Method for producing r-t-b sintered magnet

By using a metal wire saw to cut the powder molded body of RTB sintered magnets in liquid, the problems of high processing difficulty and complex equipment in the prior art are solved, and efficient and low-cost mass production and complex shape processing are realized.

CN118901110APending Publication Date: 2024-11-05PROTERIAL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028876.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-02-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing RTB-based sintered magnets are difficult to process, especially since the cutting process requires an inert gas environment, resulting in complex equipment that is not suitable for large-scale production.

Method used

A wire saw using metallic wire in liquid is employed for cutting. By controlling the wire's travel speed and tension, the powder molded body is cut in the liquid to form multiple cut surfaces, including flat and curved surfaces, thus avoiding dependence on inert gas environments.

Benefits of technology

It enables efficient cutting of powder molded parts in a conventional gas environment, improving production efficiency, reducing manufacturing costs, and enabling the processing of complex shapes, while avoiding performance degradation caused by oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901110A_ABST
    Figure CN118901110A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing an R-T-B sintered magnet, comprising: a pulverization step for preparing a powder of an alloy for an R-T-B sintered magnet; a molding step for producing a powder molded body using the powder; a cutting step for cutting the powder molded body into a plurality of molded body pieces; and a sintering step in which each of the plurality of molded body sheets is sintered to produce a plurality of sintered bodies. The cutting step includes a step of forming one or more cut surfaces including a curved surface by cutting the powder molded body immersed in the liquid with a wire traveling in a horizontal direction and moving the wire in an arbitrary cutting direction perpendicular to the traveling direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing an RTB based sintered magnet. Background Art

[0002] RTB sintered magnets (R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is at least one transition metal and must contain Fe, and B is boron) include R2Fe 14 The main phase of the compound with B-type crystal structure, the grain boundary phase located at the grain boundary of the main phase, and the compound phase generated by the influence of trace added elements and impurities. r (hereinafter sometimes referred to as "B r ”) and high coercivity H cJ (Hereinafter sometimes referred to as "H cJ ”) and has excellent magnetic properties, so it is considered to be the highest performance magnet among permanent magnets. Therefore, RTB-based sintered magnets are used in a variety of applications such as voice coil motors (VCM) for hard disk drives, motors for electric vehicles (EV, HV, PHV), motors for industrial equipment, and various other motors, home appliances, etc.

[0003] Such an RTB based sintered magnet is produced, for example, through the steps of preparing alloy powder, compacting the alloy powder to produce a powder compact, and sintering the powder compact. The alloy powder can be produced, for example, by the following method.

[0004] First, an alloy is produced from a molten metal of various raw materials by a method such as an ingot casting method or a strip casting method. The obtained alloy is used in a pulverizing step to obtain an alloy powder having a predetermined particle size distribution. The pulverizing step generally includes a coarse pulverizing step and a fine pulverizing step, the former being performed, for example, by utilizing the hydrogen embrittlement phenomenon, and the latter being performed, for example, by utilizing an air flow pulverizer (jet mill).

[0005] The sintered body obtained by the process of sintering the powder molded body is then subjected to mechanical processing such as grinding and cutting to form a single piece with the desired shape and size. More specifically, the R-Fe-B rare earth magnet powder is first compressed and molded by a pressing device to produce a molded body larger than the final magnet product. Then, after the molded body is made into a sintered body by a sintering process, the sintered body is ground by, for example, a superhard alloy saw or a rotating grindstone to give it the desired shape. For example, after first making a sintered body with a block shape, the sintered body is sliced ​​with a saw and cut into a plurality of plate-like sintered body parts.

[0006] However, the sintered body of rare earth alloy magnets such as R-Fe-B system sintered magnets is not only very hard and brittle, but also has a large processing load, so high-precision grinding is a very difficult operation and requires a long processing time. Moreover, it is inevitable that part of the material will be lost due to processing. Therefore, the processing process has become an important reason for the increase in manufacturing costs.

[0007] In order to solve the former problem, for example, Patent Document 1 describes a technique for processing a magnet molded body using a wire saw before sintering. Wire sawing is a processing technique that presses a wire running in one direction or two directions against the molded body to be processed, and grinds or cuts the molded body using abrasive grains located between the wire and the molded body. This technique cuts the powder molded body, which is softer and easier to process than a sintered body, and thus significantly reduces the time required for the cutting process.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2003-303728 Summary of the invention

[0011] Problems to be solved by the invention

[0012] Patent Document 1 discloses that a powder molded body is processed in an inert gas environment in which the oxygen concentration is adjusted to 5% to 18% of the whole by molar ratio using a wire saw having an outer diameter of 0.1 mm to 1.0 mm and abrasive grains fixed to the wire. Such wire saw processing in an inert environment with controlled oxygen concentration will complicate equipment and management, which is not conducive to large-scale production.

[0013] The embodiment of the present invention provides a novel method for producing a sintered RTB based magnet that can realize a wire saw process without preparing an inert gas environment.

[0014] Technical solutions to solve problems

[0015] In an exemplary embodiment of the method for manufacturing an RTB-based sintered magnet of the present invention, the method includes: a pulverizing step of preparing a powder of an alloy for RTB-based sintered magnet (R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is at least one transition metal and must contain Fe, and B is boron); a molding step of using the above powder to make a powder molded body; a cutting step of cutting the above powder molded body to divide it into a plurality of molded body pieces; and a sintering step of sintering each of the plurality of molded body pieces to make a plurality of sintered bodies. The above cutting step includes a step of cutting the above powder molded body immersed in a liquid with a wire rod traveling in a horizontal direction, and moving the wire rod in an arbitrary cutting direction perpendicular to the traveling direction to form one or more cut surfaces including a curved surface.

[0016] In one embodiment, the cutting step includes a step of moving the wire rod running in the horizontal direction in an arbitrary cutting direction perpendicular to the running direction to thereby separate the wire rod into a plurality of molded body pieces surrounded by the plurality of cut surfaces.

