Electromagnetic wave detector, electromagnetic wave detector array, and image sensor
By optimizing the spontaneous polarization direction of the ferroelectric layer and the configuration of the two-dimensional material layer in the electromagnetic wave detector, the problem of insufficient OFF operation sensitivity in the prior art is solved, and higher detection sensitivity and improved electromagnetic wave detection effect are achieved. .
Patent Information
- Application Number
- CN202380028949.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-01-12
- Publication Date
- 2024-11-05
AI Technical Summary
The existing electromagnetic wave detectors have insufficient sensitivity in the OFF operation, making it difficult to effectively detect the loss of electromagnetic waves.
An electromagnetic wave detector including a first ferroelectric layer, a two-dimensional material layer and an electrode pair is designed. By optimizing the spontaneous polarization direction of the ferroelectric layer and the configuration of the two-dimensional material layer, higher detection sensitivity is achieved. and improve OFF action.
It realizes higher detection sensitivity and improved OFF action, can effectively detect the existence and absence of electromagnetic waves, and improves the performance of electromagnetic wave detectors.
Smart Images

Figure CN118901146A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an electromagnetic wave detector, an electromagnetic wave detector array, and an image sensor. Background Art
[0002] As a material for the electromagnetic wave detection layer used in the next generation of electromagnetic wave detectors, graphene is known as an example of a two-dimensional material layer. Graphene has extremely high mobility. The absorptivity of graphene is as low as 2.3%. Therefore, a method for increasing the sensitivity of an electromagnetic wave detector using graphene as a two-dimensional material layer is proposed.
[0003] For example, International Publication No. 2018 / 012076 (Patent Document 1) discloses an electromagnetic wave detector having a source electrode, a drain electrode, a graphene layer, and a ferroelectric layer. In the electromagnetic wave detector of Patent Document 1, a ferroelectric layer is arranged at the lower or upper part of the graphene layer connected between the source electrode and the drain electrode. In the above-mentioned electromagnetic wave detector, a pyroelectric effect is generated in the ferroelectric layer by incident electromagnetic waves, especially electromagnetic waves in the infrared wavelength range. Through this pyroelectric effect, the gate voltage of the graphene layer is modulated. Since the graphene layer is the thickness of an atomic layer and the charge mobility is large, a huge current response change can be obtained by a small change in the gate voltage. Such an effect is called an optical gate effect. Through this optical gate effect, high sensitivity can be achieved.
[0004] Patent Document 1: International Publication No. 2018 / 012076 Summary of the invention
[0005] Problem that the invention aims to solve
[0006] However, it is difficult to perform OFF operation of the electromagnetic wave detector in Patent Document 1. The present disclosure has been made in view of the above problems, and an object thereof is to provide an electromagnetic wave detector, an electromagnetic wave detector array, and an image sensor having higher detection sensitivity and improved OFF operation.
[0007] Solutions for solving problems
[0008] The electromagnetic wave detector involved in the present disclosure comprises a first ferroelectric layer, a two-dimensional material layer, a first electrode pair and a second electrode pair. The first ferroelectric layer includes a first main surface and has spontaneous polarization. The two-dimensional material layer is arranged on the first main surface of the first ferroelectric layer. The first electrode pair includes a first electrode and a second electrode. The second electrode pair includes a third electrode and a fourth electrode. The first electrode pair is electrically connected to the two-dimensional material layer. The second electrode pair is electrically connected to the two-dimensional material layer. In a plan view of the first main surface, the third electrode and the fourth electrode are arranged facing each other in a first direction perpendicular to a first polarization direction of the spontaneous polarization of the first ferroelectric layer. In a plan view of the first main surface, the first electrode and the second electrode are arranged facing each other in a second direction different from the first direction.
[0009] The electromagnetic wave detector array according to the present disclosure includes a plurality of electromagnetic wave detectors according to the present disclosure, and the plurality of electromagnetic wave detectors are arranged in a row along at least one of a third direction and a fourth direction different from the third direction.
[0010] The image sensor according to the present disclosure includes the electromagnetic wave detector array of the present disclosure and a readout circuit connected to the electromagnetic wave detector array of the present disclosure.
[0011] Effects of the Invention
[0012] According to the electromagnetic wave detector of the present disclosure, it is possible to provide an electromagnetic wave detector, an electromagnetic wave detector array, and an image sensor having higher detection sensitivity and improved OFF operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a schematic plan view of the electromagnetic wave detector according to the first embodiment.
