Liquid crystal sealing agent, method for manufacturing liquid crystal display panel, and liquid crystal display panel
By using alumina with an α-oxidation rate of less than 80% and a liquid crystal sealant with a specific composition, the problem of balancing moisture resistance and adhesive strength in the process of narrowing the linewidth of the sealing components of the liquid crystal display panel was solved, achieving a sealing effect with high moisture resistance and high adhesive strength.
Patent Information
- Application Number
- CN202380028787.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-05
AI Technical Summary
Existing liquid crystal display panel sealing components struggle to balance high moisture resistance and high bonding strength during the narrowing of linewidth, especially with the use of inorganic filler materials leading to a decrease in bonding strength.
A liquid crystal sealant containing alumina with an α-oxidation rate of less than 80%, a thermosetting compound with an intramolecular epoxy group, and a photopolymerization initiator is used, along with an appropriate amount of inorganic filler. The bonding strength is improved by controlling the particle size and aspect ratio of the alumina.
This achieves improved adhesion strength to the substrate while maintaining high moisture resistance, reducing liquid crystal contamination, and ensuring the stability and reliability of the sealing components.
Smart Images

Figure BDA0005050841490000221
Abstract
Description
Technical Field
[0001] The present invention relates to a liquid crystal sealant, a method for manufacturing a liquid crystal display panel, and a liquid crystal display panel. Background Art
[0002] A liquid crystal display panel generally includes a pair of substrates, a frame-shaped sealing member disposed therebetween, and a liquid crystal material sealed in a region surrounded by the sealing member. Such a liquid crystal display panel is manufactured by a liquid crystal dropping process.
[0003] In the liquid crystal drop process, first, a rectangular seal pattern is formed on one of a pair of substrates by dispensing. Then, the liquid crystal material is dropped into the sealing frame of the other substrate while the sealant is not solidified, and the other substrate is overlapped under vacuum, and the seal is irradiated with light such as ultraviolet light for temporary curing. After that, it is heated for formal curing to produce a liquid crystal display panel.
[0004] In recent years, as the frame of liquid crystal display panels has become narrower, the line width of sealing components has also been required to be narrower. Therefore, even if the sealing components are narrower and wider, they are required to have the same or higher adhesion to the substrate and moisture resistance than before, that is, they are required to have a high balance between bonding strength and moisture resistance.
[0005] As a method for improving the moisture resistance of the sealant, a method of adding inorganic fillers such as talc and alumina has been studied. For example, Patent Document 1 proposes a sealant for a liquid crystal display element, which contains a curable resin, a free radical polymerization initiator and / or a thermosetting agent, and alumina, and the content of alumina exceeds 20 parts by mass relative to 100 parts by mass of the curable resin (A). In addition, Patent Document 2 proposes a sealant for a liquid crystal display element, which contains a curable resin, a free radical polymerization initiator or a thermosetting agent, and alumina or talc with an aspect ratio of 2 or more, and the content of alumina or talc is 85% by mass or more.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-218447
[0009] Patent Document 2: Japanese Patent Application Publication No. 2013-214056 Summary of the invention
[0010] Problems to be solved by the invention
[0011] As mentioned above, the moisture resistance of the sealing member can be improved by adding inorganic fillers such as talc and alumina. However, the flexibility of the sealing member is impaired by adding inorganic fillers, so there is a problem that the bonding strength is easily reduced. As mentioned above, the bonding strength and moisture resistance are usually in a trade-off relationship, and it is difficult to take them into account in the previous sealants.
[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a liquid crystal sealing agent capable of forming a sealing member having high moisture resistance and high bonding strength with a substrate, a method for manufacturing a liquid crystal display panel using the same, and a liquid crystal display panel.
[0013] Means for solving problems
[0014] [1] A liquid crystal sealing agent comprising a curable compound (A), a thermosetting agent (B) and / or a photopolymerization initiator (C), and aluminum oxide (D) having an alpha conversion rate of 80% or less.
[0015] [2] The liquid crystal sealing agent according to [1], wherein the average particle diameter of the aluminum oxide (D) is 0.01 μm to 3 μm.
[0016] [3] The liquid crystal sealing agent according to [1] or [2], wherein content of the aluminum oxide (D) is 1 to 20 parts by mass relative to 100 parts by mass of the sclerosing compound (A).
[0017] [4] The liquid crystal sealing agent according to any one of [1] to [3], wherein the aspect ratio of the aluminum oxide (D) is 2.0 or less.
[0018] [5] The liquid crystal sealing agent according to any one of [1] to [4], wherein the aluminum oxide (D) is in a particle form.
[0019] [6] The liquid crystal sealing agent according to any one of [1] to [5], comprising a thermosetting compound (A1) having an epoxy group in a molecule as the curable compound (A), and the thermosetting agent (B).
[0020] [7] The liquid crystal sealing agent according to [6], wherein content of the thermosetting compound (A1) is 5 to 20 parts by mass relative to 100 parts by mass of the curable compound (A).
[0021] [8] The liquid crystal sealing agent according to [6] or [7], wherein the content of the thermosetting agent (B) is 10 parts by mass or more relative to 100 parts by mass of the curable compound (A).
[0022] [9] The liquid crystal sealant according to any one of [6] to [8], wherein the thermosetting agent (B) contains at least one selected from the group consisting of dihydrazide-based thermolatent curing agents, imidazole-based thermolatent curing agents, amine adduct-based thermolatent curing agents, and polyamine-based thermolatent curing agents.
[0023]
[10] The liquid crystal sealant described in any one of [6] to [9], further comprising a compound (A2) having an ethylenically unsaturated double bond in the molecule as the curable compound (A), and the photopolymerization initiator (C), and the content ratio (A1 / A2) of the thermosetting compound (A1) to the compound (A2) is 30 / 70 to 50 / 50 (mass ratio).
[0024]
[11] The liquid crystal sealing agent according to any one of [6] to
[10] , further comprising a partial epoxy (meth)acrylate (A3) as the curable compound (A).
[0025]
[12] The liquid crystal sealing agent according to any one of [1] to
[10] , wherein the photopolymerization initiator (C) contains at least one selected from the group consisting of oxime ester compounds, thioxanthone compounds, and anthraquinone compounds.
[0026]
[13] The liquid crystal sealing agent according to any one of [1] to
[11] , further comprising a coupling agent.
[0027]
[14] The liquid crystal sealing agent according to any one of [1] to
[13] , which is a liquid crystal sealing agent for a liquid crystal dropping method.
[0028]
[15] A method for manufacturing a liquid crystal display panel, comprising:
[0029] A step of forming a seal pattern of the liquid crystal sealant described in any one of [1] to
[14] on one substrate;
[0030] A step of dropping liquid crystal in a region of the seal pattern or on another substrate paired with the one substrate while the seal pattern is not solidified;
[0031] a step of overlapping the one substrate and the other substrate via the seal pattern; and
[0032] A step of curing the seal pattern.
[0033]
[16] The method for manufacturing a liquid crystal display panel as described in
[15] , wherein the step of curing the seal pattern includes: a step of irradiating the seal pattern with light to cure the seal pattern.
[0034]
[17] The method for manufacturing a liquid crystal display panel according to
[16] , wherein the light irradiated onto the seal pattern includes light in the visible light region.
[0035]
[18] The method for manufacturing a liquid crystal display panel as described in
[16] or
[17] , wherein the step of curing the seal pattern further includes: a step of heating the seal pattern irradiated with light to cure it.
