Identification medium and article
By combining specific optical characteristics and phase difference materials, the cholesteric resin layer is solved, and the problem of high manufacturing difficulty and cost of cholesteric resin layer is achieved with high recognition function and design recognition medium. Reduces manufacturing complexity and cost.
Patent Information
- Application Number
- CN202380028681.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-05
AI Technical Summary
The wide band processing of the cholesteric resin layer requires precision and multiple segments to be subjected to weak ultraviolet irradiation and heating, resulting in high material cost and difficult manufacturing, making it difficult to achieve high recognition function and design.
The cholesteric resin layer that does not undergo wide banding treatment is adopted, and a specific combination of materials with specific optical characteristics and phase difference is used as the light reflective layer, including more than three types of cholesteric regular material sheets to satisfy the specific reflective band and Integrated reflectivity ratio for silver appearance and high recognition.
A recognition medium with high recognition function and design is realized, reducing manufacturing cost and complexity, and it is easy to obtain the same silver appearance as the wide banding process.
Smart Images

Figure CN118901028A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an identification medium for identifying the authenticity of an object and an object having the identification medium. Background Art
[0002] In order to easily determine whether an item is genuine, an identification medium is usually provided for the item. The identification medium is required to have anti-counterfeiting properties and an identification function. The anti-counterfeiting properties of the identification medium mentioned here refer to the properties that the identification medium cannot be easily copied by conventional techniques such as printing using conventional materials. The identification function of the identification medium refers to the function of being able to distinguish a genuine identification medium from a counterfeit identification medium forged using conventional techniques with a high degree of reliability in a certain way.
[0003] In some known identification media, materials with cholesteric regularity are used as light reflecting layers (e.g., Patent Documents 1 and 2). When light is incident on a material with cholesteric regularity, it is possible to reflect only one component of its circularly polarized components in one direction. Such a property cannot be obtained by copying using printing or other techniques using conventional materials, so such a property can be used to obtain an identification medium with high anti-counterfeiting performance and identification function.
[0004] There are many materials with cholesteric regularity, and their optical properties can be expressed by the selective reflection center wavelength λc and the half-peak width Δλ of the reflection band, and their ratio Δλ / λc as indicators. Materials with relatively large Δλ / λc values can be regarded as relatively wide-band materials, and narrow materials can be regarded as relatively narrow-band materials.
[0005] The main material having cholesteric regularity is a cholesteric resin layer, which is a layer of a material having a structure obtained by polymerizing and curing a polymerizable liquid crystal material capable of exhibiting a cholesteric liquid crystal phase in a state exhibiting a cholesteric liquid crystal phase.
[0006] In most cases, the objects that need to be judged for authenticity have high value in themselves, so they are required to have excellent aesthetics. Therefore, the identification medium given to the object is also required to have excellent aesthetics. Specifically, the appearance in the observation used to show the identification function (observation through a device such as an observer, observation under polarized light, etc.), the appearance in other ordinary observations (observation with the naked eye under natural light without an observer, etc.), or the appearance in both are required to have excellent aesthetics. In the identification medium described in Patent Document 1, a cholesteric resin layer that has been subjected to so-called broadband treatment is used as part of its structural elements. The cholesteric resin layer that has been subjected to broadband treatment can make its reflection band as wide as to the extent of covering the entire visible light region. In this case, the layer can present a mirror-like silver appearance, and as a result, it can exert high design properties.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent document 1: International Publication No. 2021 / 153761 (corresponding publication: European Patent Application Publication No. 4099067);
[0010] Patent document 2: Japanese Patent Application Publication No. 2005-055556. Summary of the invention
[0011] Problem that the invention aims to solve
[0012] Broadband treatment of a cholesteric resin layer is a known technique, but requires a difficult process of precise and multi-step weak ultraviolet irradiation and heating. As a result, the material cost of a manufacturing method involving broadband treatment is high.
[0013] Therefore, an object of the present invention is to provide an identification medium and an article which have a high identification function, can be easily manufactured, and can exhibit high design properties.
[0014] Solutions for solving problems
[0015] In order to solve the above-mentioned problems, the present inventors studied the use of a cholesteric resin layer obtained without broadband treatment as a light reflecting layer to obtain a layer having the same silver appearance as the cholesteric resin layer subjected to broadband treatment. As a result, the present inventors found that the above-mentioned problems can be solved by combining sheets of materials having specific optical properties and cholesteric regularity as light reflecting layers in a specific manner, thereby completing the present invention.
[0016] That is, the present invention includes the following contents.
[0017] [1] An identification medium comprising a light reflecting layer and a patterned phase difference layer, wherein the light reflecting layer is a layer that reflects incident light as circularly polarized light, the patterned phase difference layer is a layer that includes a region having a phase difference, and the patterned phase difference layer is a layer that is provided on the identification medium in such a manner that the region having a phase difference occupies a portion of an area of a display surface of the identification medium, the light reflecting layer comprises sheets of three or more materials having cholesteric regularity, and one or more of the three or more sheets satisfies formula (a),
[0018] Δλ / λc<0.14Formula (a)
[0019] In the formula, Δλ is the half-peak width of the reflection band of the above-mentioned sheet, λc is the selective reflection center wavelength of the above-mentioned sheet, among the above-mentioned three or more sheets, one is a sheet (R) having a selective reflection center wavelength λc(R), and the other is a sheet (G) having a selective reflection center wavelength λc(G), the above-mentioned sheet (R) and the above-mentioned sheet (G) satisfy 600nm<λc(R)≤660nm and 500nm≤λc(G)≤600nm, and the above-mentioned light reflection layer satisfies the following formulas (b-1) to (b-2),
[0020] 0.95≤B(430-490)Ave / G(500-600)Ave≤1.02 Formula (b-1)
[0021] 0.95≤R(600-660)Ave / G(500-600)Ave≤1.02 Formula (b-2)
[0022] In the formula, B(430-490)Ave is the average value of the integral reflectivity of the above-mentioned light reflecting layer at a wavelength of 430nm to 490nm, G(500-600)Ave is the average value of the integral reflectivity of the above-mentioned light reflecting layer at a wavelength of 500nm to 600nm, R(600-660)Ave is the average value of the integral reflectivity of the above-mentioned light reflecting layer at a wavelength of 600nm to 660nm, and the average value of the integral reflectivity of the above-mentioned light reflecting layer at 430-660nm is more than 20%.
[0023] [2] The identification medium according to [1], wherein the sheet (R) and the sheet (G) satisfy the following formula (c):
[0024] |Δλ(R) / λc(R)-Δλ(G) / λc(G)|≤0.01
[0025] ··Formula (c)
[0026] In the formula, Δλ(R) is the half-peak width of the reflection band of the above-mentioned sheet (R), Δλ(G) is the half-peak width of the reflection band of the above-mentioned sheet (G), and the ratio W(R) / W(G) of the weight W(R) of the above-mentioned sheet (R) contained in the above-mentioned light reflecting layer to the weight W(G) of the above-mentioned sheet (G) is greater than 1.15.
[0027] [3] The identification medium according to [1] or [2], wherein one or more of the three or more sheets satisfies formula (d),
[0028] 0.14≤Δλ / λc≤0.25 Formula (d).
[0029] [4] The identification medium according to any one of [1] to [3], wherein the three or more sheets, in addition to the sheet (R) and the sheet (G), further include a sheet (B) having a selective reflection center wavelength λc(B) and a sheet (X) having a selective reflection center wavelength λc(X), the sheet (B) satisfies 430≤λc(B)≤490, the sheet (X) satisfies 430≤λc(X)≤660, and all of Formulas (d-1) to (d-3) are satisfied,
[0030] |λc(X)-λc(R)|≥30nm Formula (d-1)
[0031] |λc(X)-λc(G)|≥30nm Formula (d-2)
[0032] |λc(X)-λc(B)|≥30nm Formula (d-3).
[0033] [5] The identification medium according to [4], wherein the sheet (R), the sheet (G), the sheet (B) and the sheet (X) all satisfy the following formula (e):
[0034] Δλ / λc≤0.10 Formula (e).
[0035] [6] The identification medium according to any one of [1] to [5], wherein the three or more sheets include, in addition to the sheet (R) and the sheet (G), a sheet (B) having a selective reflection center wavelength λc(B), the sheet (B) satisfies 430≤λc(B), and λc(R), λc(G), and λc(B) satisfy the following equations (p-1) and (p-2):
[0036] λc(R)-λc(G)≥70nm Formula (p-1)
[0037] λc(G)-λc(B)≥70nm Formula (p-2).
[0038] [7] The identification medium according to any one of [1] to [6], wherein the thickness of the sheet is 3 μm or more and 7 μm or less.
[0039] [8] The identification medium according to any one of [1] to [7], wherein the average particle size of each of the sheets is 100 μm or less.
[0040] [9] The identification medium according to any one of [1] to [8], wherein the patterned phase difference layer is located closer to the viewing side than the light reflecting layer.
[0041]
[10] The identification medium according to any one of [1] to [9], wherein the patterned phase difference layer is a λ / 4 wave plate or a λ / 2 wave plate.
[0042]
[11] The identification medium according to any one of [1] to
[10] , wherein the light reflecting layer includes a sheet having a reflection band including a region with a wavelength greater than 660 nm as the sheet.
[0043]
[12] The identification medium according to any one of [1] to
[11] , further comprising a light absorbing layer at a position of the light reflecting layer facing the viewing side.
[0044]
[13] The identification medium according to any one of [1] to
[12] , wherein the identification medium has a covering layer located closer to the viewing side than the patterned phase difference layer.
[0045]
[14] The identification medium according to any one of [1] to
[13] , further comprising a mounting member for mounting the identification medium on an article.
[0046]
[15] An article having the identification medium according to any one of [1] to
[14] .
[0047] Effects of the Invention
[0048] According to the present invention, it is possible to provide an identification medium and an article which have a high identification function, can be easily manufactured, and can exhibit high design properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a perspective view schematically showing an example of the identification medium of the present invention.
[0050] Figure 2 It is shown that the cutting along line 1a Figure 1 A longitudinal sectional view of the state of the identification medium shown. DETAILED DESCRIPTION
[0051] Hereinafter, the present invention will be described in detail with reference to examples and embodiments. However, the present invention is not limited to the examples and embodiments described below, and can be arbitrarily modified and implemented without departing from the scope of the claims of the present invention and the scope of their equivalents.