[0014] Figure 2 The electromagnetic wave detector according to the first embodiment, Figure 1 A schematic cross-sectional view along the section line II-II is shown.
[0015] Figure 3 The electromagnetic wave detector according to the first embodiment, Figure 1 A schematic cross-sectional view along the section line III-III is shown.
[0016] Figure 4 This is a schematic cross-sectional view showing an electromagnetic wave detector according to a first modified example of the first embodiment.
[0017] Figure 5 This is a schematic cross-sectional view showing an electromagnetic wave detector according to a second modified example of the first embodiment.
[0018] Fig. 6AThis is a schematic cross-sectional view showing an electromagnetic wave detector according to a third modified example of the first embodiment.
[0019] Figure 6B This is a schematic plan view showing an electromagnetic wave detector according to a fourth modified example of the first embodiment.
[0020] Figure 7 This is a schematic plan view of the electromagnetic wave detector involved in Embodiment 2.
[0021] Figure 8 This is a schematic cross-sectional view of the electromagnetic wave detector according to the third embodiment.
[0022] Fig. 9 This is a schematic cross-sectional view of the electromagnetic wave detector according to the third embodiment.
[0023] Fig.10 This is a schematic cross-sectional view of the electromagnetic wave detector according to the fourth embodiment.
[0024] Fig.11 This is a schematic cross-sectional view of an electromagnetic wave detector according to a modified example of the fourth embodiment.
[0025] Fig.12 This is a schematic cross-sectional view of the electromagnetic wave detector according to the fifth embodiment.
[0026] Fig.13 This is a schematic cross-sectional view of an electromagnetic wave detector according to a modified example of the fifth embodiment.
[0027] Fig.14 This is a schematic cross-sectional view of the electromagnetic wave detector according to the sixth embodiment.
[0028] Fig.15 This is a schematic cross-sectional view of the electromagnetic wave detector involved in the seventh embodiment.
[0029] Fig.16 This is a schematic plan view of the electromagnetic wave detector involved in embodiment 8.
[0030] Fig.17 The electromagnetic wave detector according to Embodiment 8, Fig.16 A schematic cross-sectional view along section line XVII-XVII is shown.
[0031] Fig.18 The electromagnetic wave detector according to Embodiment 8, Fig.16 A schematic cross-sectional view along the section line XVIII-XVIII is shown.
[0032] Fig.19 This is a schematic plan view of the electromagnetic wave detector involved in embodiment 9.
[0033] Fig. 20 The electromagnetic wave detector according to Embodiment 9 Fig.19 A schematic cross-sectional view taken along the section line XX-XX is shown.
[0034] Fig.21A The electromagnetic wave detector according to Embodiment 9 Fig.19 A schematic cross-sectional view taken along section line XXI-XXI is shown.
[0035] Fig. 21B This is a schematic plan view of the electromagnetic wave detector involved in the tenth embodiment.
[0036] Fig. 21C The electromagnetic wave detector according to the tenth embodiment, Fig. 21B A schematic cross-sectional view along the section line XXIC-XXIC is shown.
[0037] Fig. 22 This is a schematic plan view of the electromagnetic wave detector involved in embodiment 11.
[0038] Fig.23 The electromagnetic wave detector according to the eleventh embodiment, Fig. 22 A schematic cross-sectional view along the section line XXIII-XXIII is shown.
[0039] Fig.24 This is a schematic plan view of the electromagnetic wave detector involved in embodiment 12.
[0040] Fig.25 The electromagnetic wave detector according to embodiment 12 Fig.24 A schematic cross-sectional view along the section line XXV-XXV is shown.
[0041] Fig.26 This is a schematic plan view of the electromagnetic wave detector involved in embodiment 13.
[0042] Fig. 27 The electromagnetic wave detector according to embodiment 13, Fig.26 A schematic cross-sectional view along section line XXVII-XXVII is shown.
[0043] Fig.28 This is a schematic plan view of the electromagnetic wave detector involved in embodiment 14.
[0044] Fig.29 The electromagnetic wave detector according to the fourteenth embodiment, Fig.28 A schematic cross-sectional view taken along section line XXIX-XXIX is shown.
[0045] Fig.30This is a circuit diagram of the electromagnetic wave detector involved in embodiment 15.
[0046] Fig.31 This is a circuit diagram showing an electromagnetic wave detector according to embodiment 16.