[0036]
[19] A liquid crystal display panel comprising: a pair of substrates; a frame-shaped sealing member arranged between the pair of substrates; and a liquid crystal layer filling a space between the pair of substrates surrounded by the sealing member, wherein the sealing member comprises a cured product of the liquid crystal sealant described in any one of [1] to
[13] .
[0037] Effects of the Invention
[0038] According to the liquid crystal sealing agent of the present invention, it is possible to form a sealing member having high moisture resistance and high bonding strength with a substrate. DETAILED DESCRIPTION
[0039] In this specification, the numerical range expressed by "to" means a range including the numerical values recorded before and after "to" as the lower limit and the upper limit. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the upper limit or lower limit of the numerical range recorded in other stages.
[0040] As described above, from the perspective of imparting moisture resistance and strength to the sealing member, aluminum oxide is sometimes added to the liquid crystal sealant. Aluminum oxide has various crystalline phases such as α, β, θ, and γ depending on the manufacturing conditions such as the sintering temperature. Among them, aluminum oxide having the highest sintering temperature and an α-crystalline phase has high heat resistance and is chemically stable, so it is widely used. On the other hand, this also becomes a factor that causes the bonding strength with the substrate to decrease.
[0041] On the other hand, the present inventors have found that alumina having an alpha conversion rate of a certain value or less improves the moisture resistance of the sealing member and is less likely to reduce the bonding strength with the substrate, but can improve the bonding strength.
[0042] The reason is not clear, but it can be inferred as follows. Compared with aluminum oxide with a high alpha rate, aluminum oxide (D) with a low alpha rate has a large number of hydroxyl groups that are easily coordinated around aluminum atoms and has a large number of hydroxyl groups on the surface. Therefore, it is believed that hydrogen bonds are formed between the hydroxyl groups of aluminum oxide (D) and the hydroxyl groups on the substrate, and between the hydroxyl groups of aluminum oxide (D) and the epoxy groups and hydroxyl groups (especially epoxy groups) of the curable compound (A), thereby improving the bonding strength with the substrate. Below, the composition of the liquid crystal sealant of the present invention is specifically described.
[0043] 1. Liquid crystal sealant
[0044] The liquid crystal sealant of the present invention comprises a curable compound (A), a thermosetting agent (B) and / or a photopolymerization initiator (C) for curing the curable compound (A), and aluminum oxide (D) having an alpha conversion rate of 80% or less, and may further comprise other components such as an inorganic filler (E) as required. The curable compound may be any of a monomer, an oligomer, and a polymer.
[0045] 1-1. Curable compound (A)
[0046] 1-1-1. Thermosetting compound (A1) having an epoxy group in the molecule
[0047] The above-mentioned liquid crystal sealant may contain a thermosetting compound (A1) having an epoxy group in the molecule as the curable compound (A). The epoxy group contained in the molecule of the thermosetting compound (A1) is preferably 2 or more. It should be noted that in this specification, the thermosetting compound (A1) does not contain some epoxy (meth) acrylate. In addition, the thermosetting compound (A1) is preferably used together with the thermosetting agent (B) described later.
[0048] The thermosetting compound (A1) may be any of a monomer, an oligomer or a polymer. The thermosetting compound (A1) can further reduce the moisture permeability of the cured product and improve the display properties of the obtained liquid crystal display panel.
[0049] The weight average molecular weight of the thermosetting compound (A1) is, for example, preferably 300 to 10000, more preferably 300 to 5000. The weight average molecular weight of the thermosetting compound (A1) can be measured by gel permeation chromatography (GPC) based on polystyrene conversion.
[0050] The thermosetting compound (A1) is preferably a compound having an aromatic ring. Examples of epoxy compounds having an aromatic ring include: aromatic polyglycidyl ether compounds obtained by reacting aromatic diols represented by bisphenol A, bisphenol S, bisphenol E, bisphenol F, bisphenol AD, etc., or diols obtained by modifying these aromatic diols with ethylene glycol, propylene glycol, alkanediol, etc., with epichlorohydrin; polyphenols represented by novolac resins derived from phenol or cresol and formaldehyde, polyalkenylphenols or copolymers thereof, etc., with epichlorohydrin; and glycidyl ether compounds of xylylene phenol resins, etc. Among them, preferably cresol novolac epoxy compound, phenol novolac epoxy compound, bisphenol A epoxy compound, bisphenol F epoxy compound, trisphenol methane epoxy compound, trisphenol ethane epoxy compound, trisphenol epoxy compound, dicyclopentadiene epoxy compound, diphenyl ether epoxy compound or biphenyl epoxy compound. The liquid crystal sealant may contain only one epoxy compound or more than two. Among them, preferably a bisphenol A epoxy compound having a bisphenol A skeleton in the molecule. The thermosetting compound (A1) may be liquid or solid.
[0051] Relative to 100 parts by mass of curable compound (A), the content of thermosetting compound (A1) is preferably 2 parts by mass to 40 parts by mass. If the content of thermosetting compound (A1) is 2 parts by mass or more, it is easier to improve the bonding strength with the substrate. This is because the thermosetting compound (A1) having an epoxy group has an epoxy group and a hydroxyl group (especially an epoxy group), and it is easy to form a hydrogen bond with the hydroxyl group on the surface of aluminum oxide (D), thereby easily improving the bonding strength of the cured product. If the content of thermosetting compound (A1) is 40 parts by mass or less, the flexibility of the cured product can be made less susceptible to damage. From the same point of view, relative to 100 parts by mass of curable compound (A), the content of thermosetting compound (A1) is more preferably 5 parts by mass to 20 parts by mass, and more preferably 10 parts by mass to 20 parts by mass.
[0052] 1-1-2. Compounds having ethylenically unsaturated double bonds in their molecules (A2)
[0053] The liquid crystal sealant may also contain a compound (A2) having an ethylenically unsaturated double bond in the molecule as a curable compound (A). It should be noted that in this specification, the compound (A2) having an ethylenically unsaturated double bond in the molecule does not contain some epoxy (meth)acrylates. In addition, the compound having an ethylenically unsaturated double bond in the molecule is preferably used together with a photopolymerization initiator (C) described later.
[0054] The compound (A2) having an ethylenically unsaturated double bond in the molecule may be any of a monomer, an oligomer or a polymer. Examples of compounds having an ethylenically unsaturated double bond in the molecule include compounds having a (meth)acryloyl group in the molecule. The number of (meth)acryloyl groups in each molecule of the compound having a (meth)acryloyl group may be one or more.
[0055] It should be noted that in the present specification, "(meth)acrylate" means acrylate or methacrylate, "(meth)acryloyl" means acryloyl or methacryloyl, "(meth)acrylic acid" means acrylic acid or methacrylic acid, and "(meth)acrylic resin" means acrylic resin or methacrylic resin.
[0056] Examples of the curable compound containing one (meth)acryloyl group in one molecule include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate.