[0052] In the following description, unless otherwise specified, "(meth)acryloyl" refers to a term including "acryloyl", "methacryloyl" and a combination thereof. Similarly, "(thio)epoxy" refers to a term including "epoxy", "thioepoxy" and a combination thereof.
[0053] In the following description, unless otherwise specified, the in-plane delay Re of a certain layer is a value represented by Re=(nx-ny)×d. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the layer (in-plane direction) that gives the maximum refractive index. Ny represents the refractive index in the direction orthogonal to the direction of nx in the above-mentioned in-plane direction of the layer. D represents the thickness of the layer. Unless otherwise specified, the measurement wavelength of the delay is 590nm. The in-plane delay Re can be measured using a phase difference meter ("AxoScan" manufactured by AxoMetrix).
[0054] In the following description, unless otherwise specified, the direction of the slow axis of a certain layer means the direction of the slow axis in the in-plane direction.
[0055] In the following description, unless otherwise specified, the directions of the components "parallel" and "perpendicular" may include errors within the range of, for example, ±4°, preferably ±3°, and more preferably ±1°, within the range not impairing the effects of the present invention.
[0056] In the following description, for the sake of convenience, "right-handed circularly polarized light" and "left-handed circularly polarized light" are defined based on the rotation direction of circularly polarized light when the light emission target is observed from the light emission source. That is, when the light emission target is observed from the light emission source, polarized light whose polarization direction rotates clockwise along the traveling direction of light is defined as right-handed circularly polarized light, and polarized light whose polarization direction rotates in the opposite direction is defined as left-handed circularly polarized light.
[0057] In the following description, unless otherwise specified, the identification medium is described in a state where the display surface is facing upward and the medium is placed horizontally. Therefore, the side where the identification medium is viewed is sometimes referred to as the "upper" side, and the opposite side is sometimes referred to as the "lower" side. For example, one surface of a layer and another surface of a layer, whichever is closer to the display surface of the identification medium, is sometimes referred to as the "upper" surface. In addition, the direction perpendicular to the "upper" and "lower" directions is sometimes referred to as the "horizontal" direction.
[0058] Observation of the identification medium may be observation for the purpose of developing the identification function under specific conditions (observation through a device such as an observer, observation under polarized light, etc.), or may be ordinary observation (observation under natural light with the naked eye without observation through a device such as an observer, etc.). In the following description, unless otherwise specified, observations other than those that clearly indicate observation for the purpose of developing the identification function and those that clearly indicate observation for the purpose of developing the identification function in the context are considered ordinary observations.
[0059] [Overview of Identification Media]
[0060] The identification medium of the present invention comprises a light reflecting layer and a patterned phase difference layer.
[0061] Figure 1 It is a perspective view schematically showing an example of the identification medium of the present invention. Figure 2 It is shown that the cutting along line 1a Figure 1 A longitudinal sectional view of the state of the identification medium shown. Figure 1 and Figure 2 As shown, the identification medium 100 sequentially comprises a light absorbing layer 110, a light reflecting layer 120, a patterned phase difference layer 140 and a coating layer 150, and further comprises a structure having adhesive layers 131 and 132 between the layers. The patterned phase difference layer 140 only covers a partial area of the display surface 160, so the display surface 160 is provided with an area 160A covered by the patterned phase difference layer 140 and an area 160B not covered by the patterned phase difference layer 140.
[0062] The patterned phase difference layer is usually provided at a position closer to the viewing side than the light reflecting layer. Therefore, the display surface of the identification medium is usually the surface on the patterned phase difference layer side of the identification medium.
[0063] In this example, an example is shown in which a flat glass plate without flexibility is used as the coating layer 150, and it is pressed against the light reflecting layer and the patterned phase difference layer 140 to form the identification medium 100. Therefore, the patterned phase difference layer 140 is embedded in the light reflecting layer 120. However, Figure 1 and Figure 2 This is a schematic illustration showing the thickness of the layer relatively large, so that in the actual identification medium, the embedding can be so small that it cannot be seen. Figure 1 and Figure 2 The example shown has a different structure, which can suppress the embedding. For example, the material constituting the coating layer is not limited to an inflexible material such as a glass plate, but can also be a flexible material such as a resin film. In addition, an optically isotropic transparent layer can also be arranged on the same plane as the patterned phase difference layer 140.
[0064] [Patterned phase difference layer]
[0065] The patterned phase difference layer is a layer including an area with a phase difference, and is provided on the identification medium in such a manner that the area with a phase difference occupies a portion of the display surface of the identification medium. In the following description, the portion of the patterned phase difference layer that is different from the area with a phase difference is sometimes referred to as a "phase difference layer".
[0066] In the display surface, the area other than the area occupied by a certain phase difference layer may be an area occupied by another phase difference layer having a different phase difference, an area occupied by an isotropic layer having no phase difference, or an area where none of these exist. Figure 1 and Figure 2 In the example of FIG. 1 , the patterned phase difference layer 140 is a layer occupying only a region 160A which is a part of the display surface.
[0067] As examples of regions with phase difference, there can be cited regions that function as λ / 4 wave plates and regions that function as λ / 2 wave plates. The region that functions as a λ / 4 wave plate is a region whose in-plane delay Re is λ / 4 or a value close to λ / 4 at at least one wavelength λ within the wavelength band in which the light reflecting layer functions. For example, as a region with phase difference, a region with Re of ((λ / 4)×0.6)nm to ((λ / 4)×1.4)nm can be used, and a region with Re of ((λ / 4)×0.8)nm to ((λ / 4)×1.2)nm is preferably used. Similarly, a region that functions as a λ / 2 wave plate is a region with in-plane delay Re of λ / 2 or a value close to λ / 2, such as a region with ((λ / 2)×0.6)nm to ((λ / 2)×1.4)nm, and preferably a region with ((λ / 2)×0.8)nm to ((λ / 2)×1.2)nm. As the wavelength λ, it can be set to 590nm, which is a wavelength near the center of visible light.
[0068] exist Figure 1 and Figure 2 In the example of FIG. 1 , the patterned phase difference layer 140 occupies only a region 160A that is a part of the display surface, and the entire patterned phase difference layer 140 functions as a λ / 4 wave plate.
[0069] A more specific description of examples of the patterned phase difference layer and the materials constituting the patterned phase difference layer will be described later.
[0070] [Light reflecting layer]
[0071] The light reflecting layer in the present invention is a layer that reflects the incident light as circularly polarized light. Specifically, the light reflecting layer is a layer that reflects a certain polarization component as circularly polarized light when non-polarized light containing various polarization components is incident. The light reflecting layer can be a right-handed reflective circular polarizer (i.e., a reflective circular polarizer that selectively reflects the right-handed circular polarization component in the incident light) or a left-handed reflective circular polarizer (i.e., a reflective circular polarizer that selectively reflects the left-handed circular polarization component in the incident light). However, this selective reflection only occurs in the reflection band in the full band, and the reflected proportion depends on the reflectivity of each wavelength of the incident light. Most of the components in the incident light that are not reflected pass through the light reflecting layer, and a part is absorbed by the light reflecting layer.
[0072] The light reflecting layer in the identification medium of the present invention contains three or more sheets of materials with cholesteric regularity. The sheets have a granular structure obtained by crushing a layered structure, and the sheets of materials with cholesteric regularity can be obtained by crushing a layered structure composed of materials with cholesteric regularity. As the layered structure, a cholesteric resin layer can be used. It is preferred to select and use sheets classified into appropriate particle sizes, so that such sheets can be made into particles with a flat structure. In the case where the particles with a flat structure are used as structural elements of the layered structure, the surface that was the main surface before crushing can be easily arranged in the same direction as before crushing. Therefore, in the layered structure containing each sheet, each sheet can show the same optical properties as the cholesteric resin layer before crushing. Specific examples of cholesteric resin layers will be described separately later.
[0073] The average particle size of each of the three or more sheets is preferably 100 μm or less, more preferably 75 μm or less. By having such a small particle size, they will not be viewed as components with different colors on the display surface, and the optical properties of the three or more sheets will cooperate to present a silver pearlescent appearance, and high design properties, which is one of the effects of the present invention, can be obtained. The silver pearlescent appearance mentioned here refers to an appearance formed by uniformly distributing tiny particles with colors other than silver, such as red, green, and blue, and it will present a design that can remind people of pearl luster, unlike a uniform non-color silver appearance.
[0074] On the other hand, the lower limit of the average particle size is preferably 10 μm or more, more preferably 25 μm or more. By having an average particle size above the lower limit, the aspect ratio of the sheet can be made high, and as a result, the sheet can also well show the optical properties of the cholesteric resin layer before pulverization. In addition, the appearance of silver pearlescent feeling different from the uniform non-color silver can be well shown.
[0075] The desired average particle size can be obtained by pulverizing the cholesteric resin layer and then classifying the pulverized product by an appropriate method.
[0076] The average particle size of the sheet can be obtained by measuring the particle size distribution of the sheet using a laser scattering method and obtaining the average particle size from the particle size distribution. As a measuring device for the laser scattering method, a laser diffraction / scattering particle size distribution measuring device (e.g., LA-960 manufactured by Horiba, Ltd.) can be used. In the present invention, unless otherwise specified, the average value such as the average particle size of the sheet can be a volume average.
[0077] The thickness of the sheet is preferably 3 μm or more, and on the other hand, preferably 7 μm or less. By making the thickness above the lower limit, the desired optical effect such as high reflectivity can be well manifested. On the other hand, by making the thickness below the upper limit, the occurrence of poor orientation can be effectively suppressed. In addition, a sheet with a desired high aspect ratio can be easily obtained. The thickness of the sheet usually depends on the thickness of the cholesteric resin layer before pulverization. In the case where the thickness of the cholesteric resin layer before pulverization is uniform, the thickness of the obtained sheet can also be the same uniform value. However, in the case of deviation in thickness, the volume average value can be used as the thickness of the sheet.
[0078] For the aspect ratio of the sheet, the ratio obtained by dividing the average particle size of the sheet by the thickness of the sheet can be used as an index. The ratio is preferably 3 or more, more preferably 5 or more, particularly preferably 10 or more, preferably 40 or less, more preferably 30 or less, and particularly preferably 20 or less.