[0047] Fig.32 This is a plan view schematically showing an electromagnetic wave detector array according to the seventeenth embodiment.
[0048] Fig.33 It is a plan schematic diagram showing an electromagnetic wave detector array involved in a modified example of embodiment 17.
[0049] Fig.34 This is a schematic partial enlarged view of the image sensor involved in embodiment 17.
[0050] Fig.35 This is a schematic partial enlarged view of the image sensor involved in embodiment 17.
[0051] (Explanation of Reference Numerals)
[0052] 1: two-dimensional material layer; 2a: first electrode pair; 2b: second electrode pair; 3: first insulating film; 3b: second insulating film; 3c, 3d: gate insulating film; 4: back electrode; 5: first ferroelectric layer; 5a: first main surface; 5b: second main surface; 5c: second ferroelectric layer; 6: substrate; 6a, 6b main surfaces; 7: semiconductor layer; 7a: first semiconductor layer; 7b: second semiconductor layer; 8: gap; 8b: hole; 8c: recess; 9a: first contact layer; 9b: second contact layer; 11: first elongated portion; 12: second elongated portion; 13: common portion; 21: first electrode; 22: second electrode; 25: third electrode; 26: fourth electrode; 28, 29: gate electrode; 30: first action circuit; 31: first voltage source; 33: second action circuit; 34: second voltage source; 35: action circuit; 36: balance circuit; 40: signal detection circuit; 41 : first signal detector; 42: second signal detector; 44: differentiator; 45: differential amplifier circuit; 46: operational amplifier; 47: power supply; 48: capacitor; 51: first ferroelectric layer portion; 52: second ferroelectric layer portion; 55: step; 60: electromagnetic wave shielding member; 100, 101, 102, 103a, 103b, 104, 105, 106, 107, 108, 108b, 109, 110 , 111, 112a, 112b, 113, 114, 115, 116, 117, 118, 121, 122, 123, 124: electromagnetic wave detector; 120: electromagnetic wave detector array; 126: third direction; 127: fourth direction; 130: image sensor; 131: readout circuit; 133: insulating layer; 134, 136: lead-out electrodes; 135, 137: pads; 138, 139: bumps. DETAILED DESCRIPTION
[0053] Hereinafter, the embodiment will be described based on the drawings. In addition, the same reference numerals are attached to the same or corresponding parts, and the description thereof will not be repeated.
[0054] In the embodiments described below, the figures are schematic and are used to conceptually illustrate functions or structures. In addition, the present disclosure is not limited to the embodiments described below. Except for the cases specifically described, the basic structure of the electromagnetic wave detector is common to all embodiments. In addition, the structures with the same symbols are the same as described above or equivalent thereto. This is common throughout the entire text of the specification.
[0055] In the embodiments described below, the structure of the electromagnetic wave detector in the case of detecting visible light or infrared light is described, but the light detected by the electromagnetic wave detector of the present disclosure is not limited to visible light and infrared light. The embodiments described below are also effective as detectors for detecting radio waves such as X-rays, ultraviolet light, near-infrared light, terahertz (THz) waves, microwaves, etc. in addition to visible light and infrared light. In addition, in the embodiments of the present disclosure, these lights and radio waves are collectively referred to as electromagnetic waves.
[0056] In addition, in this embodiment, the terms p-type graphene and n-type graphene are sometimes used as graphene. In the following embodiments, graphene with more holes than graphene in an eigenstate is called p-type graphene, and graphene with more electrons than graphene in an eigenstate is called n-type graphene. That is, n-type materials are materials with electron donating properties. In addition, p-type materials are materials with electron withdrawing properties.
[0057] In addition, sometimes when there is a bias in charge in the molecule as a whole, the material in which electrons dominate is called n-type. Sometimes when there is a bias in charge in the molecule as a whole, the material in which holes dominate is called p-type. The material of the member in contact with graphene as an example of a two-dimensional material layer can also use one of organic and inorganic substances or a mixture of organic and inorganic substances.
[0058] In addition, regarding the surface plasmon resonance phenomenon as the interaction between the metal surface and light, the phenomenon called pseudo surface plasmon resonance in the sense of resonance on the metal surface outside the visible light region and the near-infrared light region, or the phenomenon called metamaterial or plasmon metamaterial in the sense of operating the wavelength by a structure with a size below the wavelength, they are not particularly distinguished by name, and are treated equally from the perspective of the effects brought about by the phenomenon. Here, these resonances are referred to as surface plasmon resonance, plasmon resonance, or simply resonance.