[0057] Examples of curable compounds having two or more (meth)acryloyl groups in one molecule include: di(meth)acrylates derived from polyethylene glycol, propylene glycol, polypropylene glycol, and the like; di(meth)acrylates derived from tris(2-hydroxyethyl)isocyanurate; di(meth)acrylates derived from a diol obtained by adding 4 or more ethylene oxide or propylene oxide to 1 mol of neopentyl glycol; di(meth)acrylates derived from a diol obtained by adding 2 mol of ethylene oxide or propylene oxide to 1 mol of bisphenol A or bisphenol F (bisphenol A type epoxy (meth)acrylate or bisphenol F type epoxy (meth)acrylate); di(meth)acrylates or tri(meth)acrylates derived from a polyol obtained by adding 2 or 3 mol of ethylene oxide or propylene oxide to 1 mol of trimethylolpropane; diols obtained by adding 4 or more ethylene oxide or propylene oxide to 1 mol of bisphenol A; di(meth)acrylate of; tri(2-hydroxyethyl)isocyanurate tri(meth)acrylate; trimethylolpropane tri(meth)acrylate or its oligomer; pentaerythritol tri(meth)acrylate or its oligomer; poly(meth)acrylate of dipentaerythritol; tri(acryloxyethyl)isocyanurate; caprolactone-modified tri(acryloxyethyl)isocyanurate; caprolactone-modified tri(methacryloxyethyl)isocyanurate; alkyl-modified poly(meth)acrylate of dipentaerythritol; caprolactone-modified poly(meth)acrylate of dipentaerythritol; hydroxypivalic acid neopentyl glycol di(meth)acrylate; caprolactone-modified hydroxypivalic acid neopentyl glycol di(meth)acrylate; ethylene oxide-modified phosphoric acid (meth)acrylate; ethylene oxide-modified alkylated phosphoric acid (meth)acrylate; and oligomeric (meth)acrylates of neopentyl glycol, trimethylolpropane and pentaerythritol, etc. Among them, di(meth)acrylates derived from diols obtained by adding 2 mol of ethylene oxide or propylene oxide to 1 mol of bisphenol A or bisphenol F (bisphenol A type epoxy (meth)acrylate or bisphenol F type epoxy (meth)acrylate) are preferred.
[0058] The weight average molecular weight of the compound (A2) having an ethylenically unsaturated double bond in the molecule, as measured by gel permeation chromatography (GPC), is in the range of, for example, 200 to 10,000, or preferably 200 to 5,000.
[0059] Relative to 100 parts by mass of curable compound (A), the content of the compound (A2) having an ethylenically unsaturated double bond in the molecule is preferably 10 parts by mass to 50 parts by mass, more preferably 15 parts by mass to 40 parts by mass, and further preferably 20 parts by mass to 35 parts by mass. If the content of the above-mentioned compound (A2) is more than 20 parts by mass, when temporarily cured by light curing, the above-mentioned compound (A2) is easily fully cured, so it is easier to suppress liquid crystal contamination. If the content of the above-mentioned compound (A2) is less than 30 parts by mass, the bonding strength to the substrate is less likely to be damaged.
[0060] 1-1-3. Partial epoxy (meth)acrylate (A3)
[0061] The liquid crystal sealant may contain a portion of epoxy (meth) acrylate (A3) as the curable compound (A). The portion of epoxy (meth) acrylate (A3) can improve the adhesion of the cured product of the liquid crystal sealant to the substrate and improve the compatibility of the thermosetting compound (A1) having an epoxy group and the compound (A2) having an ethylenically unsaturated double bond in the molecule.
[0062] The partial epoxy (meth)acrylate (A3) is a partially (meth)acryloyl-modified epoxy resin obtained by modifying at least one epoxy group of a difunctional or higher epoxy resin with a (meth)acryloyl group. The partial epoxy (meth)acrylate (A) can be obtained, for example, by reacting a difunctional or higher epoxy resin with (meth)acrylic acid in the presence of a basic catalyst.
[0063] The epoxy resin as the raw material of the partial epoxy (meth) acrylate (A3) can be an epoxy resin having two or more epoxy groups in the molecule. Examples of the epoxy resin include bisphenol A type, bisphenol F type, 2,2'-diallylbisphenol A type, bisphenol AD type and hydrogenated bisphenol type bisphenol type epoxy resins; phenol novolac type, cresol novolac type, biphenyl novolac type and trisphenol novolac type novolac type phenolic varnish type epoxy resins; biphenyl type epoxy resin; and naphthalene type epoxy resin. Among them, bisphenol A type, bisphenol F type and other bisphenol type epoxy resins are preferred from the aspects of low crystallinity and high coating stability.
[0064] It should be noted that the epoxy resin may be trifunctional or tetrafunctional, or may have a greater number of epoxy groups. Of these, a difunctional epoxy resin is preferred from the viewpoint of appropriately adjusting the crosslinking density and appropriately improving the bonding strength of the cured product to the substrate.
[0065] Regarding the partial epoxy (meth)acrylate (A3), the ratio of the number of moles of the (meth)acryloyl group to the number of moles of the epoxy group is preferably 1 or more, more preferably 2 or more. By increasing the ratio of the number of moles of the (meth)acryloyl group, liquid crystal contamination caused by elution of the sealant into the liquid crystal can be easily suppressed.
[0066] The weight average molecular weight of some epoxy (meth)acrylates (A3) measured by gel permeation chromatography (GPC) is preferably 300 to 500.
[0067] Relative to 100 parts by mass of curable compound (A), the content of partial epoxy (meth) acrylate (A3) is preferably 20 to 80 parts by mass, more preferably 30 to 70 parts by mass, and further preferably 45 to 65 parts by mass. If the content of partial epoxy (meth) acrylate (A3) is 20 parts by mass or more, it is easier to improve the bonding strength of the cured product while improving the compatibility of the thermosetting compound (A1) and the above-mentioned compound (A2). If the content of partial epoxy (meth) acrylate (A3) is 80 parts by mass or less, the flexibility of the cured product is less likely to be impaired.
[0068] 1-1-4. Common matters
[0069] The curable compound (A) preferably contains at least one of a thermosetting compound (A1), a compound having an ethylenically unsaturated double bond in the molecule (A2), and a partial epoxy (meth)acrylate (A3), and more preferably contains all of them from the viewpoint of the balance between photocuring and thermocuring.
[0070] In addition, the content ratio (A1 / A2) of the thermosetting compound (A1) and the compound (A2) having an ethylenically unsaturated double bond in the molecule can be set according to the required performance. For example, from the viewpoint of further improving the bonding strength with the substrate, the ratio of the thermosetting compound (A1) is preferably large, and A1 / A2 is preferably 30 / 70 to 50 / 50 (mass ratio), and more preferably 40 / 60 to 50 / 50 (mass ratio).
[0071] 1-2. Thermosetting agent (B)
[0072] The sealing agent contains a thermosetting agent (B) for curing the thermosetting compound (A1).
[0073] The thermosetting agent (B) is preferably a latent thermosetting agent. The so-called latent thermosetting agent is a compound that does not cure the thermosetting compound (A1) and part of the epoxy (meth) acrylate (A3) under normal storage conditions (room temperature, visible light, etc.), but cures these compounds when heated. The thermosetting agent (B) is preferably a curing agent that can cure epoxy compounds (hereinafter also referred to as "epoxy curing agent").
[0074] From the viewpoint of improving the viscosity stability of the photothermosetting resin composition and not impairing the moisture resistance of the cured product, the melting point of the epoxy curing agent is preferably 50 to 250°C, more preferably 100 to 200°C, and even more preferably 150 to 200°C.
[0075] Examples of epoxy curing agents include dihydrazide-based thermolatent curing agents, imidazole-based thermolatent curing agents, dicyandiamide-based thermolatent curing agents, amine adduct-based thermolatent curing agents, and polyamine-based thermolatent curing agents, etc. Among them, dihydrazide-based thermolatent curing agents, imidazole-based thermolatent curing agents, amine adduct-based thermolatent curing agents, and polyamine-based thermolatent curing agents are preferred, and from the viewpoint of further improving display characteristics, imidazole-based thermolatent curing agents, amine adduct-based thermolatent curing agents, and polyamine-based thermolatent curing agents are more preferred, and amine adduct-based thermolatent curing agents and polyamine-based thermolatent curing agents are further preferred.