[0017] In one embodiment, in the cutting step, the maximum running speed of the wire is 300 m / min or more.

[0018] In one embodiment, in the cutting step, the tension of the wire is 29.4 N (3 kgf) or more.

[0019] In one embodiment, a moving speed of the wire in the cutting direction is not less than 100 mm / min and not more than 800 mm / min.

[0020] In one embodiment, when forming the curved surface, a moving speed of the wire in the cutting direction is not less than 100 mm / min and not more than 600 mm / min.

[0021] In one embodiment, the surface of the wire is composed of metal.

[0022] In one embodiment, the step of preparing the powder molded body includes the step of molding the powder by wet pressing.

[0023] In one embodiment, the method further includes the step of recovering particles of the powder scraped off from the powder compact in the cutting step from the liquid.

[0024] Effects of the Invention

[0025] According to an embodiment of the present invention, it is possible to cut with a wire saw without preparing an inactive gas environment, and the mass production rate is excellent. In addition, the powder molded body can be processed into a curved surface. According to an embodiment of the present invention, the shape design freedom of the powder molded body is improved regardless of the mold shape of the pressing machine, so that the performance of the high-performance magnet can be maintained and the manufacturing cost can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a flowchart showing main steps of the manufacturing method according to the embodiment of the present invention.

[0027] Figure 2 This is a flowchart showing the contents of the cutting step of the manufacturing method according to the embodiment of the present invention.

[0028] Figure 3 It is a perspective view schematically showing the structure of a wire saw device used in an embodiment of the present invention.

[0029] Figure 4A This is a front view for explaining the step of cutting a powder molded body immersed in a liquid with a wire.

[0030] Figure 4B This is a front view for explaining the step of cutting a powder molded body immersed in a liquid with a metal wire.

[0031] Figure 5A This is a side view for explaining the process of cutting a powder molded body immersed in a liquid with a wire.

[0032] Figure 5B This is a side view for explaining the process of cutting a powder molded body immersed in a liquid with a wire.

[0033] Fig. 6A This is a side view for explaining the process of cutting a powder molded body immersed in a liquid with a wire.

[0034] Figure 6B This is a side view for explaining the process of cutting a powder molded body immersed in a liquid with a wire.

[0035] Fig. 7A The figure schematically shows a cut surface formed on the powder molded body 10 by a wire saw.

[0036] Figure 7B The figure schematically shows a cut surface formed on the powder molded body 10 by a wire saw.

[0037] Figure 7C The figure schematically shows a cut surface formed on the powder molded body 10 by a wire saw.

[0038] Fig. 8A This is a diagram schematically showing another example of a cut surface formed on the powder molded body 10 by a wire saw.

[0039] Figure 8B This is a diagram schematically showing another example of a cut surface formed on the powder molded body 10 by a wire saw.

[0040] Figure 8C This is a diagram schematically showing another example of a cut surface formed on the powder molded body 10 by a wire saw.

[0041] Fig.8D This is a diagram schematically showing another example of a cut surface formed on the powder molded body 10 by a wire saw.

[0042] Fig. 8E This is a diagram schematically showing another example of a cut surface formed on the powder molded body 10 by a wire saw.

[0043] Fig.8F This is a diagram schematically showing another example of a cut surface formed on the powder molded body 10 by a wire saw.

[0044] Fig. 9 It is a graph showing how the wire running speed and the cutting speed affect the shape of the molded body sheet.

[0045] Fig.10 It is a graph showing how the wire running speed and the cutting speed affect the shape of the molded body sheet.

[0046] Fig.11 This is a graph showing how the wire running speed affects the shape of a formed body sheet having a curved surface.

[0047] Fig.12 This is a graph showing how the wire running speed affects the shape of a formed body sheet having a curved surface. DETAILED DESCRIPTION

[0048] The following is an explanation of an embodiment of the method for producing a sintered RTB magnet according to the present invention. Figure 1 and Figure 2 As shown in the flowchart, it includes:

[0049] A pulverizing step (S10) of preparing a powder of an alloy for RTB-based sintered magnet (R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is at least one transition metal and must contain Fe, and B is boron);

[0050] A molding step (S20) of producing a powder molded body using the powder obtained in the pulverizing step (S10);

[0051] a cutting step (S30) of cutting the powder compact into a plurality of compact pieces; and

[0052] A sintering step (S40) of sintering each of the plurality of compact sheets to produce a plurality of sintered bodies.

[0053] The cutting process (S30) includes: using a moving wire to cut the above-mentioned powder molded body immersed in a liquid to form a first cutting surface, a first processing process (S32); and using a moving wire that is the same as or different from the above-mentioned wire to cut the powder molded body immersed in a liquid that is the same as or different from the above-mentioned liquid to form a second processing process (S34) that intersects with the first cutting surface.

[0054] In a preferred embodiment, the cutting step (S30) includes cutting with a wire rod traveling in a horizontal direction, and moving the wire rod in an arbitrary cutting direction perpendicular to the traveling direction to form one or more cutting surfaces including a curved surface. The cutting step (S30) may include a step of dividing the wire rod traveling in a horizontal direction into a plurality of molded body pieces surrounded by a plurality of cutting surfaces including a curved surface by moving the wire rod traveling in a horizontal direction in an arbitrary cutting direction perpendicular to the traveling direction.

[0055] According to the method for producing a sintered RTB magnet of the present invention, the powder compact is cut with a wire while being immersed in a liquid, so there is no need to prepare an inert gas environment. Examples of liquids that can be used in the embodiments of the present invention include oils such as mineral oil and synthetic oil.