[0059] In addition, in the embodiments described below, graphene is mainly used as an example of the material of the two-dimensional material layer, but the material of the two-dimensional material layer is not limited to graphene. For example, as the material of the two-dimensional material layer, multilayer graphene, turbostratic multilayer graphene, transition metal dichalcogenide (TMD), black phosphorus, silicene (a two-dimensional honeycomb structure formed by silicon atoms), germanene (a two-dimensional honeycomb structure formed by germanium atoms) and other materials can be used. As a transition metal dichalcogenide, for example, molybdenum disulfide (MoS 2 ), tungsten disulfide (WS2 ), tungsten diselenide (WSe 2 ) and other transition metal dichalcogenides.
[0060] More preferably, the two-dimensional material layer includes any material selected from the group consisting of graphene, multilayer graphene, turbostratic graphene, transition metal dichalcogenide (TMD), black phosphorus, silicene (a two-dimensional honeycomb structure formed by silicon atoms), graphene nanoribbons and borophene.
[0061] These materials have a structure similar to graphene. In these materials, atoms are arranged in a single layer in a two-dimensional plane. Therefore, when these materials are applied to a two-dimensional material layer, the same effect as when graphene is applied to a two-dimensional material layer can be obtained.
[0062] In addition, in this embodiment, a layer referred to as an insulating layer is a layer having an insulating material with a thickness that does not generate a tunnel current.
[0063] Implementation method 1.
[0064] <Structure of Electromagnetic Wave Detector 100>
[0065] Reference Figures 1 to 3 The electromagnetic wave detector 100 according to Embodiment 1 is described. The electromagnetic wave detector 100 includes a first ferroelectric layer 5 , a two-dimensional material layer 1 , a first electrode pair 2 a , a second electrode pair 2 b , a first insulating film 3 , a back electrode 4 , a first operating circuit 30 , a second operating circuit 33 , and a signal detection circuit 40 .
[0066] The first ferroelectric layer 5 includes a first principal surface 5a and a second principal surface 5b on the opposite side of the first principal surface 5a. The first principal surface 5a and the second principal surface 5b extend in the x direction and the y direction perpendicular to the x direction, respectively. The normal direction of the first principal surface 5a and the normal direction of the second principal surface 5b are the z direction perpendicular to the x direction and the y direction. The first ferroelectric layer 5 has spontaneous polarization. The first polarization direction of the spontaneous polarization of the first ferroelectric layer 5 is, for example, the +x direction.
[0067] The first ferroelectric layer 5 is sensitive to the wavelength of the electromagnetic wave irradiated to the electromagnetic wave detector 100 (hereinafter sometimes referred to as the "detection wavelength"). When the first ferroelectric layer 5 is irradiated with the electromagnetic wave having the detection wavelength, the first ferroelectric layer 5 absorbs the electromagnetic wave to generate heat. Therefore, the spontaneous polarization of the first ferroelectric layer 5 changes. That is, a pyroelectric effect is generated in the first ferroelectric layer 5. In this embodiment, the electromagnetic wave is emitted from the first ferroelectric layer 5. Figure 2 and Figure 3The electromagnetic wave detector 100 is irradiated from above. In order to detect electromagnetic waves using the electromagnetic wave detector 100, as long as the first ferroelectric layer 5 is irradiated with electromagnetic waves, the irradiation direction of the electromagnetic wave to the electromagnetic wave detector 100 is not particularly limited.
[0068] In this embodiment, the first ferroelectric layer 5 is arranged below the two-dimensional material layer 1. Specifically, the first ferroelectric layer 5 is arranged below the first electrode pair 2a, the second electrode pair 2b and the two-dimensional material layer 1. The first ferroelectric layer 5 can also be arranged on the two-dimensional material layer 1, and can also be arranged on the first electrode pair 2a and the second electrode pair 2b. The first principal surface 5a of the first ferroelectric layer 5 is covered by the first insulating film 3.
[0069] The two-dimensional material layer 1 is disposed on the first main surface 5a of the first ferroelectric layer 5. Figure 2 and Figure 3 As shown, in the present embodiment, the two-dimensional material layer 1 is arranged on the first electrode pair 2a and the second electrode pair 2b. The two-dimensional material layer 1 may also be arranged below the first electrode pair 2a and the second electrode pair 2b. In the plan view of the first principal surface 5a of the first ferroelectric layer 5, the two-dimensional material layer 1 is preferably arranged in a manner overlapping with the first ferroelectric layer 5. Therefore, the influence of the change in the spontaneous polarization of the first ferroelectric layer 5 of the two-dimensional material layer 1 can be increased.