[0079] Each of the three or more sheets has a specific reflection band. Therefore, each can have a specific half-width Δλ and a selective reflection center wavelength λc of the reflection band. The half-width Δλ is the difference between the maximum wavelength and the minimum wavelength in the wavelength region showing a reflectivity of 50% or more of the peak reflectivity in the reflection band. For example, in the case where the reflectivity of the peak is 40%, the half-width Δλ is the difference between the maximum wavelength and the minimum wavelength in the wavelength region showing a reflectivity of 20% or more. The selective reflection center wavelength λc is the average value of the maximum wavelength and the minimum wavelength (i.e., the value obtained by dividing their total by 2). The units of Δλ and λc can generally be expressed in nm. The values of Δλ and λc of the sheet are generally consistent with the values of Δλ and λc of the cholesteric resin layer before crushing, so the values of Δλ and λc of the cholesteric resin layer can be directly used as Δλ and λc of the sheet.
[0080] In the present invention, the values of Δλ and λc of a specific sheet may be indicated by adding the symbol of the sheet. For example, Δλ(R) and λc(R) respectively indicate the values of Δλ and λc of the sheet (R).
[0081] As the reflectivity at each wavelength of the light reflecting layer and the sheet, the integral reflectivity measured with non-polarized light as the incident light can be used. The integral reflectivity can be measured using an ultraviolet visible spectrophotometer with an integrating sphere (e.g., "UV-Vis770" manufactured by JASCO Corporation). Generally, for sheets, the proportion of light that is diffusely reflected instead of specularly reflected is relatively large, so the measured value of the integral reflectivity can be used as a good indicator.
[0082] In the present invention, among the three or more sheets constituting the light reflecting layer, one is a sheet (R) having a selective reflection center wavelength λc(R), and the other is a sheet (G) having a selective reflection center wavelength λc(G), and the sheet (R) and the sheet (G) satisfy 600nm<λc(R)≤660nm and 500nm≤λc(G)≤600nm. The sheets (R) and (G) are a sheet having a reflection band in the red range and a sheet having a reflection band in the green range, respectively. By making the light reflecting layer include such sheets (R) and (G) and satisfying the other necessary conditions of the present invention, even if a sheet obtained by a wide-band treatment is not used, a light reflecting layer showing the same silver appearance as a cholesteric resin layer subjected to a wide-band treatment can be obtained, and as a result, it is possible to achieve both ease of manufacturing and high designability.
[0083] The light reflecting layer satisfies the following formulae (b-1) and (b-2).
[0084] 0.95≤B(430-490)Ave / G(500-600)Ave≤1.02 Formula (b-1)
[0085] 0.95≤R(600-660)Ave / G(500-600)Ave≤1.02 Formula (b-2)
[0086] Wherein, B(430-490)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 430nm to 490nm, G(500-600)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 500nm to 600nm, and R(600-660)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 600nm to 660nm. The light reflecting layer satisfying formulas (b-1) and (b-2) can be obtained by adjusting the types and mixing ratios of the sheets constituting the light reflecting layer.
[0087] When the light reflecting layer satisfies the formulas (b-1) and (b-2), the light reflecting layer exhibits uniform reflection in a wide wavelength range within the visible light band, and as a result, can exhibit the same silver appearance as the cholesteric resin layer subjected to a wide wavelength band treatment. As a result, it can be obtained by a simple manufacturing method such as mixing sheets that can be manufactured relatively easily, and can also exhibit high design properties.
[0088] One or more of the three or more sheets included in the light reflecting layer satisfies the following formula (a).
[0089] Δλ / λc<0.14Formula (a)
[0090] The upper limit of the value of Δλ / λc is less than 0.14, preferably 0.12 or less, while the lower limit thereof is 0.05 or more, preferably 0.07 or more.
[0091] A sheet having a Δλ / λc value below the above upper limit can be easily obtained even without performing a wide-band treatment on the cholesteric resin layer, and can be manufactured using a conventionally known polymerizable liquid crystal compound. By using a sheet having such a reflection band and satisfying the other necessary conditions of the present invention, the obtained light reflection layer can satisfy formulas (b-1) and (b-2) and present the same silver appearance as the cholesteric resin layer subjected to a wide-band treatment. Therefore, in this manufacturing process, the burden of obtaining special materials and the burden of the process of precisely and multi-staged weak ultraviolet irradiation and temperature increase can be reduced, and manufacturing can be performed at low cost.
[0092] The lower limit of the value of Δλ / λc of each sheet is not particularly limited, but can be, for example, 0.08 or more from the viewpoint of effectively expressing the selective reflection.
[0093] The sheet (R) and the sheet (G) preferably have the same Δλ / λc. The equality of Δλ / λc can be expressed by the absolute value of the difference between them being smaller than a certain level. Specifically, they preferably satisfy the following formula (c).
[0094] |Δλ(R) / λc(R)-Δλ(G) / λc(G)|≤0.01··Eq.
[0095] (c)
[0096] The sheet (R) and sheet (G) contained in the light reflecting layer preferably satisfy formula (c), and the ratio W(R) / W(G) of the weight W(R) of the sheet (R) contained in the light reflecting layer to the weight W(G) of the sheet (G) is a value greater than a certain degree. In this case, W(R) / W(G) is preferably greater than 1.15, more preferably greater than 1.20. By satisfying formula (c) and making W(R) / W(G) greater than the above lower limit, a light reflecting layer satisfying formulas (b-1) and (b-2) can be more easily obtained. The upper limit value of W(R) / W(G) is not particularly limited and can be, for example, less than 1.50.
[0097] In one embodiment, it is preferred that at least one of the three or more types of sheets satisfies the formula (d).
[0098] 0.14≤Δλ / λc≤0.25Formula (d)
[0099] For example, it is possible to use a combination of two of the three sheets that satisfy formula (d) and another sheet that satisfies formula (a). In most cases, the liquid crystal compound as the material of the sheet satisfying formula (d) is disadvantageous in terms of high acquisition cost compared to the liquid crystal compound as the material of the sheet satisfying formula (a). However, by using a sheet mixture containing a sheet satisfying formula (d), it is possible to easily adjust to satisfy formulas (b-1) and (b-2). Therefore, by appropriately combining a sheet satisfying formula (a) with a sheet satisfying formula (d), a combination that appropriately balances high design and low cost and can obtain good results can be achieved.
[0100] Generally, the pitch of the helical structure of the cholesteric resin layer manufactured by performing a broadband treatment is not constant within the layer but has a gradient, and the helical structure with the pitch gradient shows a large Δλ / λc value or a Δλ so wide that the value of Δλ / λc cannot be calculated. In contrast, the pitch of the cholesteric resin layer manufactured without performing a broadband treatment is constant within the layer in most cases, so the Δλ / λc value is a relatively small value of 0.2 or less. In the case of such a relatively small value of the Δλ / λc value, the reflection band becomes relatively narrow, so the color presented by the cholesteric resin layer is monochrome.
[0101] In a certain embodiment, the three or more sheets constituting the light reflection layer may further include a sheet (B). The sheet (B) is a sheet whose selective reflection center wavelength λc(B) satisfies 430≤λc(B)≤490. Furthermore, the three or more sheets constituting the light reflection layer may further include a sheet (X) in addition to the sheet (R), the sheet (G) and the sheet (B). The sheet (X) is a sheet whose selective reflection center wavelength λc(X) satisfies 430≤λc(X)≤660, and satisfies all of the formulas (d-1) to (d-3).
[0102] |λc(X)-λc(R)|≥30nm Formula (d-1)
[0103] |λc(X)-λc(G)|≥30nm Formula (d-2)
[0104] |λc(X)-λc(B)|≥30nm Formula (d-3)
[0105] That is, the selective reflection center wavelength λc(X) of the sheet (X) is located in the visible region and is a wavelength that is different from λc(R), λc(G), and λc(B) by a certain degree or more.
[0106] When the light reflecting layer includes sheet (R), sheet (G), sheet (B) and sheet (X), even if the value of Δλ / λc of each sheet is small, as a whole, a light reflecting layer having a wide reflection band can be easily constituted. The polymerizable liquid crystal compound showing optical properties with a small value of Δλ / λc is relatively cheap, so by satisfying the above-mentioned necessary conditions, a light reflecting layer satisfying formulas (b-1) and (b-2) can be easily constituted with relatively cheap materials. From this point of view, as a more preferred embodiment, sheet (R), sheet (G), sheet (B) and sheet (X) preferably satisfy the following formula (e).
[0107] Δλ / λc≤0.10Formula (e)
[0108] From the viewpoint of obtaining a light reflecting layer satisfying the formulae (b-1) and (b-2), the three or more sheets included in the light reflecting layer preferably have selective reflection center wavelengths λc separated from each other.
[0109] Specifically, the three types of sheets included are preferably sheet (R), sheet (G) and sheet (B), and their selective reflection center wavelengths λc(R), λc(G) and λc(B) are all above 430nm and below 660nm, and satisfy the following formulas (p-1) and (p-2).
[0110] λc(R)-λc(G)≥70nm Formula (p-1)
[0111] λc(G)-λc(B)≥70nm Formula (p-2)
[0112] When λc(R), λc(G) and λc(B) satisfy equations (p-1) and (p-2), a light reflecting layer satisfying equations (b-1) and (b-2) can be more easily obtained by adjusting the ratio of sheets (R), (G) and (B).
[0113] The light reflection layer can include three or more sheets having a reflection band including a region with a wavelength greater than 660 nm. Specifically, in addition to the sheets (R), (G) and (B), a sheet (IR) having a selective reflection center wavelength λc(IR) greater than 660 nm can be included. By including the sheet (IR), the blue shift when observed at an angle can be reduced. In addition, the recognition function using incident light in the infrared region can also be displayed.
[0114] The average value of the integrated reflectivity of the light reflecting layer at 450 to 650 nm is preferably 20% or more, more preferably 30% or more. On the other hand, the theoretical upper limit of the reflectivity is 50%. By having such a high reflectivity, the color caused by reflection is clearly displayed, and an appearance with high recognition function and excellent aesthetics can be obtained. In the present invention, by using the combination of the above-mentioned sheets as the material constituting the light reflecting layer, such a high reflectivity can be obtained even without performing a complicated process such as a broadband process. Figure 1 and Figure 2 As shown in the example, when a layer such as a patterned phase difference layer 140 and a coating layer 150 is provided on the upper side of the light reflection layer 120, the loss of light caused by passing through these layers is generally sufficiently small. In this case, the reflectivity of the light reflection layer can be measured by measuring the reflectivity of the display surface in the identification medium. Alternatively, if the reflectivity of the display surface in the identification medium is 20% or more, it can be said that the reflectivity of the light reflection layer is also 20% or more.