[0056] In the prior art, in order to cut a powder molded body using wire saw technology, it is believed that the hard abrasive grains fixed to the surface of the metal wire constituting the wire must be brought into contact with the powder molded body, and a part of the powder molded body must be scraped off by friction. However, according to the experimental results of the inventors of the present invention, when the traveling metal wire contacts the powder molded body immersed in the liquid, even the metal wire without abrasive grains fixed thereto can grind and cut the powder molded body. According to the research results of the inventors, a high-speed liquid flow (jet flow) is generated in the area where the metal wire traveling at a speed within a specified range contacts the powder molded body and its vicinity, thereby scraping off the powder particles constituting the powder molded body. Some of the powder particles scraped off from the powder molded body are entrained between the metal wire and the powder molded body by the high-speed flowing liquid, and exhibit the same grinding function as the free abrasive grains, thereby promoting the cutting of the powder molded body. Based on the principle that the wire can cut the powder molded body in the liquid, it can be considered that the shape and form of the wire surface are not particularly limited. In other words, the wire surface can be as smooth as an ordinary piano wire.

[0057] In the cutting process, the travel speed of the wire is preferably above 300m / min, and the wire tension at this time is preferably above 3kgf (29.4N), for example, below 15kgf (147N). If the travel speed of the wire is less than 300m / min, it will not be possible to obtain a sufficient flow rate required to cut the powder molded body. If the tension of the wire is less than 3kgf, the wire may bend and the flatness of the cut surface may be reduced. If the tension of the wire exceeds 15kgf, breakage problems may occur. In addition, in the cutting process, the cutting speed (workpiece feed speed) in the direction perpendicular to the direction of wire travel is preferably above 100mm / min. This is because if the cutting speed is less than 100mm / min, the time required for the cutting process is extended and the production efficiency is reduced.

[0058] Among them, when the wire diameter is above 200 μm, the travel speed of the wire can be set to above 500 m / min. The higher the travel speed of the wire, the higher the penetration speed can be. For example, when the wire diameter is 250 μm and the wire travel speed is above 500 m / min, the penetration speed can be set to above 150 mm / min. In addition, as described later, when forming a curved surface, the moving speed of the wire in the penetration direction is preferably above 100 mm / min and below 600 mm / min.

[0059] One advantage of cutting the powder molded body in liquid is that it can suppress the temperature rise caused by frictional heat at the contact point between the powder molded body and the wire, and the generated heat can also be easily diffused in the liquid. If the powder molded body reaches a high temperature due to the frictional heat generated in the air, it will react with oxygen or water vapor in the air, resulting in an increase in the oxygen concentration in the final sintered magnet and deterioration of the magnet performance. However, these problems can be avoided in this embodiment.

[0060] Another advantage of cutting the powder molded body in a liquid is that the powder particles scraped off from the powder molded body by the wire are precipitated in the liquid and can be easily recovered. In a preferred embodiment, the step of preparing the powder molded body includes a step of molding the powder by wet pressing. In this case, the wet pressing is preferably performed by adding a liquid of the same type as the liquid in the cutting step to the above-mentioned powder. This is because the powder particles scraped off from the powder molded body by the cutting step can be easily recovered from the liquid and reused.

[0061] In addition, according to the manufacturing method of the RTB-based sintered magnet of the present invention, since horizontal transverse cutting is performed before vertical cutting, the surface of the powder molded body can be processed to be flat. Sometimes at least a portion of the surface of the powder molded body (for example, the upper surface) will have unevenness due to the powder pressing process, and it is necessary to cut or grind it through processing after the sintering process. According to an embodiment of the present invention, such a cutting or grinding process can be omitted, so the characteristics of the high-performance magnet can be maintained and the manufacturing cost can be reduced.

[0062] Reference Figure 3 A configuration example of a wire saw device that can be used in the above-mentioned manufacturing method will be described. Figure 3 1 is a perspective view showing a structural example of a wire saw device 100 according to an embodiment of the present invention. For reference, the figure shows an X-axis, a Y-axis and an X-axis which are perpendicular to each other. In this example, the XY plane points to the horizontal direction, and the Z axis points to the vertical direction.

[0063] Figure 3 The wire saw device 100 comprises: rollers 30a, 30b, 30c arranged in a manner that the central axes of rotation are parallel to each other and a continuous wire 40. The rollers 30a, 30b and 30c are each supported by a supporting device 50 in a rotatable manner. The supporting device 50 can be moved in the vertical longitudinal direction (positive and negative directions of the Z axis) by a driving device not shown in the figure. The driving device can obtain driving force through a hydraulic cylinder, or it can work by a motor. In addition, in order to cut along the horizontal lateral direction (X-axis direction) described later, the supporting device 50 can also be moved in the horizontal lateral direction.

[0064] The powder molded body 10 produced in the molding step (S20) is fixed to the fixing base 20 by a jig (not shown) and is arranged inside the tank 70 storing the liquid 60. Figure 3 In FIG. 7 , the groove 70 is represented by a dashed line, and the height of the surface of the liquid 60 is represented by a dotted line. Figure 3 In this example, the powder molded body 10 is entirely immersed in the liquid 60. However, the fixing base 20 may be configured to move in the vertical direction and in the horizontal direction instead of the supporting device 50 moving in the vertical direction and in the horizontal direction.

[0065] The specific example of the process of making the powder compact 10 is described below. It should be noted here that the powder compact 10 is not a sintered body, but a compact (compact) of the powder before sintering. The powder compact is obtained by compacting the powder of the RTB-based sintered magnet alloy (R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is at least one transition metal and must contain Fe, and B is boron) in an oriented magnetic field by wet pressing or dry pressing.

[0066] Rollers 30a, 30b and 30c are arranged at predetermined intervals in a manner that the central axis of rotation is located at the vertices of the triangle when viewed from a direction parallel to the X-axis. A plurality of grooves are provided on the side surfaces of each of rollers 31a, 31b and 31c. Wire 40 is wound around the plurality of grooves of rollers 30a, 30b and 30c in sequence. The center interval (pitch) of the plurality of grooves defines the width of the element to be cut by the wire saw. Both ends of wire 40 are wound around, for example, a recovery bobbin not shown.