[0070] The two-dimensional material layer 1 includes a first elongated portion 11 and a second elongated portion 12. The first long side direction of the first elongated portion 11 is different from the second long side direction of the second elongated portion 12. The first long side direction of the first elongated portion 11 is, for example, a direction (x direction) parallel to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. The second long side direction of the second elongated portion 12 is, for example, a first direction (y direction) perpendicular to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5.
[0071] like Figure 2 and Figure 3 As shown, in this embodiment, the first elongated portion 11 is the same layer as the second elongated portion 12. The first elongated portion 11 and the second elongated portion 12 share a common portion 13. The common portion 13 is the central portion of the first elongated portion 11 and the central portion of the second elongated portion 12. Figure 1As shown, in the plan view of the first principal surface 5a, a portion of the first elongated portion 11 overlaps with a portion of the second elongated portion 12. In the present embodiment, in the plan view of the first principal surface 5a, the central portion of the first elongated portion 11 overlaps with the central portion of the second elongated portion 12. In the plan view of the first principal surface 5a, the first elongated portion 11 intersects with the second elongated portion 12, and the shape of the two-dimensional material layer 1 is a cross. The shape of the two-dimensional material layer 1 in the plan view of the first principal surface 5a is not particularly limited, as long as it is a shape that produces a difference between the first electrical signal generated from the first electrode pair 2a and the second electrical signal generated from the second electrode pair 2b when the electromagnetic wave detector 100 is irradiated with electromagnetic waves (hereinafter sometimes referred to as the "bright state").
[0072] In this embodiment, the shape of the end of the two-dimensional material layer 1 is a rectangle in a plan view of the first main surface 5a. The shape of the end of the two-dimensional material layer 1 is not particularly limited, and may be a triangle or a comb shape.
[0073] In the plan view of the first main surface 5a, the shape of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is preferably the same as the shape of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26. In the case where the shape of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is the same as the shape of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26, the resistance of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is the same as the resistance of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26. Therefore, when the electromagnetic wave detector 100 is not irradiated with electromagnetic waves (hereinafter, sometimes referred to as a "dark state"), the output from the signal detection circuit 40 can be made zero. Even in the case where the shape of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is different from the shape of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26, the output from the signal detection circuit 40 can be made zero in the dark state by adjusting the signal detection circuit 40.
[0074] The two-dimensional material layer 1 is formed of any material selected from the group consisting of graphene, multilayer graphene, turbostratic graphene, transition metal dichalcogenides, black phosphorus, silicene, graphene nanoribbons, and borophene. The two-dimensional material layer 1 may also be formed of a single two-dimensional material layer.
[0075] The first electrode pair 2a is electrically connected to the two-dimensional material layer 1. Specifically, the first electrode pair 2a is electrically connected to the first elongated portion 11. The first electrode pair 2a includes a first electrode 21 and a second electrode 22. In a plan view of the first principal surface 5a, the first electrode 21 and the second electrode 22 are arranged facing each other in a second direction different from a first direction (y direction) perpendicular to a first polarization direction (+x direction) of spontaneous polarization relative to the first ferroelectric layer 5. Therefore, when an electromagnetic wave is irradiated to the electromagnetic wave detector 100, the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 changes due to a change in the spontaneous polarization of the first ferroelectric layer 5.
[0076] The second direction is preferably parallel to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5, and the first electrode 21 and the second electrode 22 are preferably arranged facing each other in the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5 in a plan view of the first main surface 5a. Therefore, the change in the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 is maximized.
[0077] The second electrode pair 2b is electrically connected to the two-dimensional material layer 1. Specifically, the second electrode pair 2b is electrically connected to the second elongated portion 12. The second electrode pair 2b includes a third electrode 25 and a fourth electrode 26. In a plan view of the first main surface 5a, the third electrode 25 and the fourth electrode 26 are arranged facing each other in a first direction (y direction) perpendicular to the first polarization direction of the spontaneous polarization of the first ferroelectric layer 5. Therefore, the second electrical signal output from the second electrode pair 2b is not affected by the change in the spontaneous polarization of the first ferroelectric layer 5 generated in the bright state. The resistance of the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26 in the bright state does not change relative to the resistance of the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26 in the dark state. Between the dark state and the bright state, the second electrical signal output from the second electrode pair 2b does not change.
