed mainly at their grain boundaries. The precipitates 6 correspond to the BCC phase as described later. The element mapping based on energy dispersive X-ray spectroscopy (EDS) is obtained in the SEM with the precipitates 6 as the object. The results are as follows: Figure 3 As shown in (b), Cr was confirmed to be locally present in the precipitated phase 6. In addition, the so-called local presence is intended to be described as existing only in a specific place, but here it has the same meaning as segregation and can be referred to as segregation. The same applies to the following.

[0125] In addition, the forged body was also observed using a scanning electron microscope. Figure 4 As shown in (a), a coarser block-shaped precipitate phase 6 with a size of more than 10 μm can be observed. Furthermore, element mapping based on EDS was also observed for the precipitate phase 6, and the result was as follows: Figure 4 As shown in (b), localized presence of Cr was confirmed.

[0126] [Phase fraction of BCC phase with body-centered cubic structure]

[0127] The phase fraction of the phase having a body-centered cubic structure (hereinafter referred to as the BCC phase fraction) of each sample was evaluated by obtaining a phase map using EBSD measurement of the XY surface after mirror polishing (manufactured by JEOL Ltd., JSM7900F). The phase map was obtained based on the Kikuchi figure for each point obtained with a step size of 1 μm in a 400 μm×400 μm area, and it was determined whether it belonged to BCC (body-centered cubic structure) or FCC (face-centered cubic structure). It is shown in Figure 5 (a)(b)(c). Figure 5 In (a), only the Ni-based matrix phase (FCC phase) is included, no Cr segregation is observed in the matrix phase, and no BCC phase is detected. Figure 5 In (b), only a very small amount of BCC phase was detected, but no BCC phase region larger than 10 μm was detected. This is believed to be because the SLM method was used to perform rapid solidification of the powder layer, which shortened the holding time of more than 300°C for the formation of the BCC phase. On the other hand, in the case of the forged body, Figure 5 In (c), a BCC phase larger than 10 μm was detected, and its morphology was similar to that in Figure 4 The precipitated phase 6 where Cr is locally present is consistent with that observed in (a) and (b).

[0128] Next, the ratio of the measurement points determined to be the BCC phase in the phase map obtained by the EBSD was calculated as the BCC phase ratio.

[0129] In addition, although it is not a method for directly measuring the BCC ratio, the diffraction spectrum is obtained by XRD (RIGAKU Smart Lab) using the same sample as EBSD, and the relative Figure 6 The BCC phase ratio can also be evaluated by the intensity ratio of the FCC (200) peak intensity (2θ = 64° to 65°) originated from the BCC phase to the FCC (200) peak intensity (2θ = 50° to 51°) originated from the FCC phase, which is a peak that does not overlap between the FCC phase and the BCC phase. The results are shown in Table 2 as the BCC peak intensity ratio.

[0130] [Mechanical properties]

[0131] Regarding mechanical properties, tensile tests and Vickers hardness tests were performed. Among them, tensile properties were measured at room temperature (22°C) and high temperature (700°C) according to ASTM standards (ASTM E8 and ASTM E21). The tensile direction was set to the XY plane direction in the molded body A and the molded body 2, and to the rolling plane direction in the rolled body. In addition, the Vickers hardness HV was set to the measured value under the load of 0.5 kg and the holding time of 10 s according to the Japanese Industrial Standards (JIS) standard (JIS Z 2244).

[0132] Table 2 shows various mechanical properties, the presence or absence of unit structures as characteristics of the microstructure, the BCC phase ratio obtained by the EBSD measurement, and the (200) peak intensity ratio obtained by the XRD measurement.

[0133] As can be seen from Table 2, the molded body A has a higher resistance and hardness than the forged body. This is believed to be because the molded body A is produced by the layered molding method and thus has a unit structure, and dislocations are introduced into the solidified structure when each layer of powder is rapidly solidified by the SLM method.

[0134] In addition, it can be seen that the high-temperature tensile strength of the molded body A is higher than that of the forged material. On the other hand, it can be seen that the high-temperature tensile strength of the molded body A is lower than the tensile strength at room temperature. It is believed that the reason for this is that the molded body A is exposed to a high-temperature environment of 700°C during the high-temperature tensile test, which promotes the disappearance of dislocations densely contained in the unit structure and promotes the movement of dislocations at high temperatures. However, even if exposed to a high-temperature environment, dislocations will not completely disappear, so it is believed that the high-temperature tensile strength of the molded body A is higher than that of the forged body.

[0135] In addition, from the results of the molded body B, it was confirmed that the unit structure disappeared by performing the solution heat treatment, and the hardness could be adjusted (the hardness could be reduced) without significantly increasing the BCC phase ratio.

[0136] In addition, according to Figure 2 , a high density of dislocations is included in the unit structure of the shaped body A. That is, since the shaped body A having the same composition and only a high dislocation density has a higher hardness than the shaped body B, it is considered that the dislocation density is correlated with these mechanical properties.

[0137] [Table 2]

[0138]

[0139] N / A: No measurement data

[0140] [Corrosion resistance]

[0141] Next, corrosion resistance was evaluated using the molded body A and the forged body.