[0067] The wire 40 of the embodiment of the present invention is a metal wire with no fixed abrasive grains fixed on the surface. In the existing wire saw technology, the wire has a wire (core wire) and abrasive grains located on the outer peripheral surface of the wire. The average particle size of the abrasive grains ranges from several microns to tens of microns, for example. A typical example of such abrasive grains is artificial diamond, which has a higher hardness than rare earth alloys. Unlike the wire portion used in such existing wire saw technology, the wire 40 of the present embodiment is formed of a metal material such as carbon steel, and can be used in a non-stretched state even if a tension of, for example, 3.0 kgf or more is applied during the cutting process. The material of the metal wire that can be used for the wire 40 can be, for example, piano wire, high-tension steel wire, etc. The surface of the wire 40 can be electroplated. The diameter of the wire 40 is, for example, in the range of 100 μm to 350 μm, preferably in the range of 180 μm to 300 μm. When the diameter of the wire 40 is less than 100 μm, there is a problem that the wire 40 stretches during cutting due to insufficient strength. The larger the diameter of the wire 40 is, the better the chip discharge performance is. However, since the amount of chips increases, the diameter is preferably 350 μm or less.

[0068] During cutting, the rollers 30a, 30b, 30c and the recovery spool rotate. The direction of rotation of the rollers 30a, 30b, 30c depends on their configuration and the way the wire 40 is hung. Figure 3 In the illustrated wire saw device 100 , the rollers 30 a , 30 b , and 30 c rotate in the same direction.

[0069] After the wire 40 of a predetermined length is wound on a recovery bobbin, the recovery bobbin and the rollers 30a, 30b and 30c are rotated in the opposite direction. In this way, the wire 40 moves in the opposite direction, and by repeating this operation, the reciprocating motion (movement) of the wire 40 can be achieved.

[0070] In the present embodiment, the step of cutting the powder molded body 10 with the wire 40 is performed while the powder molded body 10 is immersed in the liquid 60. When the powder molded body 10 is formed by wet pressing, a preferred example of the liquid 60 is an oil of the same type as the dispersion medium such as an oil (mineral oil or synthetic oil) used for wet pressing.

[0071] When processing the powder compact 10 using such a wire saw device 100, the powder particles constituting the powder compact 10 form chips and fall off from the portion cut by the wire 40. These chips are formed by the powder particles constituting the powder compact 10 falling off from the powder compact 10, and do not each have a rough fracture surface like metal chips (cutting debris). The shape and size of the particles constituting the chips scraped off from the pre-sintered powder compact by the wire are the same as the shape and size of the powder particles used to make the powder compact 10. The inventors of the present invention have studied the reuse of such chips. When cutting a hard sintered body obtained by sintering a powder compact, these chips are particles or particle aggregates whose particles have grown due to sintering or whose composition has changed due to a chemical reaction. Therefore, even if they are mixed with the powder of a rare earth magnet and reused, the magnet performance is likely to deteriorate. On the other hand, chips obtained from a pre-sintered powder compact are the same in composition and size as other particles contained in the powder compact, and thus are easily reused.

[0072] In addition, when the powder compact 10 is produced by wet pressing, if wire sawing is performed in an oil agent of the same type as the dispersant, the recovered powder (chips) can be directly used for wet pressing, improving the production efficiency.

[0073] The manufacturing method of the R-T-B sintered magnet according to the present embodiment will be described in detail below.

[0074] S10: Crushing process

[0075] In the crushing process (S10), a powder of an alloy for an R-T-B sintered magnet is prepared. The composition of the alloy for an R-T-B sintered magnet, the manufacturing process of the alloy, and the process of preparing the alloy powder will be described in sequence below.

[0076] <Composition of alloy for R-T-B sintered magnet>

[0077] R is a rare earth element and must contain at least one selected from Nd, Pr, and Ce. It is preferably a combination of rare earth elements represented by Nd-Dy, Nd-Tb, Nd-Dy-Tb, Nd-Pr-Dy, Nd-Pr-Tb, Nd-Pr-Dy-Tb, Nd-Ce-Dy, Nd-Ce-Tb, Nd-Ce-Dy-Tb, Nd-Pr-Ce-Dy, Nd-Pr-Ce-Tb, Nd-Pr-Ce-Dy-Tb.

[0078] In R, Dy and Tb increase H cJIt is particularly effective in terms of... In addition to the above elements, other rare earth elements such as La may also be contained, and mixed rare earth metals or praseodymium-neodymium alloys may also be used. In addition, R may not be a pure element and may also contain impurities inevitable in the manufacturing process within the industrial accessibility range. Its content is, for example, 27% by mass or more and 35% by mass or less. Preferably, the R content of the R-T-B system sintered magnet is 31% by mass or less (27% by mass or more and 31% by mass or less, preferably 29% by mass or more and 31% by mass or less). By having the R content of the R-T-B system sintered magnet be 31% by mass or less and the oxygen content be 500 ppm or more and 3500 ppm or less (preferably 500 ppm or more and 3200 ppm or less, more preferably 500 ppm or more and 2500 ppm or less), higher magnetic properties can be obtained.

[0079] T contains iron (including the case where T consists essentially of iron), and up to 50% of it by mass ratio can be replaced by cobalt (Co) (including the case where T consists essentially of iron and cobalt). Co can effectively improve the temperature performance and corrosion resistance, and the alloy powder may contain 10% by mass or less of Co. The T content may account for the remainder of R and B, or the remainder of R, B, and M described below.

[0080] The content of B can be a known content. For example, the range of 0.9% by mass to 1.2% by mass is a preferred range. When it is less than 0.9% by mass, sometimes high H cJ cannot be achieved, while when it is more than 1.2% by mass, B r may decrease. Among them, a part of B can be replaced by C (carbon).

[0081] In addition to the above elements, in order to improve H cJ , an M element may also be added. The M element is one or more selected from Al, Si, Ti, V, Cr, Mn, Ni, Cu, Zn, Ga, Zr, Nb, Mo, In, Sn, Hf, Ta, and W. The addition amount of the M element is preferably 5.0% by mass or less. This is because once it exceeds 5.0% by mass, B r may decrease. In addition, inevitable impurities are also allowed.