[0078] In contrast, as described above, the first electrode 21 and the second electrode 22 are arranged facing each other in a second direction different from the first direction (y direction) perpendicular to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. Therefore, the first electrical signal output from the first electrode pair 2a is affected by the change in the spontaneous polarization of the first ferroelectric layer 5 generated in the bright state. The resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 in the bright state changes relative to the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 in the dark state. The first electrical signal output from the first electrode pair 2a changes between the dark state and the bright state.
[0079] The resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 in the dark state is made equal to the resistance of the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26 in the dark state. The signal detection circuit 40 outputs a differential signal between the first electrical signal output from the first electrode pair 2a and the second electrical signal output from the second electrode pair 2b. In this way, the signal output from the signal detection circuit 40 in the dark state is zero.
[0080] In contrast, in the bright state, the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 changes, but the resistance of the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26 in the dark state does not change. The signal detection circuit 40 outputs a differential signal between the first electrical signal output from the first electrode pair 2a and the second electrical signal output from the second electrode pair 2b. Therefore, the influence of the dark current can be eliminated from the signal output by the signal detection circuit 40 in the bright state. The OFF action of the electromagnetic wave detector 100 is improved.
[0081] The first insulating film 3 is formed on the first main surface 5a of the first ferroelectric layer 5. The first insulating film 3 is arranged between the first ferroelectric layer 5 and the two-dimensional material layer 1. The first insulating film 3 absorbs the electromagnetic wave incident on the electromagnetic wave detector 100 and generates heat. Therefore, the first insulating film 3 can enhance the change of the spontaneous polarization of the first ferroelectric layer 5 in the bright state.
[0082] The back electrode 4 is formed on the second main surface 5b of the first ferroelectric layer 5. By applying a back gate voltage V to the two-dimensional material layer 1 via the back electrode 4, bg , which can efficiently apply a back gate voltage V to the two-dimensional material layer 1 bg In the case where the electromagnetic wave detector 100 includes the back electrode 4, it is preferable to Figure 2 and Figure 3 The electromagnetic wave detector 100 is irradiated with electromagnetic waves in the upper direction.
[0083] The first operating circuit 30 is connected to the first electrode pair 2a. The first operating circuit 30 includes, for example, a circuit that applies a bias voltage V between the first electrode 21 and the second electrode 22. d1 The first voltage source 31 applies a bias voltage V to the first elongated portion 11 of the two-dimensional material layer 1. d1 .
[0084] The second operating circuit 33 is connected to the second electrode pair 2b. The second operating circuit 33 includes, for example, a circuit that applies a bias voltage V between the third electrode 25 and the fourth electrode 26. d2 The second voltage source 34 applies a bias voltage V to the second elongated portion 12 of the two-dimensional material layer 1. d2 .
[0085] The signal detection circuit 40 includes a first signal detector 41 , a second signal detector 42 , and a differentiator 44 .
[0086] The first signal detector 41 is connected to the first electrode pair 2a. Specifically, the first signal detector 41 is connected to one of the first electrode 21 and the second electrode 22 included in the first electrode pair 2a (the first electrode 21 in the present embodiment). The other of the first electrode 21 and the second electrode 22 (the second electrode 22 in the present embodiment) is, for example, grounded. The first signal detector 41 is connected to the first action circuit 30. The first signal detector 41 detects a first electrical signal output from the first electrode pair 2a. The first signal detector 41 includes, for example, a first ammeter. The first ammeter detects a bias voltage V applied between the first electrode 21 and the second electrode 22 by the first action circuit 30. d1 The current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 d1 .
[0087] The second signal detector 42 is connected to the second electrode pair 2b. Specifically, the second signal detector 42 is connected to one of the third electrode 25 and the fourth electrode 26 included in the second electrode pair 2b (the third electrode 25 in the present embodiment). The other of the third electrode 25 and the fourth electrode 26 (the fourth electrode 26 in the present embodiment) is, for example, grounded. The second signal detector 42 is connected to the second action circuit 33. The second signal detector 42 detects a second electrical signal output from the second electrode pair 2b. The second signal detector 42 includes, for example, a second ammeter. The second ammeter detects the second electrical signal by applying a bias voltage V between the third electrode 25 and the fourth electrode 26 by the second action circuit 33. d2 The current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 d2 .