[0076] Examples of dihydrazide-based thermal latent curing agents include adipic acid dihydrazide (melting point 181° C.), 1,3-bis(hydrazinocarbonylethyl)-5-isopropylhydantoin (melting point 120° C.), 7,11-octadecadiene-1,18-dicarbohydrazide (melting point 160° C.), dodecanedioic acid dihydrazide (melting point 190° C.), and sebacic acid dihydrazide (melting point 189° C.).
[0077] Examples of the imidazole-based thermal latent curing agent include 2,4-diamino-6-[2′-ethylimidazolyl-(1′)]-ethyltriazine (melting point: 215° C. to 225° C.) and 2-phenylimidazole (melting point: 137° C. to 147° C.).
[0078] Examples of the dicyandiamide-based heat latent curing agent include dicyandiamide (melting point: 209° C.) and the like.
[0079] The amine addition-based thermolatent curing agent is a thermolatent curing agent containing an addition compound obtained by reacting an amine-based compound having catalytic activity with an arbitrary compound. Examples of the amine addition-based thermolatent curing agent include Amicure PN-40 (melting point 110° C.) manufactured by Ajinomoto Fine-Techno, Amicure PN-50 (melting point 120° C.) manufactured by Ajinomoto Fine-Techno, Amicure PN-23 (melting point 100° C.) manufactured by Ajinomoto Fine-Techno, Amicure PN-31 (melting point 115° C.) manufactured by Ajinomoto Fine-Techno, Amicure PN-H (melting point 115° C.) manufactured by Ajinomoto Fine-Techno, Amicure MY-24 (melting point 120° C.) manufactured by Ajinomoto Fine-Techno, Amicure MY-H (melting point 131° C.) manufactured by Ajinomoto Fine-Techno, and the like.
[0080] The polyamine-based thermal latent curing agent is a thermal latent curing agent having a polymer structure obtained by reacting amine with epoxy, and examples thereof include Adeka Hardener EH4339S (softening point 120° C. to 130° C.) and Adeka Hardener EH4357S (softening point 73° C. to 83° C.) manufactured by Adeka Corporation.
[0081] The content of the thermosetting agent (B) is preferably 10 parts by mass or more, and more preferably 15 to 30 parts by mass, relative to 100 parts by mass of the curable compound (A). If the content of the thermosetting agent (B) is 10 parts by mass or more, it is easy to improve the curability of the thermosetting compound (A1). If the content of the thermosetting agent (B) is 30 parts by mass or less, it is easier to suppress liquid crystal contamination caused by the dissolution of the thermosetting agent (B) into the liquid crystal.
[0082] Moreover, content of a thermosetting agent (B) becomes like this. Preferably it is 50-300 mass parts with respect to 100 mass parts of thermosetting compounds (A1), More preferably, it is 100-200 mass parts.
[0083] 1-3. Photopolymerization initiator (C)
[0084] The said liquid crystal sealing compound may contain the photoinitiator (C) for starting hardening (polymerization) of the compound (A2) which has an ethylenically unsaturated double bond in a molecule|numerator.
[0085] The photopolymerization initiator (C) is not particularly limited as long as it is a compound that can initiate curing (polymerization) of the above-mentioned compound. For example, the photopolymerization initiator (C) may be a free radical polymerization initiator, a self-cleavage type photopolymerization initiator, or a hydrogen abstraction type photopolymerization initiator.
[0086] Examples of self-cleaving photopolymerization initiators include alkylphenone compounds, acylphosphine oxide compounds, titanocene compounds, acetophenone compounds, benzoylformate compounds, benzoin ether compounds, and oxime ester compounds. Examples of the alkylphenone compounds include benzyldimethyl ketal such as 2,2-dimethoxy-1,2-diphenylethane-1-one (IRGACURE 651 manufactured by BASF), α-aminoalkylphenone such as 2-methyl-2-morpholinyl (4-thiomethylphenyl) propane-1-one (IRGACURE 907 manufactured by BASF), and 1-hydroxy-cyclohexyl-phenyl-ketone (IRGACURE 651 manufactured by BASF). 184 and other α-hydroxyalkyl phenones. Examples of the above-mentioned acyl phosphine oxide compounds include 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, etc. Examples of the above-mentioned titanocene compounds include bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, etc. Examples of the above-mentioned acetophenone compounds include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-morpholin Examples of the above-mentioned benzoylformate-based compounds include methyl benzoylformate, etc. Examples of the above-mentioned benzoin ether-based compounds include benzoin, benzoin methyl ether, and benzoin isopropyl ether, etc. Examples of the above-mentioned oxime ester-based compounds include 1,2-octanedione-1-[4-(phenylthio)-2-(O-benzoyl oxime)] (IRGACURE OXE01 manufactured by BASF) and ethyl ketone-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-1-(O-acetyl oxime) (IRGACURE OXE02 manufactured by BASF) and the like.
[0087] Examples of hydrogen abstraction type photopolymerization initiators include benzophenone compounds, thioxanthone compounds, anthraquinone compounds, benzil compounds, etc. Examples of the above benzophenone compounds include benzophenone, methyl o-benzoylbenzoate-4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetrakis(tert-butylcarbonylperoxy)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone. Examples of the thioxanthone compounds include thioxanthone, 2-chlorothioxanthone, 1-chloro-4-propoxythioxanthone, 1-chloro-4-ethoxythioxanthone (Speedcure CPTX manufactured by Lambson Limited), 2-isopropylthioxanthone (Speedcure ITX manufactured by Lambson Limited), 4-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone (Speedcure DETX manufactured by Lambson Limited), 2,4-dichlorothioxanthone and (2-carboxymethoxythioxanthone)-(polytetramethylene glycol 250) diester (Omnipol TX manufactured by IGM). Examples of the anthraquinone compounds include 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-hydroxyanthraquinone (2-Hydroxyanthraquinone manufactured by Tokyo Chemical Industry Co., Ltd.), 2,6-dihydroxyanthraquinone (Anthraflavic Acid manufactured by Tokyo Chemical Industry Co., Ltd.), and 2-hydroxymethylanthraquinone (2-(Hydroxymethyl)anthraquinone manufactured by Junsei Chemical Co., Ltd.).
[0088] The absorption wavelength of the photopolymerization initiator (C) is not particularly limited, and for example, it can be set to a photopolymerization initiator that absorbs light with a wavelength of 360 nm or more. Among them, a photopolymerization initiator that absorbs light in the visible light region is more preferred, a photopolymerization initiator that absorbs light with a wavelength of 360 nm to 780 nm is further preferred, and a photopolymerization initiator that absorbs light with a wavelength of 360 nm to 430 nm is particularly preferred.
[0089] Examples of photopolymerization initiators that absorb light of wavelengths of 360 nm or more include alkylphenone compounds, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, thioxanthone compounds, and anthraquinone compounds. Among them, oxime ester compounds, thioxanthone compounds, and anthraquinone compounds are preferred, and oxime ester compounds are more preferred.
[0090] The molecular weight of the photopolymerization initiator (C) can be set to 200 to 5000, for example. If the molecular weight of the photopolymerization initiator (C) is 200 or more, the photopolymerization initiator (C) is not easily dissolved into the liquid crystal. On the other hand, if the molecular weight of the photopolymerization initiator (C) is 5000 or less, the compatibility with various curable compounds (A) is improved, and the curability of the sealant tends to become good. The molecular weight of the photopolymerization initiator (C) is more preferably 230 to 3000, and more preferably 230 to 1500.