[0082] The N (nitrogen) content in the R-T-B system sintered magnet is preferably 50 ppm or more and 600 ppm or less. In addition, the C (carbon) content in the R-T-B system sintered magnet is preferably 50 ppm or more and 1000 ppm or less.

[0083] <Manufacturing process of the alloy for the R-T-B system sintered magnet>

[0084] The manufacturing process of the alloy for RTB-based sintered magnets is illustrated. The metal or alloy pre-adjusted to the above composition can be melted and the alloy ingot can be obtained by an ingot casting method of injecting into a mold. In addition, the alloy flakes can be produced by a strip casting method or a quenching method represented by a centrifugal casting method, which makes the molten liquid contact with a single roll, double roll, rotating disk or rotating cylindrical mold for quenching to produce a thinner solidified alloy than the alloy produced by the ingot casting method.

[0085] In an embodiment of the present invention, materials obtained by either ingot casting or quenching can be used, but preferably manufactured by a quenching method such as a strip casting method. The thickness of the quenched alloy obtained by the quenching method is generally in the range of 0.03 mm to 1 mm and is in the form of a sheet. The alloy melt solidifies from the surface (roller contact surface) contacted by the cooling roller, and the crystal grows in a columnar shape from the roller contact surface along the thickness direction. Compared with the alloy (ingot alloy) obtained by the conventional ingot casting method (mold casting method), the quenched alloy can be cooled in a short time, so the structure is refined and the crystal grain size is small. And the grain boundary area is large. Since the R-rich phase expands greatly within the grain boundary, the R-rich phase of the quenching method has excellent dispersibility. Therefore, it is easy to produce fractures at the grain boundary using the hydrogen pulverization method. By hydrogen pulverizing the quenched alloy, the size of the hydrogen pulverized powder (coarse pulverized powder) can reach, for example, less than 1.0 mm. The coarse pulverized powder obtained in this way can be finely pulverized using, for example, a jet mill.

[0086] <Step of Preparing Powder of RTB Based Sintered Magnet Alloy>

[0087] The rare earth alloy powder used in RTB-based sintered magnets is an active powder that is easily oxidized. Therefore, in order to avoid the risk of heat generation and ignition, reduce the content of oxygen as an impurity, and achieve high performance of the magnet, inert gases such as nitrogen, argon, and helium can be used as the gas used in the jet mill.

[0088] The material to be crushed (coarsely crushed powder) put into the jet mill is crushed into fine powders with a particle size distribution such as an average particle size (median particle size d50) of 2.0 μm or more and 4.5 μm or less, and then transferred to a cyclone collector. The cyclone collector is used to separate the powder from the airflow that transports the powder. Specifically, the coarsely crushed powder of the alloy for RTB-based sintered magnet is crushed in the front-stage jet mill, and the fine powder generated by the crushing is supplied to the cyclone collector together with the gas used for the crushing. The mixture of the inert gas (crushing gas) and the crushed fine powder forms a high-speed airflow and is sent to the cyclone collector. The cyclone collector is used to separate these crushing gases from the fine powder. The fine powder separated from the crushing gas is recovered by the powder collector.

[0089] S20: Forming process

[0090] In the molding step ( S20 ), a powder molded body is produced using the powder obtained in the pulverizing step ( S10 ).

[0091] In this embodiment, the powder molded body is produced from the above-mentioned powder by pressing in a magnetic field. From the perspective of suppressing oxidation, the pressing in a magnetic field is preferably performed by pressing in an inert gas environment or wet pressing to form a powder molded body. In particular, in wet pressing, the surface of the particles constituting the powder molded body is coated with a dispersant such as an oil agent, which can suppress contact with oxygen or water vapor in the atmosphere. Therefore, it is possible to prevent or suppress oxidation of the particles by the atmosphere before, during, or after the pressing process.

[0092] In the case of wet pressing in a magnetic field, a slurry in which a dispersion medium is mixed with fine powder is prepared, supplied to the cavity of a wet pressing device mold, and pressed in a magnetic field. The powder molded body thus formed has a density of, for example, 4 g / cm 3 Above 5g / cm 3 The following density.

[0093] Dispersion medium

[0094] The dispersion medium is a liquid in which the alloy powder can be dispersed to obtain a slurry.

[0095] As the preferred dispersion medium used in the present invention, mineral oil or synthetic oil can be cited. The type of mineral oil or synthetic oil is not limited, but once the kinematic viscosity at room temperature exceeds 10 cSt, the bonding force between the alloy powders will increase due to the increase in viscosity, which sometimes has an adverse effect on the orientation of the alloy powder during wet molding in a magnetic field. Therefore, the kinematic viscosity of the mineral oil or synthetic oil at room temperature is preferably 10 cSt or less. In addition, when the fractionation temperature of the mineral oil or synthetic oil exceeds 400°C, it may cause difficulty in degreasing after obtaining the molded body, increase the amount of residual carbon in the sintered body, and reduce the magnetic properties. Therefore, the fractionation temperature of the mineral oil or synthetic oil is preferably 400°C or less. In addition, vegetable oil can also be used as a dispersion medium. Vegetable oil refers to oil extracted from plants, and the plant species are not limited to specific plants.

[0096] ·Slurry preparation

[0097] The obtained alloy powder is mixed with a dispersion medium to obtain a slurry.

[0098] The mixing ratio of the alloy powder and the dispersion medium is not particularly limited, but the concentration of the alloy powder in the slurry is preferably 70% or more (i.e., 70% by mass or more). 3At a flow rate of 1 / sec, not only can the alloy powder be efficiently supplied to the inside of the mold cavity, but also excellent magnetic properties can be obtained. The concentration of the alloy powder in the slurry is preferably less than 90% by mass ratio. There is no particular restriction on the mixing method of the alloy powder and the dispersion medium. The alloy powder and the dispersion medium can be prepared separately, and the two can be weighed and mixed in a specified amount to produce. In addition, when the coarse pulverized powder is dry-pulverized by a jet mill or the like to obtain the alloy powder, a container equipped with a dispersion medium can be configured at the alloy powder discharge port of the pulverizing device such as a jet mill, and the alloy powder obtained by the pulverization is directly recovered into the dispersion medium in the container to obtain a slurry. In this case, it is preferred that the container is also set to an environment formed by nitrogen and / or argon gas, so that the obtained alloy powder is not in contact with the atmosphere and is directly recovered into the dispersion medium to form a slurry. In addition, a vibration mill, a ball mill or a stirred mill can be used to perform wet pulverization while the coarse pulverized powder is maintained in the dispersion medium to obtain a slurry consisting of an alloy powder and a dispersion medium.