[0115] In addition to the above-mentioned sheet, the light reflecting layer can also include a material for accommodating the sheet to form an integrated material. Specifically, it can include a medium commonly used to make ink. It can also include a diluent for diluting the medium.
[0116] The method for forming the light reflecting layer is not particularly limited, and a known method can be used. For example, a sheet mixed ink containing the sheet and the medium and any other components is prepared, applied to a suitable substrate, and cured by drying, etc., thereby forming the light reflecting layer.
[0117] [Other structural elements]
[0118] The identification medium of the present invention may have any structural elements in addition to the above-mentioned light reflection layer and patterned phase difference layer. Figure 1 and Figure 2 As exemplified in the illustrated identification medium 100 , the identification medium can include a light absorbing layer, a coating layer, and an adhesive layer.
[0119] The light absorbing layer is a layer that absorbs incident light. The light absorbing layer can be a black layer. The material of the light absorbing layer can be any material, and can be, for example, a film colored in black. The light absorbing layer can be arranged on the back side of the light reflecting layer, that is, at a position opposite to the viewing side of the light reflecting layer. In the case where the light reflecting layer is a reflective circular polarizer, most of the incident light that is not reflected is transmitted. When the light absorbing layer is arranged on the back side of the light reflecting layer, the transmitted light is absorbed, and as a result, the effect brought by the reflected light can be seen more clearly. On the other hand, in the case where the light absorbing layer is not arranged on the back side of the light reflecting layer, the back side of the light reflecting layer is viewed, and the effect brought by the reflected light becomes unclear, but a design effect that can make the identification medium into a transparent object can be obtained.
[0120] The coating layer can be arranged at a position closer to the viewing side than the patterned phase difference layer. The coating layer can be a transparent material such as a glass plate or a resin film. By providing the coating layer, the light reflecting layer and the patterned phase difference layer can be protected during use.
[0121] The adhesive layer is a layer for bonding the above-mentioned various layers together. As a material constituting the adhesive layer, a known adhesive having a transparency high enough not to significantly inhibit the transmission of light in the identification medium can be appropriately selected and adopted.
[0122] The identification medium may also have a mounting member. The mounting member is a member that performs a function when the identification medium is mounted on an article. Part or all of the mounting member may also serve as a decorative member. Examples of mounting members include members such as rings, buckles, hooks, wires, chains, ropes, etc. extending from the periphery of the identification medium, and shells such as trays that also serve as decorative members. The mounting member may be directly attached to the light reflecting layer and / or patterned phase difference layer that are necessary structural elements of the identification medium, or may be combined via any other member. The combination of the identification medium and the mounting member may be any of adhesion using an adhesive, adhesion using welding processing, mechanical bonding such as threaded fastening or ligation, and the like. In addition, the mounting member may be the same layer as the above-mentioned adhesive layer, in which case the identification medium may also be bonded to the member of the installation object via this layer.
[0123] [Example of the role of identification medium]
[0124] When the identification medium of the present invention is used, incident light is made incident on the display surface of the identification medium, and is reflected by the light reflecting layer to become reflected light, and the reflected light is observed.
[0125] Examples of light incident on the identification medium include non-polarized light, linearly polarized light, circularly polarized light, and elliptically polarized light. When the incident light is non-polarized light, the identification medium can be used by selectively observing the linear polarization component or circular polarization component of the reflected light when observing the reflected light. As the incident non-polarized light, ordinary ambient light such as sunlight and indoor lighting can be used.
[0126] Selective observation of the linear polarization component of the reflected light can be performed by visually observing the reflected light across the observation linear polarizer. Selective observation of the circular polarization component of the reflected light can be performed by visually observing the reflected light across the observation circular polarizer. In order to avoid obstructing the incidence of ambient light, the observation linear polarizer and the observation circular polarizer can usually be used in a state separated from the identification medium. The lower limit of the separation distance can be appropriately adjusted according to the size of the identification medium and the observation linear polarizer, etc., and can usually be more than 100mm. On the other hand, the upper limit of the separation distance can be appropriately adjusted within the range of being able to observe the reflected light of the identification medium, and can usually be less than 30m.
[0127] In this way, the linear polarizer for observation used at a position separated from the identification medium can be a special product for the method of use of the present invention, or it can be a common linear polarizer for other purposes. For example, most commercially available polarized sunglasses can function as linear polarizers, so such commercially available polarized sunglasses can also be used as linear polarizers for observation. As an example of a circular polarizer for observation, a circular polarizer composed of a combination of a linear polarizer and a phase difference film, and a circular polarizer comprising a cholesteric material layer (for example, a circular polarizer described in International Publication No. 2020 / 121791) can be cited.
[0128] refer to Figure 1 and Figure 2 In the following description, an example is described in which the light reflecting layer 120 is a right-handed reflective circular polarizer (i.e., a reflective circular polarizer that selectively reflects the right-handed circular polarization component in the incident light), the patterned phase difference layer 140 is a layer that functions as a λ / 4 wave plate as a whole, the incident light is non-polarized light, and the outgoing light is observed through the linear polarizer.
[0129] When the non-polarized light incident on the area 160B of the display surface 160 of the identification medium 100 passes through the transparent coating layer 150 and the adhesive layer 132 downward and reaches the light reflecting layer 120, the right-handed circularly polarized component in the reflection band is reflected and travels upward, and the other components pass through the reflection layer 120 and are absorbed by the light absorbing layer. The reflected light is emitted from the area 160B of the display surface 160 as right-handed circularly polarized light with a hue corresponding to the reflection band. When it is observed through a linear polarizer, the linear polarization component of a certain direction in the right-handed circularly polarized light is separated and observed. Even if the azimuth angle of the identification medium 100 is changed (the rotation angle when the identification medium is rotated with the direction perpendicular to the display surface as the axis), the amount of the linear polarization component will not change.
[0130] On the other hand, the non-polarized light incident on the area 160A of the display surface 160 of the identification medium 100 passes through the transparent coating layer 150 and the adhesive layer 132 downward, and then reaches the patterned phase difference layer 140. When the light passes through the patterned phase difference layer 140, its linear polarization component is converted into a circular polarization component, and the circular polarization component is converted into a linear polarization component, but since the original incident light is non-polarized light, the result is that no change in the polarization state occurs. When the light further reaches the light reflecting layer 120, the right-handed circular polarization component within the reflection band is reflected and travels upward, and the other components pass through the reflection layer 120 downward and are absorbed by the light absorbing layer. The reflected light passes through the patterned phase difference layer 140 upward, where it is converted into linear polarized light, and is emitted from the area 160A of the display surface 160 as linear polarized light having a hue corresponding to the reflection band. The polarization direction of the linear polarized light is a certain direction specified according to the slow axis direction of the patterned phase difference layer 140. When the identification medium 100 is observed through a linear polarizer, a phenomenon of brightness change can be observed by changing the azimuth angle of the identification medium 100 and the transmission axis direction of the linear polarizer relative to each other.
[0131] Therefore, by changing the relative angle relationship between the identification medium 100 and the observation linear polarizer, it is possible to observe a phenomenon in which the brightness of the region 160B does not change but only the brightness of the region 160A changes.
[0132] On the other hand, in the case of the identification medium 100 that is not separated by the observation linear polarizer to observe the state after the non-polarized light is incident, the observer observes the circularly polarized light emitted from the area 160B and the linearly polarized light emitted from the area 160A. Since the loss of light when the light passes through the patterned phase difference layer 140 can be extremely small, the brightness of the light emitted from the area 160A and the light emitted from the area 160B is substantially the same. Human vision cannot recognize the difference in the polarization state of these lights, so the observer cannot recognize these differences. In addition, even if the relative angle relationship between the identification medium 100 and the observer changes, the observer cannot recognize the changes based on the change in the polarization state.
[0133] In the method of use of this example, the identification medium of the present invention can bring about a special effect that the change in relative brightness can be observed only when the linear polarizer is separated. Such a special effect cannot be obtained by a copy easily obtained by a conventional printing technique. Therefore, the identification medium of the present invention exerts a high identification function and anti-counterfeiting function in such use.
[0134] By changing the relative brightness, characters, graphics, etc. can be displayed on the display surface. Thus, an image that cannot be observed in normal observation but can be observed only in a specific observation of the identification medium is called a "latent image" of the identification medium.
[0135] The above example is an example when the patterned phase difference layer 140 is a λ / 4 wave plate. When the patterned phase difference layer 140 is a λ / 2 wave plate, the light emitted from the region 160A becomes left-handed circularly polarized light. Therefore, by using a right-handed circular polarizer and a left-handed circular polarizer in combination as observation polarizers, observation can be performed through each observation polarizer and the observation results can be compared, and the identification function of the identification medium can be utilized.
[0136] [Specific examples of cholesteric resin layer]
[0137] Hereinafter, a material having cholesteric regularity as a material of a sheet serving as a structural element of a light reflecting layer and a cholesteric resin layer as an example thereof will be described.
[0138] Cholesteric regularity is a structure in which the molecular axes are arranged in a fixed direction on a certain plane inside the material, and the direction of the molecular axes in the next plane overlapping it is slightly deflected at an angle, and then the angle is further deflected in the next plane, and like this, as it passes through the overlapping planes in sequence, the angle of the molecular axes in the plane gradually deflects (twists). That is, in the case where the molecules inside a certain material layer have cholesteric regularity, the molecules are arranged in a manner in which the molecular axes are in a fixed direction in a certain first plane inside the layer. In the next second plane inside the layer that overlaps with the first plane, the direction of the molecular axes is deflected at a small angle compared to the direction of the molecular axes in the first plane. In the next third plane that further overlaps with the second plane, the direction of the molecular axes is further deflected at an angle compared to the direction of the molecular axes in the second plane. In this way, in the overlapping planes, the angles of the molecular axes in the plane are deflected (twisted) in sequence. A structure in which the direction of the molecular axes is gradually twisted like this is usually a helical structure, which is optically a chiral structure.