[0091] The molecular weight of the photopolymerization initiator (C) can be determined as the “relative molecular mass” of the molecular structure of the main peak detected when analyzing by high performance liquid chromatography (HPLC).
[0092] Specifically, a sample solution is prepared by dissolving a photopolymerization initiator (C) in THF (tetrahydrofuran), and the sample solution is subjected to high performance liquid chromatography (HPLC) measurement. Then, the area percentage of the detected peaks (the ratio of the area of each peak to the total area of all peaks) is determined to confirm the presence or absence of a main peak. The so-called main peak refers to the peak with the highest intensity (the peak with the highest peak height) among all peaks detected at the characteristic detection wavelength of each compound (for example, 400nm for thioxanthone compounds). The relative molecular mass corresponding to the peak vertex of the detected main peak can be measured by liquid chromatography mass spectrometry (LC / MS: Liquid Chromatography Mass Spectrometry).
[0093] The content of the photopolymerization initiator (C) is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and still more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the photocurable compound (e.g., the total of the compound (A2) having an ethylenically unsaturated double bond in the molecule and a portion of the epoxy (meth)acrylate (A3)). If the content is 0.01 parts by mass or more, it is easy to improve the photocurability of the sealant, and if it is 10 parts by mass or less, it is easier to suppress liquid crystal contamination caused by the dissolution of the photopolymerization initiator (C) into the liquid crystal.
[0094] 1-4. Alumina (D)
[0095] The liquid crystal sealing agent contains aluminum oxide (D) having an alpha conversion rate of 80% or less. As described above, since aluminum oxide (D) having a low alpha conversion rate has a large number of hydroxyl groups on the surface, hydrogen bonds are easily formed, especially between the hydroxyl groups of aluminum oxide (D) and the epoxy groups of the thermosetting compound (A1), and between the hydroxyl groups of aluminum oxide (D) and the hydroxyl groups on the substrate, and it is believed that the bonding strength with the substrate is improved.
[0096] The alpha conversion rate of aluminum oxide (D) is 80% or less, preferably 50% or less, and more preferably 20% or less. If the alpha conversion rate of aluminum oxide (D) is 50% or less, it is easier to improve the bonding strength with the substrate. The lower limit of the alpha conversion rate is not particularly limited, and for example, from the viewpoint of easy formation of uniform spherical shapes, it is 1%, preferably 4%. The alpha conversion rate of aluminum oxide (D) can be adjusted by manufacturing conditions such as sintering temperature.
[0097] The alpha conversion rate of aluminum oxide (D) can be measured by the following procedure.
[0098] α-phase alumina powder AA-05 (manufactured by Sumitomo Chemical Co., Ltd.) and θ-phase alumina powder Taimicron TM-100D (manufactured by Daming Chemical Co., Ltd.) were mixed in mass ratios of 0:10, 5:5, and 10:0, and the resulting powders were subjected to X-ray diffraction measurement. The integrated intensity of the α-phase peak detected at 2θ=43° was calculated, and a standard curve of the mixing ratio and the integrated intensity was prepared.
[0099] Next, the powder of aluminum oxide (D) is subjected to X-ray diffraction measurement, and the integrated intensity of the peak at 2θ=43° is calculated, and the content of the α phase, i.e., the α conversion rate (%), is obtained by comparing it with the above-mentioned standard curve. It should be noted that the X-ray diffraction can be performed using a JDX-3500 X-ray diffractometer (manufactured by JEOL Ltd.).
[0100] The shape of the aluminum oxide (D) is not particularly limited as long as the alpha conversion rate satisfies the above range, and may be any of spherical, crushed (plate-like), needle-like, etc. Among them, spherical aluminum oxide is preferred from the viewpoint of large surface area and easy improvement of bonding strength with the substrate.
[0101] The aspect ratio of aluminum oxide (D) is not particularly limited, and is preferably 2.0 or less, and more preferably 1.0 to 1.5. Aluminum oxide (D) having an aspect ratio of 2.0 or less has a large surface area and is easy to improve the bonding strength with the substrate. In addition, when used in a liquid crystal display panel, it is less likely to cause peeling caused by the generation of stress concentration points, and the reduction in bonding strength can be further suppressed.
[0102] The aspect ratio of aluminum oxide (D) is obtained by selecting any 20 particles from an image measured by a scanning electron microscope (SEM), measuring the major axis and the minor axis respectively, and calculating the average major axis and the average minor axis. Then, the average major axis and the average minor axis can be substituted into the following formula to calculate.
[0103] Aspect ratio = average major diameter (μm) / average minor diameter (μm)
[0104] The average particle size of aluminum oxide (D) is not particularly limited as long as it is in the range suitable for the liquid crystal cell gap of the liquid crystal display panel. The average particle size of aluminum oxide (D) can be, for example, 0.01 μm to 25 μm, preferably 0.01 μm to 3 μm, and more preferably 0.1 μm to 2 μm. If the average particle size of aluminum oxide (D) is 0.01 μm or more, it is easier to improve the moisture resistance of the cured product of the liquid crystal sealant. If the average particle size of aluminum oxide (D) is 3 μm or less, it is easier to suppress the poor curing of compounds (A2) and partial epoxy (meth) acrylates (A3) having ethylenically unsaturated double bonds in the molecule caused by aluminum oxide (D) blocking or reflecting light during photocuring, and liquid crystal contamination can be further suppressed. The average particle size of aluminum oxide (D) can be measured by Microtrac MT3300.
[0105] Relative to 100 parts by mass of curable compound (A), the content of aluminum oxide (D) is preferably 2 to 25 parts by mass, more preferably 5 to 20 parts by mass, and further preferably 7 to 15 parts by mass. The more aluminum oxide (D) is contained, the easier it is to further reduce the moisture permeability of the cured product. On the other hand, by not making the content of aluminum oxide (D) too much, the flexibility of the cured product is less likely to be damaged, and the bonding strength is also less likely to be damaged. In addition, the poor photocuring caused by the light reflection caused by aluminum oxide (D) can be further suppressed, so the liquid crystal contamination can be further reduced.
[0106] 1-5. Inorganic filler (E)
[0107] The liquid crystal sealing agent may further contain other inorganic fillers (E) other than alumina. The inorganic filler (E) can provide a predetermined hardness and linear expansion property to the cured product, and can also inhibit water from penetrating through the cured product, thereby further reducing the moisture permeability of the cured product.
[0108] Examples of the inorganic filler (E) include calcium carbonate, magnesium carbonate, barium sulfate, magnesium sulfate, aluminum silicate, zirconium silicate, iron oxide, titanium oxide, titanium nitride, aluminum oxide other than the above, zinc oxide, silica, potassium titanate, kaolin, talc, glass beads, sericite, activated clay, bentonite, aluminum nitride, silicon nitride, etc. Among them, silica and talc are preferred.
[0109] The shape of the inorganic filler (E) may be a fixed shape such as a sphere, a plate, or a needle, or may be an unfixed shape. When the inorganic filler (E) is spherical, the average primary particle size of the inorganic filler (E) is preferably 1.5 μm or less. In addition, the specific surface area of the inorganic filler (E) is preferably 0.5 m 2 / g or more and 20m 2 / g or less. The average primary particle size of the inorganic filler (E) can be measured according to the laser diffraction method described in JIS Z8825 (2013). The specific surface area of the filler can be measured by the BET method described in JIS Z8830 (2013).