[0099] By molding the slurry thus obtained using a known wet pressing device, a powder molded body having a predetermined size and shape can be obtained. In the prior art, the powder molded body is usually sintered to obtain a sintered body, but in this embodiment, as described below, the powder molded body is divided using a wire saw device before sintering.

[0100] S30: Cutting process

[0101] In the cutting step ( S30 ), the powder compact is cut and divided into a plurality of compact pieces.

[0102] First, a method of forming a cut surface on a plane by forming a cut vertically or horizontally will be described, and then a method of forming a cut surface extending obliquely or a curved cut surface will be described.

[0103] The cutting of the powder compact in this step is performed by, for example, Figure 3 The wire saw device shown is carried out. Figure 4A and 4B Each of them is a front view for explaining a step of cutting the powder molded body 10 immersed in the liquid 60 by the wire 40 . Figure 4A Indicates the state before the cutting process begins. Figure 4B Indicates the status of the cutting process in progress. Figure 4B The dashed line in the powder molded body 10 schematically indicates the position of the wire 40 during cutting of the powder molded body 10. When the position of the wire 40 indicated by the dashed line moves downward from the upper surface of the powder molded body 10 and reaches the bottom surface of the powder molded body 10, the powder molded body 10 is divided into a plurality of molded body pieces.

[0104] In the example shown in the figure, the wire 40 moves in a direction perpendicular to the moving direction of the wire 40 (negative direction of the Z axis) while moving at a predetermined speed in the Y-axis direction. The direction perpendicular to the moving direction of the wire 40 is the cutting direction, and the speed in this direction (cutting speed) is set to, for example, 100 mm / min or more. Figure 4B In the example shown, the advancing wire 40 moves in the negative direction of the Z axis relative to the stationary powder molded body 10 , but the powder molded body 10 may be lifted in the positive direction of the Z axis together with the fixing base 20 .

[0105] Figure 5A and 5B Each of them is a side view for explaining a process of cutting the powder molded body 10 immersed in the liquid 60 by the wire 40 . Figure 5A Indicates the state before the cutting process begins. Figure 5B The figure shows a state in the middle of the cutting process. In the example shown in the figure, one powder compact 10 is divided into eight compact pieces.

[0106] The diameter of the wire 40 is, for example, 100 μm to 350 μm. The running speed of the wire 40 (wire speed) can be set within a range of, for example, 100 m / min to 800 m / min. Figure 3 The feed speed of the wire relative to the powder molded body 10 in the negative direction of the Z axis can be set within a range of, for example, 100 mm / min to 600 mm / min. The tension applied to the wire 40 is, for example, 3 kgf to 15 kgf. The tension can be adjusted by, for example, adjusting the relative distance between the roller 30c and the rollers 30a and 30b. By cutting with a wire saw, the powder molded body 10 can be divided into molded body sheets with a thickness of, for example, about 1 to 10 mm. The thickness of the molded body sheet is as follows: Figure 5B The distance shown is determined by the spacing of the wires 40 and the diameter of the wires 40 .

[0107] By performing the wire sawing process in liquid, there is also the advantage of promoting the discharge of cutting chips. In addition, as described above, by performing the wire sawing process in a state where the powder molded body 10 is immersed in the dispersion medium (mineral oil or synthetic oil) used when the powder molded body 10 is produced by wet pressing (cutting in oil), the powder particles precipitated in the liquid during the wire sawing process can be recovered, and the recovered powder particles can be directly reused in the molding process.

[0108] Fig. 6A and 6B 4 is a side view for explaining the process of cutting the powder molded body 10 immersed in the liquid 60 in the horizontal direction with the wire 40. In the example shown in the figure, in the cutting process, the rollers 30a, 30b and 30c move relative to the powder molded body 10 in the horizontal direction (the direction of the rotation axis of each roller). Figures 4A to 5B Before the described process, the surface of the powder molded body 10 can be flattened by cutting in the horizontal direction with the wire 40. At least a portion of the surface of the powder molded body 10 (for example, the upper surface) sometimes has unevenness due to the powder pressing process. For example, after the powder is filled in the die hole of the powder pressing device and before the powder is pressed with the punch, a "filter cloth" may be arranged between the punch and the powder to allow the dispersant (oil agent) to be discharged through the filter cloth. In this case, the upper surface of the obtained powder molded body may be uneven due to the filter cloth.

[0109] In the embodiment of the present invention, since such an uneven surface is cut away by a wire rod before the sintering step, it is possible to omit a step of cutting or polishing for planarization after the sintering step.

[0110] Figures 7A to 7C Schematically shows a cut surface formed on the powder molded body 10 by a wire saw. Fig. 6A and 6B In the process described (first processing process), the wire 40 is moved along Fig. 7A The dotted line 11c moves relative to the powder molded body 10 immersed in the liquid 60, so that the rough surface area 10T of the powder molded body 10 is thinly cut to form a first cut surface 11 perpendicular to the Z-axis direction. Then, by referring to Figure 5A and Figure 5B The described process (second processing process) forms a plurality of second cut surfaces 12 intersecting with the first cut surface 11. In the second processing process, the second cut surface 12 is formed by the traveling wire moving along the dotted line 12c. The first processing process and the second processing process may be performed using the same wire saw device, or may be performed using different wire saw devices. In other words, the second processing process may be cut using the same wire while immersed in the same liquid as the liquid in which the powder molded body is immersed in the first processing process, or may be cut using different wires while immersed in different liquids.