[0139] The cholesteric resin layer is a layer obtained by curing a curable liquid crystal compound of a substance exhibiting a cholesteric liquid crystal phase. The cholesteric resin layer can be obtained, for example, by polymerizing a polymerizable liquid crystal compound in a state exhibiting a cholesteric liquid crystal phase. More specifically, a liquid crystal composition containing a polymerizable liquid crystal compound can be coated on a suitable substrate, etc., to form a layer, and the cholesteric liquid crystal phase can be oriented and cured, thereby obtaining a cholesteric resin layer.
[0140] As a polymerizable liquid crystal compound, a photopolymerizable liquid crystal compound is preferred. As a photopolymerizable liquid crystal compound, a photopolymerizable liquid crystal compound that can be polymerized by irradiating active energy rays can be used. As active energy rays, energy rays that can cause the photopolymerizable liquid crystal compound to undergo a polymerization reaction can be used among a wide range of energy rays such as visible light, ultraviolet rays and infrared rays, and ionizing radiation such as ultraviolet rays is particularly preferred. As a photopolymerizable liquid crystal compound suitable for use in a cholesteric liquid crystal composition, a rod-shaped liquid crystal compound having two or more reactive groups in one molecule is particularly preferred, and a compound represented by formula (1) is particularly preferred.
[0141] R 3 -C 3 -D 3 -C 5 -MC 6 -D 4 -C 4 -R 4 Formula (1)
[0142] In formula (1), R 3 and R 4 are reactive groups, each independently selected from (meth)acryloyl, (thio)epoxy, oxetanyl, thietanyl, aziridine, pyrrolyl, vinyl, allyl, fumarate, cinnamoyl, The reactive groups include oxazoline, mercapto, iso(thio)cyanate, amino, hydroxyl, carboxyl and alkoxysilyl groups. When the liquid crystal composition is cured, a liquid crystal composition cured layer having high mechanical strength can be obtained.
[0143] In formula (1), D 3 and D 4 Each independently represents a group selected from the group consisting of a single bond, a linear or branched alkyl group having 1 to 20 carbon atoms, and a linear or branched oxyalkylene group having 1 to 20 carbon atoms.
[0144] In formula (1), C 3 ~C 6Each independently represents a group selected from a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O- and -CH2O-(C=O)-.
[0145] In formula (1), M represents a mesogenic group. Specifically, M represents an unsubstituted or substituted azomethine, azoxy, phenyl, biphenyl, terphenyl, naphthalene, anthracene, benzoate, cyclohexanecarboxylic acid phenyl ester, cyanophenylcyclohexane, cyano substituted phenyl pyrimidine, alkoxy substituted phenyl pyrimidine, phenyl diphenyl ester, A group formed by two to four identical or different skeletons in alkanes, diphenylacetylenes and alkenylcyclohexylbenzonitriles being bonded via bonding groups such as -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O- and -CH2O-(C=O)-.
[0146] Examples of the substituent that the mesogenic group M may have include a halogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cyano group, a nitro group, an -OR 5 、-OC(=O)-R 5 、-C(=O)-OR 5 、-OC(=O)-OR 5 、-NR 5 -C(=O)-R 5 、-C(=O)-NR 5 R 7 or -OC(=O)-NR 5 R 7 Here, R 5 and R 7 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 5 and R 7 In the case of an alkyl group, -O-, -S-, -OC(=O)-, -C(=O)-O-, -OC(=O)-O-, -NR 6 -C(=O)-, -C(=O)-NR 6 -、-NR 6 - or -C(=O)- (excluding the case where two or more -O- are inserted adjacently and two or more -S- are inserted adjacently). 6 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0147] Examples of the substituent in the above-mentioned “alkyl group having 1 to 10 carbon atoms which may have a substituent” include a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkoxy group having 1 to 6 carbon atoms, an alkoxyalkoxy group having 2 to 8 carbon atoms, an alkoxyalkoxyalkoxy group having 3 to 15 carbon atoms, an alkoxycarbonyl group having 2 to 7 carbon atoms, an alkylcarbonyloxy group having 2 to 7 carbon atoms, and an alkoxycarbonyloxy group having 2 to 7 carbon atoms.
[0148] In addition, the above-mentioned rod-shaped liquid crystal compound is preferably an asymmetric structure. Here, the asymmetric structure means that in formula (1), the mesogenic group M is the center, and the relative R 3 -C 3 -D 3 -C 5 -M- vs. -MC 6 -D 4 -C 4 -R 4 , they have different structures. By using a compound with an asymmetric structure as the rod-like liquid crystal compound, the alignment uniformity can be further improved.
[0149] Preferred specific examples of the rod-like liquid crystal compound include the following compounds (B1) to (B14). However, the rod-like liquid crystal compound is not limited to the following compounds.
[0150] [Chemical formula 1]
[0151]
[0152] [Chemical formula 2]
[0153]
[0154] [Chemical formula 3]
[0155]
[0156] When the liquid crystal composition contains the rod-like liquid crystal compound, the liquid crystal composition preferably contains a compound represented by formula (2) as an alignment aid in combination with the rod-like liquid crystal compound.
[0157] R 1 -A 1 -BA 2 -R 2 (2)
[0158] In formula (2), R 1 and R 2Each is independently a group selected from a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched oxyalkylene group having 1 to 20 carbon atoms, a hydrogen atom, a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acryloyl group into which any bonding group may be inserted, an epoxy group, a mercapto group, an isocyanate group, an amino group and a cyano group.
[0159] The above-mentioned alkyl group and alkylene oxide group may be unsubstituted or substituted with one or more halogen atoms. Furthermore, the above-mentioned halogen atom, hydroxyl group, carboxyl group, (meth)acryloyl group, epoxy group, mercapto group, isocyanate group, amino group and cyano group may be bonded to the alkyl group and alkylene oxide group having 1 to 2 carbon atoms.
[0160] As R 1 and R 2 Preferred examples of the group include a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, an amino group and a cyano group.
[0161] In addition, R 1 and R 2 At least one of is preferably a reactive group. 1 and R 2 At least one of the above-mentioned reactive groups has a reactive group, and the compound represented by the above-mentioned formula (2) is fixed in the liquid crystal composition cured layer during curing, and a more solid layer can be formed. Here, the reactive group can include, for example, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, and an amino group.
[0162] In formula (2), A 1 and A 2 Each independently represents a group selected from 1,4-phenylene, 1,4-cyclohexylene, cyclohexene-1,4-ene, 4,4′-biphenylene, 4,4′-bicyclohexylene and 2,6-naphthylene. The above-mentioned 1,4-phenylene, 1,4-cyclohexylene, cyclohexene-1,4-ene, 4,4′-biphenylene, 4,4′-bicyclohexylene and 2,6-naphthylene may be unsubstituted or substituted with one or more halogen atoms, hydroxyl groups, carboxyl groups, cyano groups, amino groups, alkyl groups having 1 to 10 carbon atoms, halogenated alkyl groups and the like. In A 1 and A 2 When there are two or more substituents in each of the groups, these substituents may be the same or different.
[0163] As A 1 and A 2 Particularly preferred groups include groups selected from 1,4-phenylene, 4,4'-biphenylene and 2,6-naphthylene. These aromatic ring skeletons are relatively rigid compared to alicyclic skeletons, have high affinity with the mesogen of the rod-like liquid crystal compound, and further improve the alignment uniformity.
[0164] In formula (2), B is selected from a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O- and -CH2O-(C=O)-.
[0165] Particularly preferred groups for B include a single bond, -O-(C=O)-, and -CH=NN=CH-.
[0166] Particularly preferred specific examples of the compound represented by formula (2) include the following compounds (A1) to (A10). These may be used alone or in combination of two or more at any ratio.
[0167] [Chemical formula 4]
[0168]
[0169] In the above compound (A3), "*" represents a chiral center.
[0170] The weight ratio represented by (total weight of the compounds represented by formula (2)) / (total weight of the rod-like liquid crystal compounds) is preferably 0.001 or more, more preferably 0.01 or more, further preferably 0.05 or more, preferably 1 or less, and more preferably 0.65 or less. By making the above-mentioned weight ratio above the above-mentioned lower limit, the orientation uniformity can be improved in the layer of the liquid crystal composition. In addition, by making the above-mentioned weight ratio below the upper limit, the orientation uniformity can be improved. In addition, the stability of the liquid crystal phase of the liquid crystal composition can be improved. Furthermore, the refractive index anisotropy Δn of the liquid crystal composition can be improved, so that a liquid crystal composition cured layer having desired optical properties such as selective reflection performance of circularly polarized light can be stably obtained. Here, the total weight of the compounds represented by formula (2) represents its weight when only one compound represented by formula (2) is used, and represents the total weight when two or more are used. Similarly, the total weight of the rod-like liquid crystal compounds represents its weight when only one rod-like liquid crystal compound is used, and represents the total weight when two or more are used.
[0171] In addition, when the compound represented by formula (2) and a rod-shaped liquid crystal compound are used in combination, the molecular weight of the compound represented by formula (2) is preferably less than 600, and the molecular weight of the rod-shaped liquid crystal compound is preferably greater than 600. As a result, the compound represented by formula (2) can enter the gap between the rod-shaped liquid crystal compound having a larger molecular weight than the compound, thereby improving the alignment uniformity.
[0172] The liquid crystal composition for forming a cholesteric resin layer can also include any component constituting the cholesteric resin layer, and a solvent for facilitating the processing of the liquid crystal composition. As examples of any component, a chiral agent, a polymerization initiator, and a surfactant can be cited. As specific examples of any component and solvent, and a liquid crystal composition, those described in Japanese Patent Publication No. 2019-188740 can be cited.
[0173] In the present invention, it is preferred that all three or more sheets constituting the light reflecting layer are solidified products of liquid crystal compositions, and the liquid crystal compositions contain common polymerizable liquid crystal compounds. Specifically, for all cholesteric resin layers used to obtain three or more sheets, it is preferred that the liquid crystal compositions used to manufacture them contain any one of the above-mentioned rod-shaped liquid crystal compounds as polymerizable liquid crystal compounds. In addition, it is more preferred that the liquid crystal compositions of all sheets have the same composition except for the proportion of the chiral agent, and the reflection band is adjusted according to the proportion of the chiral agent. By using a sheet with a common composition like this, a good color can be obtained. In addition, the deterioration over time during the use of the identification medium can be made more uniform, so that the reduction in aesthetics and the reduction in identification function accompanied by degradation over time can be suppressed.