[0110] Relative to 100 parts by mass of curable compound (A), the content of inorganic filler (E) is preferably 2 parts by mass to 30 parts by mass, more preferably 2 parts by mass to 20 parts by mass, and further preferably 5 parts by mass to 20 parts by mass. The more the content of inorganic filler (E), the easier it is to further reduce the moisture permeability of the cured product, and the harder the cured product can be. On the other hand, by not making the content of inorganic filler (E) too much, the softness of the cured product is less likely to be damaged, and the bonding strength is also less likely to be damaged.
[0111] 1-6. Others
[0112] The liquid crystal sealing agent may contain a thermal radical polymerization initiator, organic fine particles, a coupling agent such as a silane coupling agent, an ion scavenger, an ion exchanger, a leveling agent, a pigment, a dye, a sensitizer, a plasticizer, a defoaming agent, and the like in addition to the above components.
[0113] Examples of the thermal radical polymerization initiator include organic peroxides, azo compounds, benzoins, benzoin ethers, and acetophenones.
[0114] The organic particles can reduce the residual stress when the liquid crystal sealant is applied. For example, the organic particles can be provided as organic particles having an elastic core and an outer shell, wherein the elastic core comprises a conjugated diene rubber and a silicone rubber, etc., and the outer shell is formed of a polymer such as a (meth)acrylate, a vinyl monomer, and an epoxy monomer that improves compatibility with other components.
[0115] Alternatively, the following coated particles can also be used, that is, coated particles having a core particle (core) formed by inorganic particles and a polymer layer coating the core, and having a functional group containing a carbon-carbon double bond on the surface. The functional group containing a carbon-carbon double bond can be a vinyl, an allyl group, an acryloyl group, or a methacryloyl group. For the example of the core particle, the same material as that listed as the above-mentioned inorganic filler (E) can be used, and from the viewpoint of excellent thermal stability, preferably silica.
[0116] The content of organic particles is preferably 5 to 17 parts by mass relative to 100 parts by mass of liquid crystal sealant. If the content of organic particles is 5 parts by mass or more, the bonding strength between the cured product and the substrate can be further improved. On the other hand, if the content of organic particles is 17 parts by mass or less, the amount of other components (such as curable compounds) is sufficiently large, which can further improve the strength of the cured product.
[0117] Examples of the silane coupling agent include vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltriethoxysilane.
[0118] It is preferable that content of the silane coupling agent is 0.01 mass part - 5 mass parts with respect to 100 mass parts of liquid crystal sealing agents. When content of the silane coupling agent is 0.01 mass part or more, the adhesive strength between a hardened|cured material and a board|substrate can be improved further.
[0119] The liquid crystal sealing compound may further contain a spacer for adjusting the gap of a liquid crystal display panel, and the like.
[0120] The total amount of other components is preferably 0.1 to 50 parts by mass with respect to 100 parts by mass of the liquid crystal sealing agent. When the total amount is 50 parts by mass or less, the viscosity of the sealant is unlikely to increase excessively, and the coating stability of the sealant is unlikely to be impaired.
[0121] 1-7. Physical properties of sealants
[0122] The viscosity of the liquid crystal sealing agent at 25° C. and 2.5 rpm of an E-type viscometer is preferably 200 to 450 Pa·s, more preferably 300 to 400 Pa·s. When the viscosity is within the above range, the coating properties of the sealing agent using a dispenser become good.
[0123] 2. Liquid crystal display panel and manufacturing method thereof
[0124] The liquid crystal display panel of the present invention includes: a pair of substrates (a display substrate and a counter substrate); a frame-shaped sealing member disposed between the pair of substrates; and a liquid crystal layer filling a space between the pair of substrates surrounded by the sealing member.
[0125] The display substrate and the counter substrate are both transparent substrates. The transparent substrate can be made of inorganic materials such as glass, or plastics such as polycarbonate, polyethylene terephthalate, polyether sulfone, and PMMA (polymethyl methacrylate).
[0126] On the surface of the display substrate or the counter substrate, a matrix of TFTs (thin film transistors), color filters, black matrices, etc. may be arranged. On the surface of the display substrate or the counter substrate, an alignment film may be arranged. The alignment film may contain a known organic alignment agent or an inorganic alignment agent.
[0127] The sealing member may be disposed between the display substrate and the counter substrate, and preferably between the alignment films of the pair of substrates. The sealing member is a cured product of the above-mentioned liquid crystal sealant.
[0128] The liquid crystal display panel is manufactured using the liquid crystal sealing agent of the present invention. The manufacturing method of the liquid crystal display panel generally includes a liquid crystal dropping process and a liquid crystal injection process, but the liquid crystal display panel of the present invention is preferably manufactured by the liquid crystal dropping process.
[0129] The method for manufacturing a liquid crystal display panel using a liquid crystal dropping process includes:
[0130] 1) a step of forming a sealing pattern of the liquid crystal sealing agent on one of a pair of substrates;
[0131] 2) A step of dropping liquid crystal into a region surrounded by a seal pattern on one substrate or onto another substrate while the seal pattern is not cured;
[0132] 3) a step of overlapping one substrate with another substrate via a seal pattern; and
[0133] 4) A step of curing the seal pattern.
[0134] In the step 1), the liquid crystal sealing agent may be applied on one substrate to form a seal pattern. The seal pattern may be arranged on the alignment film of one substrate or on the outer peripheral side of the alignment film, and is preferably arranged on the alignment film.
[0135] In the step 2), the state in which the sealing pattern is not cured refers to a state in which the curing reaction of the liquid crystal sealant has not proceeded to the gel point. Therefore, in the step 2), in order to suppress the dissolution of the liquid crystal sealant into the liquid crystal, the sealing pattern may be semi-cured by light irradiation or heating. One substrate and the other substrate are respectively a display substrate or a counter substrate.
[0136] In the step 4), curing by light irradiation and subsequent curing by heating can be performed. By performing curing by light irradiation, the liquid crystal sealant can be cured in a short time, so that dissolution into the liquid crystal can be suppressed. By combining curing by light irradiation with curing by heating, it is possible to reduce damage to the liquid crystal layer caused by light compared to the case of performing curing by light irradiation alone.
[0137] The irradiated light can be appropriately selected according to the type of photopolymerization initiator (C) in the above-mentioned sealant, and is preferably light in the visible light region, for example, preferably light with a wavelength of more than 370nm and less than 450nm. This is because the light of the above-mentioned wavelength causes relatively little damage to the liquid crystal material and the drive electrode. The irradiation of light can use a known light source that emits ultraviolet rays and visible light. In the case of irradiating visible light, a high-pressure mercury lamp, a low-pressure mercury lamp, a metal halide lamp, a xenon lamp, a fluorescent lamp, etc. can be used.
[0138] The light irradiation energy may be energy capable of curing the compound (A2) and part of the epoxy (meth)acrylate (A3). The light curing time depends on the composition of the liquid crystal sealing agent, but is, for example, about 10 minutes.
[0139] Although it depends on the composition of the liquid crystal sealing agent, the heat curing temperature is, for example, 120° C., and the heat curing time is about 2 hours.
[0140] Example
[0141] Hereinafter, the present invention will be described in more detail by way of examples. However, the scope of the present invention is not limited by these examples at all, and the embodiments can be modified within the scope not departing from the gist of the present invention.