[0111] exist Figure 7A to Figure 7C In the example shown, the first cut surface 11 is parallel to the horizontal plane, and the second cut surface 12 is orthogonal to the first cut surface 11. The directions of the first cut surface 11 and the second cut surface 12 are not limited to this example.

[0112] The second cutting speed is preferably, for example, not less than 100 mm / min and not more than 800 mm / min.

[0113] Among them, before the second processing step of cutting the powder molded body in the liquid in the vertical direction, the first processing step of cutting in the horizontal direction is first performed, and its technical effect is not limited to the case of using a wire composed of metal wires, and can also be achieved when using a wire with abrasive grains fixed on the surface of the metal wire. However, when cutting the powder molded body in the liquid, it is preferred to cut it with a metal wire without abrasive grains fixed, because the problem caused by the falling of abrasive grains can be avoided.

[0114] Figures 8A to 8F This is a diagram for explaining a process of dividing a powder molded body 10 immersed in a liquid 60 into a plurality of molded body pieces surrounded by a plurality of cut surfaces including curved surfaces by moving a wire 40 in an arbitrary cutting direction perpendicular to the traveling direction. In the example shown in the figure, in the cutting process, the rollers 30a, 30b, 30c and the support device 50 that rotate the wire 40 can move simultaneously in both directions relative to the Z-axis direction and the X-axis direction.

[0115] In from Fig. 8A The status changes to Figure 8B During the process of being in the state of , the wire 40 moves horizontally in the negative direction of the X axis. As a result, a horizontal cut surface is formed on the powder molded body 10.

[0116] Then from Figure 8B The status changes to Figure 8C During the process of being in the state of Z, the wire 40 moves vertically in the negative direction of the Z axis. As a result, a vertical cut surface is formed on the powder molded body 10.

[0117] Furthermore, in Figure 8C The status changes to Fig.8D In the process of the state, the wire 40 moves in the positive direction of the X axis while moving in the negative direction of the Z axis. As a result, a downward convex curved cut surface is formed on the powder molded body 10. At this time, for example, when the moving speed in the X-axis direction is constant, an arbitrary curved surface can be formed by gradually changing the moving speed in the Z-axis direction.

[0118] In from Fig.8D The status changes to Fig. 8E During the process of the state of the wire 40, the wire 40 moves in the positive direction of the X axis while moving in the positive direction of the Z axis. As a result, a downward convex curved cut surface is formed on the powder molded body 10.

[0119] Finally, from Fig. 8E The status changes to Fig.8F During the process of the state, the wire 40 moves vertically to the positive direction of the Z axis. As a result, a vertical cut surface is formed on the powder molded body 10, and a molded body piece with a downward convex fish cake shape is finally obtained.

[0120] exist Figures 8A to 8FIn the example shown, one molded body sheet is formed from one powder molded body 10, but the present invention is not limited to this example. By controlling the movement of the wire 40, a plurality of molded body sheets can also be formed from one powder molded body 10. In addition, the shape and size of the formed molded body sheet are not limited to the example shown in the figure.

[0121] S40: Sintering process

[0122] In the sintering step (S40), the plurality of molded body sheets are sintered to produce a plurality of sintered bodies. That is, the molded body sheets cut by the wire sawing step are sintered to obtain RTB-based sintered magnets (sintered bodies). The sintering step of the molded body sheets can be carried out at, for example, 0.13 Pa (10 ﹣3 Torr) or less, preferably 0.07 Pa (5.0×10 ﹣4 Torr), at a temperature range of, for example, 1000°C to 1150°C. In order to prevent oxidation due to sintering, the residual gas in the environment can be replaced with an inactive gas such as helium or argon. It is preferred to subject the obtained sintered body to additional heat treatment such as aging treatment. This heat treatment can improve the magnetic properties. The heat treatment conditions such as heat treatment temperature and heat treatment time can adopt known conditions. The RTB system sintered magnet obtained in this way is subjected to a grinding / polishing process, a surface treatment process and an excitation process as needed, and the final RTB system sintered magnet is completed.

[0123] In a preferred embodiment, the method for manufacturing an RTB-based sintered magnet of the present invention further includes a diffusion step of diffusing a heavy rare earth element RH (RH is at least one of Tb, Dy, and Ho) from the surface of the sintered body to the inside. When the heavy rare earth element RH diffuses from the surface of the sintered body to the inside, the coercive force can be efficiently improved. The method of the diffusion step is not limited, and a known method can be used.

[0124] (Example)

[0125] The raw materials of each element were weighed according to the composition of Nd: 22.6%, Pr: 7.8%, B: 0.9%, Co: 0.5%, Al: 0.1%, Cu: 0.2%, Ga: 0.4% (all by mass%), and the balance Fe, and an alloy was prepared by strip casting. The obtained alloy was hydrogen-pulverized to obtain a coarse pulverized powder.

[0126] Then, zinc stearate as a lubricant is added to the obtained coarsely pulverized powder in a ratio of 0.04 mass % relative to 100 mass % of the coarsely pulverized powder, and dry pulverized using a jet mill in a nitrogen stream to obtain a finely pulverized powder (alloy powder) with a particle size D50 of 4 μm. The finely pulverized powder is immersed in a mineral oil with a fractionation temperature of 250°C and a kinematic viscosity of 2 cSt at room temperature in a nitrogen environment to prepare a slurry. The slurry concentration is 85 mass %. The obtained slurry is molded (wet molding) in a magnetic field to produce a powder molded body. The size of the powder molded body is 80 mm × 45 mm × 60 mm.

[0127] The powder molded body was divided into 8 molded body pieces using a wire rod (metal wire formed by piano wire) with a diameter of 250 μm. The cutting with the wire saw was performed while the powder molded body was immersed in a liquid (the liquid used was the same substance as the mineral oil used during molding). Each powder molded body was cut using 8 wire rods (multi-wires) running in parallel. The tension applied to the wire rod during cutting was 10 kg, and the roller interval was 250 mm.