[0174] The method for forming a cholesteric resin layer using a liquid crystal composition is not particularly limited and can be performed by a known method. Specifically, the liquid crystal composition is coated on the surface of a support film having an orientation-limiting force, an orientation treatment is performed as required, and further, the polymerizable material constituting the liquid crystal composition is cured by an appropriate method such as ultraviolet irradiation, thereby forming a cholesteric resin layer.
[0175] [Specific example of patterned phase difference layer]
[0176] The patterned phase difference layer is a layer including a region having a phase difference. The region having a phase difference occupies a part of the display surface area in the identification medium.
[0177] Examples of the retardation layer (the portion of the patterned retardation layer having a retardation region) include the region functioning as a λ / 4 wave plate and the region functioning as a λ / 2 wave plate exemplified above.
[0178] As the material constituting the phase difference layer, various solid materials with optical anisotropy can be cited. As an example thereof, a stretched film obtained by stretching a transparent material can be cited. More specifically, a film that is stretched by stretching an optically isotropic film to impart in-plane retardation Re that can function as a λ / 4 wave plate or a λ / 2 wave plate can be cited. From the viewpoint of being relatively cheap, easily imparting a desired value of Re, and being formed into a desired arbitrary shape, a stretched film is preferred.
[0179] As another example of a material constituting a phase difference layer, a solidified material of a liquid crystal compound can be cited. Specifically, it is a layer obtained by curing a liquid crystal compound oriented to present a liquid crystal state that can function as a λ / 4 wave plate or a λ / 2 wave plate. As examples of such layers and methods of manufacturing them, those described in International Publication No. 2019 / 116995 can be cited. The solidified material of a liquid crystal compound can easily form a film having a different phase difference between a certain part and other parts, so when it is required to form a film as a patterned phase difference layer, the solidified material of a liquid crystal compound is particularly preferred.
[0180] [thing]
[0181] The article of the present invention has the above-mentioned identification medium of the present invention.
[0182] Examples of articles include clothing, shoes, hats, jewelry, jewellery, daily necessities and other articles. The article of the present invention can have an identification function by having an identification medium. By having this identification function, it is possible to identify that the identification medium and the article are not counterfeits but genuine products. In addition, the identification medium can give a design effect to the article. The identification medium can be set on the article as a decoration, component or accessory of an article such as a label, ornament, badge, sticker, etc.
[0183] In addition to the identification medium of the present invention, the article of the present invention can also have a polarizer observer. As the polarizer observer, there can be cited a device having an observation polarizer such as the above-mentioned observation linear polarizer or observation circular polarizer, and being arranged on the article in a manner that the identification medium can be observed across the observation polarizer. The polarizer observer can be in the shape of a label, for example, and can be arranged on the article body by a rope or the like. In this way, by having a polarizer observer in addition to the identification medium, it is possible to make ordinary article users easily identify the identification medium.
[0184] Example
[0185] Hereinafter, the present invention will be described in detail with reference to the examples. However, the present invention is not limited to the examples shown below, and can be arbitrarily modified and implemented without departing from the scope of the claims of the present invention and the scope of their equivalents.
[0186] In the following description, "%" and "parts" indicating amounts are based on weight unless otherwise specified. In addition, the following operations are performed in an atmosphere of normal temperature and pressure unless otherwise specified.
[0187] In the following description, unless otherwise specified, a commercially available adhesive is a transparent adhesive tape “LUCIACSCS9621T” (thickness 25 μm, visible light transmittance 90% or more, in-plane retardation 3 nm or less) manufactured by Nitto Denko Corporation.
[0188] In the following description, the word "CLC" may be used as an abbreviation to represent a cholesteric resin layer or a sheet obtained by pulverizing the cholesteric resin layer.
[0189] [Method for measuring reflectivity of CLC layer]
[0190] The support film was peeled off from the multilayer member to obtain a CLC layer. The reflectance of the CLC layer when non-polarized light (wavelength 300 nm to 950 nm) was measured using an ultraviolet visible spectrophotometer with an integrating sphere ("UV-Vis770" manufactured by JASCO Corporation).
[0191] [Method for measuring the rotation direction of circularly polarized light reflected by the CLC layer]
[0192] The CLC layer is irradiated with non-polarized light, and the reflected light is observed through a right-handed circular polarizing plate and a left-handed circular polarizing plate to determine whether the rotation direction of the circularly polarized light as the reflected light is right-handed or left-handed.
[0193] [Measurement method of in-plane retardation and slow axis direction]
[0194] The in-plane retardation and the slow axis direction were measured at a measurement wavelength of 550 nm using a phase difference meter (“Axoscan” manufactured by AxoMetrix Corporation).
[0195] [Measurement of average particle size of tablets]
[0196] The particle size distribution of the sheet was measured by a laser scattering method, and the average particle size was measured from the particle size distribution. As a measuring device, a laser diffraction / scattering particle size distribution measuring apparatus (manufactured by Horiba, Ltd., LA-960) was used.
[0197] [Manufacturing Example 1. Manufacture of a Broadband Red Reflecting CLC Layer]
[0198] (P1-1. Liquid crystal composition)
[0199] A liquid crystal composition is prepared by mixing 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X1), 25 parts of a photopolymerizable non-liquid crystal compound represented by the following formula (X2), 7 parts of a chiral agent ("LC756" manufactured by BASF), 5 parts of a photopolymerization initiator ("Irgacure907" manufactured by Ciba Specialty Chemicals Japan Ltd.), 0.15 parts of a surfactant ("S-420" manufactured by AGC Seimi Chemical Co., Ltd.), and 320 parts of cyclopentanone as a solvent.
[0200] [Chemical formula 5]
[0201]
[0202] (P1-2. Multilayer structure including CLC layer)
[0203] As a supporting film, a long polyethylene terephthalate film ("A4100" manufactured by Toyobo Co., Ltd.; thickness 100 μm) was prepared. The supporting film was attached to the delivery portion of a film conveying device, and the following operation was performed while conveying the supporting film in the longitudinal direction.
[0204] The surface of the support film was subjected to a rubbing treatment in a longitudinal direction parallel to the conveying direction. Next, the liquid crystal composition obtained in (P1-1) was applied to the surface of the support film after the rubbing treatment using a die coater to form a layer of the liquid crystal composition. The layer of the liquid crystal composition was subjected to an orientation treatment by heating at 120°C for 5 minutes to orient the liquid crystal composition to exhibit a cholesteric liquid crystal phase. Thereafter, the layer of the liquid crystal composition was irradiated with 830 mJ / cm 2 The layer of the liquid crystal composition was cured by applying ultraviolet rays. Thus, a multilayer structure (CLC_Ra) having a support film and a red reflective CLC layer (thickness 3 μm) having a circularly polarized light separation function was obtained.
[0205] The reflectivity of the CLC layer of the multilayer component (CLC_Ra) was measured by the above-mentioned measuring method. The measuring result showed that the reflectivity of the CLC layer at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.15. In addition, the rotation direction of the circularly polarized light reflected by the CLC layer was measured by the above-mentioned measuring method, and the result was right-handed. Visual observation under natural light showed that the CLC layer was red.
[0206] [Manufacturing Example 2. Manufacture of a Broadband Blue Reflecting CLC Layer]
[0207] The amount of chiral agent ("LC756" manufactured by BASF) was changed to 9.8 parts. In addition, a multilayer component (CLC_Ba) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1. Although the coating thickness of the liquid crystal composition was set to a CLC layer thickness of 7 μm, poor orientation and turbidity often occurred in this case, so this manufacturing example adopts an example in which the thickness of the CLC layer is 3 μm. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results are: the reflectivity at the selective reflection center wavelength λc is 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc is Δλ / λc=0.15. Visual observation under natural light showed that the CLC layer was blue.
[0208] [Manufacturing Example 3. Manufacture of Mid-band Red Reflective CLC Layer]
[0209] A multilayer component (CLC_Rb) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 1, except that 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X3) were used instead of 100 parts of a liquid crystal compound represented by the formula (X1), and the amount of a chiral agent ("LC756" manufactured by BASF) was changed to 6.5 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measuring method. The measured results showed that the reflectivity at the selected reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. In addition, the rotation direction of the circularly polarized light reflected by the CLC layer was measured by the above-mentioned measuring method, and the result was right-handed. Visual observation under natural light showed that the CLC layer was red.
[0210] [Chemical formula 6]
[0211]
[0212] [Manufacturing Example 4. Manufacture of a Mid-Band Green Reflecting CLC Layer]
[0213] A multilayer component (CLC_Gb) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 3 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 8.2 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. Visual observation under natural light showed that the CLC layer was green.
[0214] [Manufacturing Example 5. Manufacture of a Mid-Band Blue Reflecting CLC Layer]
[0215] A multilayer component (CLC_Bb) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 3 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 10.2 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. Visual observation under natural light showed that the CLC layer was blue.
[0216] [Manufacturing Example 6. Manufacture of a mid-band infrared reflective CLC layer]
[0217] A multilayer component (CLC_IRb) having a supporting film and a CLC layer (thickness 3 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 3 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 5.2 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.12. Visual observation under natural light showed that the CLC layer was blue.
[0218] [Manufacturing Example 7. Manufacture of a narrow-band red reflective CLC layer]
[0219] (P7-1. Liquid crystal composition)
[0220] A liquid crystal composition was prepared by mixing 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X4), 5.7 parts of a chiral agent ("LC756" manufactured by BASF), 5 parts of a photopolymerization initiator ("Irgacure907" manufactured by Ciba Specialty Chemicals Japan Ltd.), 0.15 parts of a surfactant ("S-420" manufactured by AGC Seimi Chemical Co., Ltd.), and 320 parts of cyclopentanone as a solvent.
[0221] (P7-2. Multilayer structure including CLC layer)
[0222] As a liquid crystal composition, the liquid crystal composition obtained in (P7-1) is used instead of the liquid crystal composition prepared in (P1-1) of Manufacturing Example 1, and the coating thickness of the liquid crystal composition is changed. In addition, a multilayer component (CLC_Rc) having a supporting film and a CLC layer (thickness 5μm) having a circularly polarized light separation function is manufactured by the same method as Manufacturing Example 1. Although the coating thickness of the liquid crystal composition of Manufacturing Example 1 is not changed and the thickness of the CLC layer is set to 3μm, the reflectivity is as low as 35% in this case, and sufficient optical properties cannot be obtained. Therefore, this manufacturing example adopts an example in which the thickness of the CLC layer is set to 5μm. The reflectivity of the CLC layer of the multilayer component is measured by the above-mentioned measurement method. The measurement results are: the reflectivity at the selective reflection center wavelength λc is 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc is Δλ / λc=0.09. In addition, the rotation direction of the circularly polarized light reflected by the CLC layer is measured by the above-mentioned measurement method, and the result is right-handed. Visual observation under natural light revealed that the CLC layer was red.