[0142] 1. Preparation of Materials
[0143] 1-1. Curable compound (A)
[0144] 1-1-1. Thermosetting compound (A1) having an epoxy group in the molecule
[0145] ·Bisphenol A type epoxy resin (manufactured by ADEKA, EP-4000S, epoxy equivalent 260 g / eq)
[0146] 1-1-2. Compounds having ethylenically unsaturated double bonds in their molecules (A2)
[0147] Bisphenol A type acrylic resin (manufactured by Daicel Allnex, EBECRYL 3700, weight average molecular weight 485)
[0148] 1-1-3. Partial epoxy (meth)acrylate (A3)
[0149] Acrylic / epoxy hybrid resin (manufactured by Neo Chemical, BFEA-50, epoxy equivalent 470 g / eq)
[0150] 1-2. Thermosetting agent (B)
[0151] · Amine adduct-based thermal latent curing agent (Amicure PN-50 manufactured by Ajinomoto Fine Technologies Co., Ltd. ("Amicure" is a registered trademark of Ajinomoto Co., Ltd.)
[0152] 1-3. Photopolymerization initiator (C)
[0153] ·IRGACURE OXE-02 (manufactured by BASF Japan, oxime ester type)
[0154] 1-4. Alumina (D)
[0155] Alumina particles (D-1): manufactured by DENKA, ASFP-20 (alpha conversion rate: 10%, average particle size 0.3 μm, aspect ratio 1.1)
[0156] Alumina particles (D-2): manufactured by DENKA, ASFP-40 (alpha conversion rate: 10%, average particle size 0.4 μm, aspect ratio 1.1)
[0157] Alumina particles (D-3): ASFP-03S (alpha conversion rate: more than 99%, average particle size 0.4 μm, aspect ratio 1.1)
[0158] Alumina particles (D-4): DAW-01 manufactured by DENKA Corporation (alpha conversion rate: 5%, average particle size 1.9 μm, aspect ratio 1.1)
[0159] Alumina particles (D-5): DAW-03 manufactured by DENKA Corporation (alpha conversion rate: 30%, average particle size 4.9 μm, aspect ratio 1.1)
[0160] Alumina particles (D-6): DAW-10 manufactured by DENKA Corporation (alpha conversion rate: 50% to 80%, average particle size 12.0 μm, aspect ratio 1.1)
[0161] Alumina particles (D-7): DAW-20 manufactured by DENKA Corporation (alpha conversion rate: 50% to 80%, average particle size 24.0 μm, aspect ratio 1.1)
[0162] The alpha conversion rate and average particle size of the aluminum oxide particles were measured by the following methods.
[0163] (Determination of α-ratio)
[0164] α-phase alumina powder AA-05 (manufactured by Sumitomo Chemical Co., Ltd.) and θ-phase alumina powder Taimicron TM-100D (manufactured by Daming Chemical Co., Ltd.) were mixed in mass ratios of 0:10, 5:5, and 10:0, and the resulting powders were subjected to X-ray diffraction measurement. The integrated intensity of the α-phase peak detected at 2θ=43° was calculated, and a standard curve of the mixing ratio and the integrated intensity was prepared.
[0165] Next, the powder of aluminum oxide (D) was subjected to X-ray diffraction measurement, and the integrated intensity of the peak at 2θ=43° was calculated, and compared with the above-mentioned standard curve to obtain the content of the α phase, that is, the α conversion rate (%). It should be noted that the X-ray diffraction was performed using a JDX-3500 X-ray diffractometer (manufactured by JEOL Ltd.).
[0166] (Measurement of average particle size)
[0167] The average particle size of aluminum oxide (D) was measured by Microtrac MT3300.
[0168] (Determination of aspect ratio)
[0169] The aspect ratio of aluminum oxide (D) is obtained by selecting any 20 particles from an image measured by a scanning electron microscope (SEM), measuring the major axis and the minor axis respectively, and calculating the average major axis and the average minor axis. Then, the average major axis and the average minor axis are substituted into the following formula to calculate the aspect ratio.
[0170] Aspect ratio = average major diameter (μm) / average minor diameter (μm)
[0171] 1-5. Others
[0172] 1-5-1. Inorganic filler (E)
[0173] Silica particles: SO-C1 manufactured by Admatechs Co., Ltd.
[0174] 1-5-2. Organic particles
[0175] · Micro-particle polymer F351 (manufactured by Aica Industries)
[0176] 1-5-3. Silane coupling agent
[0177] Silane coupling agent (KBM-403, manufactured by Shin-Etsu Silicone Co., Ltd.)
[0178] 2. Preparation of Liquid Crystal Sealant
[0179] (Example 1)
[0180] Using a three-roll mill, 100 parts by mass of a thermosetting compound (A1), 140 parts by mass of a compound having an ethylenically unsaturated double bond in a molecule (A2), 400 parts by mass of a partial epoxy (meth)acrylate (A3), 100 parts by mass of a thermosetting agent (B), 10 parts by mass of a photopolymerization initiator (C), 50 parts by mass of aluminum oxide particles (D-1), 130 parts by mass of an inorganic filler (E), 60 parts by mass of organic fine particles (F), and 10 parts by mass of a silane coupling agent (G) were fully mixed to form a uniform liquid, thereby obtaining a liquid crystal sealing agent.
[0181] (Example 2 to Example 10, Comparative Example 1 to Comparative Example 2)
[0182] Except having changed the composition as shown in Table 1, it carried out similarly to Example 1, and obtained a liquid crystal sealing compound.
[0183] 3. Evaluation
[0184] About the liquid crystal sealing agent obtained in Example 1-Example 10 and Comparative Example 1-Comparative Example 2, adhesive strength, moisture permeability, and liquid crystal contamination property were evaluated by the following method.
[0185] <Adhesion Strength>
[0186] The obtained liquid crystal sealing agent was formed into a 38 mm × 38 mm square sealing pattern (cross-sectional area 2500 μm) on a 40 mm × 45 mm glass substrate (RT-DM88-PIN, manufactured by EHC) on which a transparent electrode and an alignment film were previously formed using a dispenser (Shotmaster, manufactured by Musashi Engineering). 2 ).
[0187] Next, the paired glass substrates were bonded together under reduced pressure in a manner perpendicular to the glass substrate on which the seal pattern was formed, and then bonded together by opening to the air. The two bonded glass substrates were then kept in a light-shielding box for 1 minute and then irradiated with 3000 mJ / cm 2 The sealant was cured by heating at 120° C. for 1 hour to obtain a test piece.
[0188] Using a press-in tester (Model 210, manufactured by INTESCO), the obtained test piece was vertically pressed at a speed of 5 mm / min at a position 4.5 mm from the corner of the seal pattern. The above operation was performed on 10 glass substrates (n=10), and the number of glass substrates that were broken was counted. Then, the bonding strength was evaluated according to the following criteria.
[0189] ◎: The number of glass substrates that were broken was 7 to 10
[0190] ○: The number of glass substrates that were broken was 1 to 6
[0191] ×: The number of glass substrates that were broken was 0
[0192] The greater the number of broken glass substrates, the higher the adhesive strength can be judged to be. If it is ○ or more, it is a level with no practical problems and is judged to be good.
[0193] <Moisture permeability>
[0194] The obtained liquid crystal sealing agent was applied to a release paper with a thickness of 300 μm using an applicator. After that, the applied sealing agent was placed in a nitrogen replacement container and nitrogen purged for 5 minutes, and then irradiated with 3000 mJ / cm 2 The film was exposed to light (light calibrated by a sensor with a wavelength of 365 nm) and then heated at 120° C. for 1 hour to produce a cured film.
[0195] Two cured films were placed on an aluminum cup sealed with calcium chloride (anhydrous) as a moisture absorbent, and then an aluminum ring was placed and screwed in, and then the initial weight of the entire aluminum cup was measured. After that, the aluminum cup was placed in a constant temperature bath set at 60°C 90%Rh, and after 24 hours, the aluminum cup was taken out and the weight was measured. The obtained weight value was substituted into the following calculation formula to calculate the moisture permeability.