[0142] Regarding the evaluation of corrosion resistance, the XY surface of the shaped body A and the rolled surface of the forged body were polished with No. 1000 abrasive paper, and then immersed in each of three corrosion solutions (2% hydrochloric acid aqueous solution (boiling), 10% sulfuric acid aqueous solution (boiling), 3% fluoric acid-17% nitric acid aqueous solution (60°C)) for 24 hours to calculate the corrosion rate (mm / year).

[0143] [Table 3]

[0144]

[0145] As shown in Table 3, the shaped body A exhibited a corrosion rate much lower than that of the forged body, particularly when immersed in a 2% hydrochloric acid aqueous solution (boiling). Figure 7 Figure 2 shows the shaped body A after the immersion test in a 2% hydrochloric acid aqueous solution (boiling). Figure 7 (a))、Forging body( Figure 7 (b)) tissue appearance. Figure 7 In the forged body (b), in addition to the grain boundary, it is confirmed that Figure 4 The observed preferential corrosion portion 7 corresponds to the precipitated phase 6. Such preferential corrosion portion 7 is not observed in the molded body A. The difference is presumably due to the difference in the BCC phase ratio shown in Table 2, that is, the difference in the amount of BCC phase precipitation, thereby showing the superiority of the stacked molded body in the present invention. It cannot be said that the Ni-Cr alloy has high corrosion resistance to chlorine, but it can be said that even if the chemical composition is the same, the corrosion resistance is improved because it is a stacked molded body in which Cr segregation is suppressed.

[0146] The above evaluation results are summarized as follows.

[0147] (1) Mechanical properties

[0148] Compared with the forged body, the laminated molded body has improved endurance and hardness.

[0149] As shown in Table 2, according to the stacked shaped body (shaped body A) of this embodiment, it can be confirmed that in the state without heat treatment, it has an endurance of more than 500 MPa and a tensile strength of more than 700 MPa at room temperature, and an endurance of more than 300 MPa, a tensile strength of more than 500 MPa, and a Vickers hardness of more than 240HV 0.5 at 700°C.

[0150] In addition, in the stacked shaped body (shaped body B) subjected to the solution heat treatment, the BCC phase ratio can be suppressed, and the Vickers hardness can be adjusted without causing a large amount of precipitation of the BCC phase.

[0151] (2) Corrosion resistance

[0152] The corrosion resistance of the laminated shaped body of this embodiment is better than that of the forged body with the same chemical composition.

[0153] Explanation of symbols

[0154] 1: Stacking direction

[0155] 2: Columnar grains (columnar crystals)

[0156] 3: Columnar unit organization

[0157] 4: Columnar unit boundary

[0158] 5: Black stripes

[0159] 6: Precipitated phase

[0160] 7: Priority Corrosion Department

[0161] Dashed line ab: STEM observation position

Claims

1. A Ni-Cr alloy component comprising, by mass ratio, Cr: 25% or more and 49% or less, Mo: more than 0% and 10% or less, and the remainder Ni and unavoidable impurities, The Ni-Cr alloy component is a Ni-Cr alloy component including a stacked shaped body having a face-centered cubic structure as the main structure and a phase fraction of a phase having a body-centered cubic structure of less than 2.5%.

2. The Ni-Cr alloy component according to claim 1, wherein The size of the phase having a body-centered cubic structure contained in the stacked shaped body is less than 10 μm.

3. The Ni-Cr alloy component according to claim 1 or 2, wherein: The stacked structure includes crystal grains having a plurality of columnar unit structures, and a dislocated accumulation portion is provided between adjacent columnar unit structures.

4. The Ni-Cr alloy component according to claim 3, wherein: The matrix phase including the crystal grains includes a Ni-based phase, and no segregation of Cr is contained in the matrix phase.

5. The Ni-Cr alloy component according to claim 1, wherein Vickers hardness is above 240HV.

6. The Ni-Cr alloy component according to claim 1, wherein The endurance is above 400MPa.

7. A product using the Ni-Cr alloy member according to claim 1.

8. A method for manufacturing a Ni-Cr alloy component including a laminated molded body, comprising a laminated molding step of obtaining a laminated molded body including a Ni-Cr alloy by laminated molding using a laser beam or an electron beam, wherein the Ni-Cr alloy includes, by mass ratio, Cr: 25% to 49%, Mo: more than 0% to 10% and the remainder Ni and unavoidable impurities, During melting and solidification accompanying the stacking formation, by rapidly cooling in a temperature range exceeding 300° C. and below the solidification point, the precipitation amount of the phase having a body-centered cubic structure relative to the phase having a face-centered cubic structure is set to less than 2.5% in terms of phase fraction.

9. The method for manufacturing a Ni-Cr alloy member according to claim 8, wherein: The stacked shaped body is heat treated at a temperature of 1000° C. to 1350° C.

10. The method for manufacturing a Ni-Cr alloy member according to claim 9, wherein: The heat treatment is performed for 0.5 hours to 3 hours.

Citation Information

Cited By

  • Nickel-chromium alloy material with negative Seebeck coefficient as well as preparation method and application of nickel-chromium alloy material

    CN122303687A