[0223] [Chemical formula 7]
[0224]
[0225] [Manufacturing Example 8. Manufacture of a Narrow-Band Green Reflective CLC Layer]
[0226] A multilayer component (CLC_Gc) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 7 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 6.9 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. Visual observation under natural light showed that the CLC layer was green.
[0227] [Manufacturing Example 9. Manufacture of a narrow-band blue reflective CLC layer]
[0228] A multilayer component (CLC_Bc) having a supporting film and a CLC layer (thickness 5 μm) having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 7 except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 8.1 parts. The reflectivity of the CLC layer of the multilayer component was measured by the above-mentioned measurement method. The measurement results showed that the reflectivity at the selective reflection center wavelength λc was 50%, and the ratio of the half-peak width Δλ of the reflection band to the above-mentioned λc was Δλ / λc=0.09. Visual observation under natural light showed that the CLC layer was blue.
[0229] [Manufacturing Example 10. Manufacture of a Broadband Silver Reflective CLC Layer]
[0230] (P10-1. Liquid crystal composition)
[0231] A liquid crystal composition was prepared by the same method as in (P1-1) of Production Example 1, except that the amount of the chiral agent ("LC756" manufactured by BASF) was changed to 8.2 parts.
[0232] (P10-2. CLC layer contains multi-layer components)
[0233] As a supporting film, a long polyethylene terephthalate film ("A4100" manufactured by Toyobo Co., Ltd.; thickness 100 μm) was prepared. The supporting film was attached to the delivery portion of a film conveying device, and the following operation was performed while conveying the supporting film in the longitudinal direction.
[0234] The surface of the support film is subjected to a friction treatment along the length direction parallel to the conveying direction. Next, the liquid crystal composition obtained in (P10-1) is coated on the surface of the support film after the friction treatment using a die coater to form a layer of the liquid crystal composition. The layer of the liquid crystal composition is subjected to an orientation treatment by heating at 120°C for 5 minutes to orient the liquid crystal composition to exhibit a cholesteric liquid crystal phase. Thereafter, the layer of the liquid crystal composition is subjected to a broadband treatment. In the broadband treatment, 5 mJ / cm 2 ~30mJ / cm 2 The liquid crystal composition layer was irradiated with weak ultraviolet light and heated to 100°C to 120°C, thereby controlling the wavelength range in which the circularly polarized light separation function can be exerted to have the desired wavelength width. 2 The layer of the liquid crystal composition was cured by ultraviolet light. Thus, a multilayer structure (CLC_S) having a support film and a broadband silver reflective CLC layer (thickness 5 μm) having a circularly polarized light separation function was obtained.
[0235] The reflectivity of the CLC layer of the multilayer component (CLC_S) was measured by the above-mentioned measurement method. The measurement results show that the CLC layer shows a roughly uniform reflection in the entire visible light region (450nm to 650nm), so it is impossible to determine the half-peak width Δλ of the reflection band and the selective reflection center wavelength λc, and it is impossible to calculate the ratio Δλ / λc. In addition, the rotation direction of the circularly polarized light reflected by the CLC layer was measured by the above-mentioned measurement method, and the result was right-handed. Visual observation under natural light showed that the CLC layer was silver.
[0236] [Manufacturing Example 11. Manufacture of CLC Sheet_Ra]
[0237] The support film was peeled off from the multilayer member (CLC_Ra) obtained in Production Example 1, and the obtained CLC layer was pulverized to obtain a CLC layer flake. The obtained flake was classified using a sieve to obtain a CLC flake_Ra having an average particle size of 25 μm.
[0238] [Manufacturing Examples 12 to 16, 20 to 22 and 27. Manufacture of CLC Sheet]
[0239] Various sheets shown in Table 1 were obtained by the same method as in Production Example 11 except that the multilayered members shown in Table 1 were used among the multilayered members obtained in Production Examples 2 to 10.
[0240] [Manufacturing Examples 17 to 19 and 23 to 26. Manufacture of CLC Sheets]
[0241] Various flakes having an average particle size of 75 μm shown in Table 1 were obtained by the same method as in Production Example 11 except that the multilayered members shown in Table 1 among the multilayered members obtained in Production Examples 1 to 10 were used and the sieve used for classification was changed.
[0242] [Table 1]
[0243] Table 1
[0244]
[0245] [Production Example 28. λ / 4 stretched resin film]
[0246] A resin film formed of a thermoplastic norbornene resin ("ZEONOR FILM" manufactured by Zeonor Co., Ltd. of Japan; a film manufactured by extrusion molding. Unstretched product) was prepared. The resin film was stretched in one direction at a stretching temperature of 130°C to obtain a phase difference film (R1) having an in-plane retardation capable of functioning as a 1 / 4 wave plate. The phase difference film (R1) had a thickness of 48 μm and an in-plane retardation of 144 nm. The resin film was punched out with a craft punch to obtain a λ / 4 stretched resin film having a star shape used as a phase difference layer.
[0247] [Production Example 29: λ / 2 stretched resin film]
[0248] Two sheets of the λ / 4 stretched resin film obtained in Production Example 28 were bonded together by an adhesive ("CS9621T" manufactured by Nitto Denko Corporation). When bonding, the two sheets of the resin film were aligned so that the slow axes thereof were in the same direction. The multi-resin film was punched out with a punch to obtain a λ / 2 stretched resin film having a star shape used as a phase difference layer.
[0249] [Example 1]
[0250] (1-1. Tablet mixture)
[0251] The CLC sheet_Rb, CLC sheet_Gb, and CLC sheet_Bb obtained in the above-mentioned manufacturing example were mixed in the weight ratio shown in Table 2 to obtain a CLC sheet mixture.
[0252] (1-2. Production of Light Reflecting Layer)
[0253] 10 parts of the CLC flake mixture obtained in (1-1), 85 parts of screen printing ink ("No. 2500 medium" manufactured by Jujo Chemical Industry Co., Ltd.), and 5 parts of a special diluent for the screen printing ink (Tetron standard solvent) were mixed to obtain a CLC flake mixed ink. The obtained ink was applied to a light absorbing layer (Toyobo, black PET film, 100 μm thick) using a notch wheel coater and dried to form a light reflecting layer 1 with a thickness of 40 μm.
[0254] (1-3. Reflection spectrum measurement of light reflecting layer)
[0255] The reflectance spectrum of the light reflecting layer 1 obtained in (1-2) was measured by an ultraviolet visible spectrophotometer ("UV-Vis770" manufactured by JASCO Corporation) using an integrating sphere. Based on the obtained results, the average values of the integrated reflectances B (430-490) Ave, G (500-600) Ave, and R (600-660) Ave in the blue region (B), green region (G), and red region (R) in the visible light region were obtained, and their ratios R / G and B / G were further calculated. The results are shown in Table 2.
[0256] (1-4. Visual observation of light reflecting layer)
[0257] The light reflecting layer 1 obtained in (1-2) was visually observed to evaluate the color, the degree of glare, and the presence or absence of color change when the observation angle was changed from the front to an oblique angle.
[0258] (1-5. Color measurement of light reflecting layer)
[0259] The light reflecting layer 1 obtained in (1-2) was measured for a* value and b* value as color indices under a D65 light source in accordance with the method of JIS Z 8781-4.
[0260] (1-6. Reflectivity of light reflecting layer)
[0261] The reflectance when non-polarized light (wavelength 430 nm to 660 nm) was incident on the surface of the light reflecting layer 1 was measured using an ultraviolet visible spectrophotometer with an integrating sphere ("UV-Vis770" manufactured by JASCO Corporation), and the average reflectance at wavelengths of 430 nm to 660 nm was determined.
[0262] (1-7. Production of Identification Medium (1))
[0263] The star-shaped λ / 4 stretched resin film obtained in Production Example 28 was bonded as a patterned phase difference layer via an adhesive so as to cover a part of the surface of the light reflecting layer 1 obtained in (1-2). Furthermore, a glass plate with a thickness of 0.4 mm as a coating layer was bonded via an adhesive so as to cover the surface of the light reflecting layer 1 and the surface of the star-shaped λ / 4 stretched resin film. Figure 1 and Figure 2 The schematic structure of the identification medium (1) is shown in FIG. Figure 1 and Figure 2As shown, the identification medium (1) 100 has the following structure: it has a light absorption layer 110, a light reflection layer 120, a patterned phase difference layer 140 and a coating layer 150 in sequence, and also has adhesive layers 131 and 132 between the layers. On its display surface 160, there are provided an area 160A covered by the patterned phase difference layer 140 and an area 160B not covered by the patterned phase difference layer 140.
[0264] (1-8. Observation of identification medium (1))
[0265] The identification medium (1) is kept horizontally placed, and the azimuth angle of the identification medium (1) is rotated 360 degrees, and the observer observes the identification medium (1) from a vertical direction. The observation is performed with the naked eye and through a linear polarizer of polarized sunglasses. The observation is performed in a bright room with a fluorescent lamp as a light source.
[0266] In naked eye observation, a non-color silver pearlescent appearance generated by reflection of the light reflecting layer 120 is observed in the display surface 160. The patterned phase difference layer 140 is observed as a transparent member, and its star-shaped shape is hardly observed. The difference in brightness between the area 160A and the area 160B in the display surface 160 is not observed, and it does not change with rotation.
[0267] When observing through polarized sunglasses, the region 160A is viewed in a star-like shape. The difference in brightness between the region 160A and the region 160B changes according to the rotation.
[0268] (1-9. Contrast measurement of identification medium (1))
[0269] The identification medium (1) was kept in a horizontal position, and the azimuth angle of the identification medium (1) was rotated 360° under a D65 light source. The areas 160A and 160B of the display surface were observed from the vertical direction through the linear polarizer of the same polarized sunglasses as used in (1-8), and the L* values of each area were measured under the photometric condition SCE using a spectrophotometer CM-700d manufactured by Konica Minolta. The L* value of area 160A changes with the change of the azimuth angle of the identification medium. The difference ΔL* value between the L* of area 160A and the L* of area 160B was obtained in the observation at the azimuth angle at which the difference between them was the largest. The ΔL* value was the largest when area 160A became the darkest or the brightest. The results are shown in Table 3.