[0196] Calculation formula:
[0197] Water vapor permeability = (weight after test - weight before test) × film thickness / (film area × 100)
[0198] Then, evaluation was performed based on the following criteria.
[0199] ◎: Moisture permeability less than 25g / m 2
[0200] ○: Moisture permeability: 25g / m 2 Above and less than 30g / m 2
[0201] ×: Moisture permeability: 30g / m 2 above
[0202] If it is ○ or more, it is a level without any practical problem and is judged to be good.
[0203] <Liquid crystal contamination>
[0204] The obtained liquid crystal sealing agent was formed into a 35 mm × 35 mm square sealing pattern (cross-sectional area 3500 μm) on a 40 mm × 45 mm glass substrate (RT-DM88-PIN, manufactured by EHC) on which a transparent electrode and an alignment film were previously formed using a dispenser (Shotmaster, manufactured by Musashi Engineering). 2 ) as the main seal, and a 38mm×38mm quadrilateral sealing pattern is formed on its periphery.
[0205] Next, use a dispensing machine to precisely drip a liquid crystal material (MLC-6609-000, manufactured by Merck) equivalent to the amount of the panel after bonding into the frame of the main seal. Next, bond the paired glass substrates under reduced pressure and then open them to the atmosphere. Then, keep the two bonded glass substrates in a light-shielding box for 1 minute, and then use a 36mm×36mm quadrilateral substrate coated with a black matrix to shield the main seal. In this state, irradiate 500mJ / cm 2The main seal was cured by irradiating the liquid crystal cell with light containing visible light (light with a wavelength of 370 nm to 450 nm) and then heating at 120°C for 1 hour. After that, polarizing films were attached to both sides of the obtained liquid crystal cell to obtain a liquid crystal display panel. Then, the liquid crystal contamination was evaluated according to the following criteria.
[0206] ◎: The liquid crystal is aligned until the main seal edge of the LCD panel, and there is no color unevenness at all
[0207] ○: Color unevenness occurs within a range of less than 0.5 mm near the main seal edge
[0208] Δ: Color unevenness occurs in the range of 0.5 mm to less than 1 mm near the main seal edge
[0209] ×: Color unevenness occurs in an area of 1 mm or more from the vicinity of the main seal edge
[0210] If it is Δ or more, it is a level that does not cause any practical problems and is judged to be good.
[0211] Table 1 shows the evaluation results of the liquid crystal sealing agents of Example 1 to Example 10 and Comparative Example 1 to Comparative Example 2.
[0212] [Table 1]
[0213]
[0214] As shown in Table 1, all of the liquid crystal sealing agents of Examples 1 to 10 containing aluminum oxide having an alpha conversion rate of 80% or less showed high bonding strength with the substrate while maintaining a low moisture permeability.
[0215] In particular, it is known that by reducing the average particle size of aluminum oxide to 3.0 μm or less, color unevenness can be further reduced (comparison of Examples 1, 4, 5, and 8). In addition, it is known that by setting the content of aluminum oxide to a predetermined value or less, color unevenness can be further suppressed (comparison of Examples 1 to 3 and 7).
[0216] In contrast, the liquid crystal sealing agent of Comparative Example 2 containing aluminum oxide (D-3) having an alpha conversion rate exceeding 80% has low bonding strength to the substrate. In addition, the liquid crystal sealing agent of Comparative Example 1 containing no aluminum oxide has a large amount of moisture permeability and low bonding strength to the substrate.
[0217] This application claims the priority based on Japanese Patent Application No. 2022-048549 filed on March 24, 2022. The contents described in the specification of that application are hereby incorporated by reference in their entirety.
[0218] Industrial Applicability
[0219] The liquid crystal sealing agent of the present invention can form a sealing member having high adhesive strength with a substrate while having high moisture resistance. Therefore, the liquid crystal sealing agent is very useful as a liquid crystal sealing agent for a liquid crystal dropping process in particular.
Claims
1. A liquid crystal sealing agent comprising a curable compound (A), a thermosetting agent (B) and / or a photopolymerization initiator (C), and aluminum oxide (D) having an alpha conversion rate of 80% or less.
2. The liquid crystal sealant according to claim 1, in, The average particle size of the aluminum oxide (D) is 0.01 μm to 3 μm.
3. The liquid crystal sealant according to claim 1, in, The content of the aluminum oxide (D) is 1 to 20 parts by mass relative to 100 parts by mass of the sclerosing compound (A).
4. The liquid crystal sealant according to claim 1, in, The aspect ratio of the aluminum oxide (D) is 2.0 or less.
5. The liquid crystal sealant according to claim 1, in, The aluminum oxide (D) is in a particle form.
6. The liquid crystal sealant according to claim 1, comprising: As the curable compound (A), a thermosetting compound (A1) having an epoxy group in the molecule, and The thermal curing agent (B).
7. The liquid crystal sealing agent according to claim 6, in, The content of the thermosetting compound (A1) is 5 to 20 parts by mass based on 100 parts by mass of the curable compound (A).
8. The liquid crystal sealant according to claim 6, in, The content of the thermosetting agent (B) is 10 parts by mass or more relative to 100 parts by mass of the curable compound (A).
9. The liquid crystal sealing agent according to claim 6, in, The thermal curing agent (B) includes at least one selected from the group consisting of dihydrazide-based thermal latent curing agents, imidazole-based thermal latent curing agents, amine adduct-based thermal latent curing agents, and polyamine-based thermal latent curing agents.
10. The liquid crystal sealant according to claim 6, further comprising: The curable compound (A) includes a compound (A2) having an ethylenically unsaturated double bond in the molecule, and The photopolymerization initiator (C), and The content ratio of the thermosetting compound (A1) to the compound (A2), ie, A1 / A2, is 30 / 70 to 50 / 50 in terms of mass ratio. 11 . The liquid crystal sealing agent according to claim 6 , further comprising a partial epoxy (meth)acrylate (A3) as the curable compound (A).
12. The liquid crystal sealant according to claim 1, in, The photopolymerization initiator (C) includes at least one selected from the group consisting of oxime ester compounds, thioxanthone compounds, and anthraquinone compounds. 13 . The liquid crystal sealant according to claim 1 , further comprising a coupling agent. The liquid crystal sealing agent according to claim 1 , which is a liquid crystal sealing agent for a liquid crystal dropping method.
15. A method for manufacturing a liquid crystal display panel, include: forming a sealing pattern of the liquid crystal sealing agent according to claim 1 on a substrate; A step of dropping liquid crystal in a region of the seal pattern or on another substrate paired with the one substrate while the seal pattern is not solidified; a step of overlapping the one substrate and the other substrate via the seal pattern; and A step of curing the seal pattern.
16. The method for manufacturing a liquid crystal display panel according to claim 15, in, The step of curing the seal pattern includes the step of irradiating the seal pattern with light to cure the seal pattern.
17. The method for manufacturing a liquid crystal display panel according to claim 16, in, The light irradiated onto the seal pattern includes light in the visible light region.
18. The method for manufacturing a liquid crystal display panel according to claim 17, in, The step of curing the seal pattern further includes a step of heating and curing the seal pattern irradiated with light.
19. A liquid crystal display panel, include: a pair of base plates; a frame-shaped sealing member disposed between the pair of substrates; as well as a liquid crystal layer filling a space between the pair of substrates and surrounded by the sealing member, and The said sealing member contains the hardened|cured material of the liquid crystal sealing agent of Claim 1.