[0088] The differentiator 44 is connected to the first signal detector 41 and the second signal detector 42. The differentiator 44 outputs a differential signal between the first electrical signal and the second electrical signal. For example, the first electrical signal is a current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22. d1 The second electrical signal is the current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26. d2 , the output current I of the differentiator 44 d1 With current I d2 Therefore, in the dark state, the signal output from the signal detection circuit 40 can be made zero. The influence of the dark current can be eliminated from the signal output from the signal detection circuit 40 in the bright state. The OFF operation of the electromagnetic wave detector 100 is improved.
[0089] Next, the structures of the two-dimensional material layer 1 , the first electrode pair 2 a , the second electrode pair 2 b , the first insulating film 3 , and the first ferroelectric layer 5 are described in detail.
[0090] <Structure of Two-Dimensional Material Layer 1>
[0091] The two-dimensional material layer 1 is, for example, a single layer of graphene. A single layer of graphene is a single atomic layer of a two-dimensional carbon crystal. Graphene has a plurality of carbon atoms respectively arranged on each of a plurality of chains arranged in a hexagonal shape. The absorptivity of graphene is as low as 2.3%. Specifically, the absorptivity of white light of graphene is 2.3%. In addition, in the present embodiment, white light is light in which light having wavelengths of visible light is equally mixed. In addition, the two-dimensional material layer 1 may also be a multilayer graphene formed by stacking a plurality of graphene layers. The orientation of the lattice vectors of the hexagonal lattice of each graphene in the multilayer graphene may be consistent or different. In addition, the orientation of the lattice vectors of the hexagonal lattice of each graphene in the multilayer graphene may also be completely consistent. In addition, the two-dimensional material layer 1 may also be graphene doped with p-type or n-type impurities.
[0092] For example, by stacking more than two layers of graphene layers, a band gap is formed in the two-dimensional material layer 1. That is, by changing the number of stacked graphene layers, the size of the band gap can be adjusted. As a result, the two-dimensional material layer 1 can have a wavelength selection effect of selecting electromagnetic waves (detection wavelengths) as the object of photoelectric conversion. In addition, for example, if the number of graphene layers of the multilayer graphene increases, the mobility of the two-dimensional material layer 1 decreases. On the other hand, if the number of graphene layers of the multilayer graphene increases, the influence of carrier scattering from the substrate supporting the two-dimensional material layer is suppressed, so that the noise of the electromagnetic wave detector 100 decreases. Therefore, if multilayer graphene is used as the two-dimensional material layer 1, the absorption of electromagnetic waves in the two-dimensional material layer 1 increases, and the detection sensitivity of the electromagnetic wave detector 100 for electromagnetic waves is improved.
[0093] In addition, the multilayer graphene may also include a turbostratic structure portion. The method for making the turbostratic structure portion may also be appropriately determined. For example, a single layer of graphene made by a CVD method may be transferred multiple times to stack multilayer graphene, thereby forming a turbostratic structure portion. In addition, ethanol or methane may be configured on the graphene as a carbon source, and the graphene may be grown by a CVD method to form a turbostratic structure portion.
[0094] More specifically, in a normal stacked graphene that does not include a turbostratic structure portion, a plurality of graphene layers are stacked in a state where the crystal lattices of the graphene layers match each other. Such a stacked state of a plurality of graphene layers is called AB stacking.
[0095] In contrast, a multilayer graphene including a turbostratic structure portion is formed in the following manner. The graphene produced by the CVD method has polycrystalline. Therefore, when graphene is further transferred multiple times on the graphene of the lower layer, or when graphene is further stacked with the graphene of the lower layer as the core by the CVD method, the lattices of multiple graphenes are stacked in a mutually mismatched state. That is, a turbostratic structure portion is formed in the multilayer graphene. In the turbostratic structure portion, there is little interaction between adjacent graphene layers, and each graphene layer of the turbostratic structure portion has the same properties as a single-layer graphene. Moreover, if the two-dimensional material layer 1 is affected by carrier scattering from the substrate, the mobility of the two-dimensional material layer 1 decreases. However, in the turbostratic structure portion, although the graphene in contact with the substrate is affected by carrier scattering, the upper layer of graphene stacked on the graphene with a turbostratic structure is not easily affected by carrier scattering from the substrate. In addition, in turbostratic graphene, there is little interaction between adjacent graphene layers, and thus the conductivity is improved. Based on the above, in turbostratic graphene, the mobility of carriers is improved, and the electromagnetic wave detector 100 including turbostratic graphene has improved sensitivity to electromagnetic waves.