[0270] (1-10. Reflectivity)
[0271] The reflectance when non-polarized light (wavelength 430nm to 660nm) was incident on the area 160B of the display surface 160 of the identification medium (1) was measured using an ultraviolet-visible spectrophotometer with an integrating sphere ("UV-Vis770" manufactured by JASCO Corporation), and the average reflectance at wavelengths of 430nm to 660nm was obtained. The results are shown in Table 3.
[0272] [Examples 2 to 6 and Comparative Examples 1 to 4]
[0273] Except for changing the type and ratio of the CLC sheets mixed in (1-1) as shown in Table 2, light reflecting layers 2 to 10 with a thickness of 40 μm were obtained by the same method as in Example 1, and identification media (2) to (10) were obtained using them and evaluated.
[0274] In the observation of the identification medium (corresponding to (1-8) of Example 1), the same results as those of Example 1 were obtained for the identification media of Examples 2 to 6. That is, in the naked eye observation, a non-color silver pearlescent appearance generated by the reflection of the light reflection layer 120 was observed in the display surface 160. The patterned phase difference layer 140 was observed as a transparent member, and its star-shaped shape was almost invisible. The difference in brightness between the area 160A and the area 160B in the display surface 160 was not observed, and it did not change according to the rotation.
[0275] In the case of the identification media of Comparative Examples 1 to 4, a light yellow, light blue, or light red appearance caused by the reflection of the light reflecting layer 120 is observed in the display surface 160 when observed with the naked eye. The patterned phase difference layer 140 is observed as a transparent member, and its star-shaped shape is hardly observed. The difference in brightness between the area 160A and the area 160B in the display surface 160 is not observed, and it does not change with rotation.
[0276] When observed through polarized sunglasses, the identification media of Examples 2 to 6 and Comparative Examples 1 to 4 all showed a star-shaped shape in region 160A. The difference in brightness between region 160A and region 160B changed according to the rotation.
[0277] Other evaluation results are shown in Tables 2 and 3. In particular, the ΔL* value of the contrast measurement in the Examples was significantly higher than that in the Comparative Examples.
[0278] [Examples 7 to 12]
[0279] Identification media (11) to (16) were obtained and evaluated in the same manner as in Examples 1 to 6 except for the following changes.
[0280] As the patterned phase difference layer in (1-6), the star-shaped λ / 2 stretched resin film obtained in Production Example 29 was used instead of the star-shaped λ / 4 stretched resin film obtained in Production Example 28.
[0281] In the observation of the identification medium of (1-8) and (1-9), a circular polarizer was used instead of the linear polarizer of the polarized sunglasses. As the circular polarizer, both the observation using a right-hand circular polarizer and the observation using a left-hand circular polarizer were used, and the observation results were compared. When calculating the ΔL* value, the difference between the L* values of the observation using the right-hand circular polarizer and the observation using the left-hand circular polarizer in the observation in which the difference between the L* of the region 160A and the L* of the region 160B was the largest was calculated as the ΔL* value.
[0282] In the observation of the identification medium (corresponding to (1-8) of Example 1), the following results were obtained for any of the identification media. That is, in the naked eye observation, the non-color silver pearlescent appearance produced by the reflection of the light reflecting layer 120 is observed in the display surface 160. The patterned phase difference layer 140 is observed as a transparent component, and its star shape is almost invisible. The difference in brightness between area 160A and area 160B in the display surface 160 is not observed, and it does not change according to the rotation. In the observation through the circular polarizer, the star shape of area 160A is observed. The difference in brightness between area 160A and area 160B is that area 160A is relatively bright when one of the right-handed circular polarizer and the left-handed circular polarizer is used, and area 160B is relatively bright when the other is used.
[0283] Other evaluation results are shown in Tables 2 and 3.
[0284] [Comparative Example 5]
[0285] A light reflecting layer 8 having a thickness of 40 μm and an identification medium ( 11 ) were obtained and evaluated in the same manner as in Example 1 except that the type of CLC sheet mixed in (1-1) was only CLC sheet_S.
[0286] In the observation of the identification medium (corresponding to (1-8) of Example 1), the following results were obtained. That is, in the observation with the naked eye, a silver appearance with a pearly feel that is not a non-color is observed in the display surface 160 due to the reflection of the light reflecting layer 120. The patterned phase difference layer 140 is observed as a transparent component, and its star shape is almost invisible. The difference in brightness between the area 160A and the area 160B in the display surface 160 is not observed, and it does not change according to the rotation. In the observation through polarized sunglasses, the star shape of the area 160A is observed. The difference in brightness between the area 160A and the area 160B changes according to the rotation.
[0287] Other evaluation results are shown in Tables 2 and 3.
[0288] [Table 2]
[0289] Table 2
[0290]
[0291] In Table 2, the type of the sheet used is indicated by the end of the symbol of each sheet. For example, "b" in the R column indicates that a CLC sheet_Rb is used.
[0292] [Table 3]
[0293] Table 3
[0294]
[0295] According to the results shown in Table 3, in the identification medium of the present invention, the appearance of the light reflection layer is silver with a pearly feel, and each sheet monomer exerts an unexpectedly beautiful design. In addition, the visibility of the latent image embedded by the phase difference pattern that cannot be viewed with the naked eye can also be clearly viewed due to the large light-dark contrast difference. The latent image visibility is equivalent to the latent image visibility of the previously known case of using a silver CLC layer obtained by broadband processing, so it can be said that the identification medium of the present invention can show the same latent image visibility even without the complicated processing for broadbandization.
[0296] Description of Reference Numerals
[0297] 100: Identify the medium
[0298] 110: Light absorption layer
[0299] 120: Light reflection layer
[0300] 131: Adhesive layer
[0301] 132: Adhesive layer
[0302] 140: Patterned phase difference layer
[0303] 150: Coating layer
[0304] 160: Display surface
[0305] 160A: Area
[0306] 160B: Area
Claims
1. An identification medium comprising a light reflecting layer and a patterned phase difference layer, The light reflecting layer is a layer that reflects incident light as circularly polarized light. The patterned phase difference layer is a layer including a region having a phase difference, and the patterned phase difference layer is a layer provided on the identification medium in such a manner that the region having a phase difference occupies a part of the display surface of the identification medium. The light reflecting layer comprises three or more sheets of materials having cholesteric regularity, One or more of the three or more sheets satisfies formula (a), Δλ / λc<0.14 Formula (a) Wherein, Δλ is the half-peak width of the reflection band of the sheet, λc is the selective reflection center wavelength of the sheet, Among the three or more sheets, one is a sheet (R) having a selective reflection center wavelength λc(R), and the other is a sheet (G) having a selective reflection center wavelength λc(G), and the sheet (R) and the sheet (G) satisfy 600nm<λc(R)≤660nm and 500nm≤λc(G)≤600nm, The light reflecting layer satisfies the following formulas (b-1) to (b-2): 0.95≤B(430-490)AveG(500-600)Ave≤1.02 Formula (b-1) 0.95≤R(600-660)Ave / G(500-600)Ave≤1.02 Formula (b-2) In the formula, B(430-490)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths from 430 nm to 490 nm, G(500-600)Ave is the average value of the integrated reflectivity of the light reflecting layer at a wavelength of 500nm to 600nm, R(600-660)Ave is the average value of the integrated reflectivity of the light reflecting layer at wavelengths of 600nm to 660nm, The average value of the integrated reflectivity of the light reflecting layer at 430 to 660 nm is greater than 20%.
2. The identification medium according to claim 1, in, The sheet (R) and the sheet (G) satisfy the following formula (c), |Δλ(R) / λc(R)-Δλ(G) / λc(G)|≤0.01··Formula (c) In the formula, Δλ(R) is the half-peak width of the reflection band of the sheet (R), Δλ(G) is the half-peak width of the reflection band of the sheet (G), A ratio W(R) / W(G) of a weight W(R) of the sheet (R) to a weight W(G) of the sheet (G) included in the light reflecting layer is 1.15 or more.
3. The identification medium according to claim 1, in, One or more of the three or more sheets satisfies formula (d), 0.14≤Δλ / λc≤0.25 Formula (d).
4. The identification medium according to claim 1, in, The three or more sheets include the sheet (R) and the sheet (G), It also includes a plate (B) having a selective reflection center wavelength λc(B) and a plate (X) having a selective reflection center wavelength λc(X), The sheet (B) satisfies 430≤λc(B)≤490, The sheet (X) satisfies 430≤λc(X)≤660 and satisfies all equations (d-1) to (d-3), |λc(X)-λc(R)|≥30nm Formula (d-1) |λc(X)-λc(G)|≥30nm Formula (d-2) |λc(X)-λc(B)|≥30nm Formula (d-3).
5. The identification medium according to claim 4, in, The sheet (R), the sheet (G), the sheet (B) and the sheet (X) all satisfy the following formula (e), Δλ / λc≤0.10 Formula (e).
6. The identification medium according to claim 1, in, The three or more sheets include, in addition to the sheet (R) and the sheet (G), a sheet (B) having a selective reflection center wavelength λc (B), The sheet (B) satisfies 430≤λc(B), λc(R), λc(G) and λc(B) satisfy the following equations (p-1) and (p-2), λc(R)-λc(G)≥70nm Formula (p-1) λc(G)-λc(B)≥70nm Formula (p-2).
7. The identification medium according to claim 1, in, The thickness of the sheet is 3 μm or more and 7 μm or less.
8. The identification medium according to claim 1, in, The average particle size of each of the flakes is 100 μm or less.
9. The identification medium according to claim 1, in, The patterned phase difference layer is located closer to the viewing side than the light reflecting layer.
10. The identification medium according to claim 1, in, The patterned phase difference layer is a λ / 4 wave plate or a λ / 2 wave plate.
11. The identification medium according to claim 1, in, The light reflecting layer includes, as the sheet, a sheet having a reflection band including a region having a wavelength greater than 660 nm.
12. The identification medium according to claim 1, in, The identification medium further includes a light absorbing layer at a position of the light reflecting layer that is opposite to the viewing side.
13. The identification medium according to claim 1, in, The identification medium has a coating layer located closer to the viewing side than the patterned phase difference layer.