[0128] Fig. 9 This is a graph showing how the wire running speed and the cutting speed affect the shape of the molded body sheet. The horizontal axis of the graph is the wire running speed [m / min], and the vertical axis is the cutting speed [mm / min]. The "×" shown in the graph means that a part of the molded body sheet cut by the wire saw has a "crack", and the "○" means that the molded body sheet has no such cracks and can be divided into molded body sheets with good shapes.

[0129] When using a wire with a diameter of 250 μm, a crack-free molded body sheet can be obtained at a cutting speed of 100 to 150 mm / min at a running speed of 300 m / min. In addition, a crack-free molded body sheet can be obtained at a cutting speed of 250 mm / min at a running speed of 500 m / min. In addition, at a running speed of 700 m / min, even at a cutting speed of 400 mm / min, the wire will not bend during cutting, and a crack-free molded body sheet can be obtained. Therefore, the maximum running speed of the wire is preferably 300 m / min or more.

[0130] In addition, when a wire with a diameter of 160 μm is used, it can be divided into good molded body pieces when both the travel speed and the cutting speed are relatively low. It can be considered that the smaller the diameter of the wire, the easier it is for the wire to extend and bend, so when high tension is applied and high-speed travel is performed, the powder molded body is more likely to crack or notch when cut. Therefore, the diameter of the wire (metal wire) is preferably 200 μm or more. In addition, the larger the wire diameter, the more raw material is cut, but normal cutting can be achieved.

[0131] By comparison, it was confirmed that a powder molded body placed in the air could not be cut normally by only using a metal wire, and that the contact between the running metal wire and the powder molded body must be performed in a liquid (preferably oil).

[0132] Fig.10 Indicates Fig. 6A and Figure 6B The experimental results shown are after cutting the upper surface area of ​​the powder molded body in oil in a horizontal direction with a wire. "Lateral feed" is the horizontal cutting speed, and "wire speed" is the travel speed of the wire. When using a wire with a diameter of 250μm, a crack-free molded body sheet can be obtained at a travel speed of 300m / min and a cutting speed of 100 to 300mm / min. In addition, at a travel speed of 500m / min, a crack-free molded body sheet can be obtained at a cutting speed of 300mm to 500mm / min. In addition, even at a travel speed of 700m / min, a crack-free molded body sheet can be obtained at a cutting speed of 500mm / min.

[0133] When cutting the upper surface of the powder molded body by "lateral feeding", it is preferred that the powder molded body has sufficient "hardness". The hardness of the powder molded body can be evaluated by, for example, the molding pressure or density during powder molding. It is known that the density of the powder molded body is less than 4 g / cm when placed in air. 3 Therefore, the density of the powder molded body is preferably 4g / cm 3 above.

[0134] Fig.11 and Fig.12 Each of the graphs shows how the moving speed of the wire in the cutting direction affects the shape of the molded body sheet having a curved surface when forming a molded body sheet in a kamaboko-shaped shape. Fig.11 The data in the figure are obtained when the wire tension is 9kgf (88.2N). Fig.12 The data in the figure are obtained when the wire tension is 12kgf (117.6N). The wire diameter is 250μm. In this example, when cutting the curved surface, the wire cuts in the direction of increasing the position (coordinate) in the X-axis direction. It can be seen that in the second half of the cut, the position of the cut surface deviates from the target position. The reason is the deflection of the wire.

[0135] According to the inventor's research, when the moving speed of the wire in the cutting direction is 100 mm / min or more and 600 mm / min or less, by adjusting the tension of the wire, it can be cut into the target curved surface shape with a good yield. The tension is preferably 9 kgf (88.2 N) or more. In addition, the moving speed of the wire in the cutting direction is preferably 540 mm / min or less.

[0136] Explanation of symbols

[0137] 10: powder molded body; 20: fixing base; 30a, 30b, 30c: rollers; 40: wire; 50: supporting device; 60: liquid; 70: groove; 100: wire saw device.

Claims

1. A method for producing a RTB based sintered magnet, characterized in that: include: A pulverizing step of preparing a powder of an alloy for RTB-based sintered magnet, wherein R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is at least one transition metal and must contain Fe, and B is boron; A molding step of using the powder to make a powder molded body; A step of cutting the powder compact into a plurality of compact pieces; and a sintering step of sintering each of the plurality of compact sheets to produce a plurality of sintered bodies; The cutting step includes a step of cutting the powder molded body immersed in a liquid by using a wire that travels in a horizontal direction, and moving the wire in an arbitrary cutting direction perpendicular to the traveling direction to form one or more cut surfaces including a curved surface.

2. The method for producing a RTB based sintered magnet according to claim 1, wherein: The cutting step includes the step of moving the wire material traveling in the horizontal direction in an arbitrary cutting direction perpendicular to the traveling direction to thereby divide the wire material into a plurality of molded body pieces surrounded by the plurality of cut surfaces.

3. The method for producing a RTB based sintered magnet according to claim 1 or 2, characterized in that: In the cutting step, the maximum running speed of the wire is 300 m / min or more.

4. The method for producing a sintered RTB based magnet according to any one of claims 1 to 3, wherein: In the cutting step, the tension of the wire is 29.4 N (3 kgf) or more.

5. The method for producing a sintered RTB based magnet according to any one of claims 1 to 4, wherein: The moving speed of the wire in the cutting direction is not less than 100 mm / min and not more than 800 mm / min.

6. The method for producing a RTB based sintered magnet according to claim 5, wherein: When forming the curved surface, the moving speed of the wire in the cutting direction is 100 mm / min to 600 mm / min.

7. The method for producing a sintered RTB based magnet according to any one of claims 1 to 6, wherein: The surface of the wire is composed of metal.

8. The method for producing a sintered RTB based magnet according to any one of claims 1 to 7, wherein: The step of preparing the powder molded body includes the step of molding the powder by wet pressing.

9. The method for producing a sintered RTB based magnet according to any one of claims 1 to 8, wherein: The method further includes a step of recovering particles of the powder scraped off from the powder compact in the cutting step from the liquid.