[0096] In addition, as the two-dimensional material layer 1, nanoribbon-shaped graphene (graphene nanoribbon) can also be used. The two-dimensional material layer 1 can also be a graphene nanoribbon monomer. The two-dimensional material layer 1 can also have a structure in which a plurality of graphene nanoribbons are stacked. The two-dimensional material layer 1 can also have a structure in which graphene nanoribbons are periodically arranged on a plane. In the case where the two-dimensional material layer 1 has a structure in which graphene nanoribbons are periodically arranged, plasma resonance is generated in the graphene nanoribbons, and thus the sensitivity of the electromagnetic wave detector 100 is improved. The structure in which graphene nanoribbons are periodically arranged is sometimes referred to as a graphene metamaterial. In the electromagnetic wave detector 100 using the graphene metamaterial as the two-dimensional material layer 1, plasma resonance is generated, and thus the sensitivity of the electromagnetic wave detector 100 is improved.
[0097] The end of the two-dimensional material layer 1 may be a graphene nanoribbon. In this case, since the graphene nanoribbon has a band gap, a Schottky junction is formed in the junction region between the graphene nanoribbon and the electrode.
[0098] The two-dimensional material layer 1 is in contact with the first electrode pair 2a, and carriers are doped from the first electrode pair 2a to the two-dimensional material layer 1. For example, in the case where the two-dimensional material layer 1 is formed of graphene and the first electrode pair 2a is formed of gold (Au), the carriers are holes. According to the difference between the work function of graphene and the work function of gold (Au), holes are doped in the portion of the two-dimensional material layer 1 that is in contact with the first electrode pair 2a. If the electromagnetic wave detector 100 is driven in an electron conduction state in a state where the portion of the two-dimensional material layer 1 is doped with holes, the mobility of electrons flowing in the channel due to the influence of holes decreases. Therefore, the contact resistance between the two-dimensional material layer 1 and the first electrode pair 2a increases. In particular, in the case where the entire region of the two-dimensional material layer 1 is formed of a single layer of graphene, the amount of carriers (doping amount) injected into the two-dimensional material layer 1 from the first electrode pair 2a is large. Therefore, the mobility of electrons in the electromagnetic wave detector 100 decreases significantly. Therefore, in the case where the entire region of the two-dimensional material layer 1 is formed of a single-layer graphene, the performance of the electromagnetic wave detector 100 is degraded.
[0099] In addition, the amount of carriers doped from the first electrode pair 2a to the multilayer graphene is less than the amount of carriers doped from the first electrode pair 2a to the single-layer graphene. Therefore, by forming a junction with the first electrode pair 2a that is easily doped with carriers by the multilayer graphene, the increase in the contact resistance between the two-dimensional material layer 1 and the first electrode pair 2a can be suppressed. Thus, the decrease in the mobility of the electrons of the electromagnetic wave detector 100 can be suppressed, and the performance of the electromagnetic wave detector 100 can be improved.
[0100] <Structure of the First Electrode Pair 2a and the Second Electrode Pair 2b>
[0101] The first electrode pair 2a and the second electrode pair 2b are formed of any conductive material. The materials of the first electrode pair 2a and the second electrode pair 2b may include at least one of gold (Au), silver (Ag), copper (Cu), aluminum (Al), nickel (Ni), chromium (Cr) and palladium (Pd). A sealing layer (not shown) may also be provided between the first electrode pair 2a and the first insulating film 3 and between the second electrode pair 2b and the first insulating film 3. The sealing layer improves the sealing between the first electrode pair 2a and the first insulating film 3 and the sealing between the second electrode pair 2b and the first insulating film 3. The material of the sealing layer includes, for example, metal materials such as chromium (Cr) or titanium (Ti).
[0102] <Structure of First Insulating Film 3>
[0103] The material of the first insulating film 3 is, for example, silicon oxide (SiO 2 The material of the first insulating film 3 is not limited to silicon oxide, for example, it can also be tetraethyl orthosilicate (Si(OC 2 H 5 )4 ), silicon nitride (Si 3 N 4 ), hafnium oxide (HfO 2 ), aluminum oxide (Al 2 O 3 ), nickel oxide (NiO), boron nitride (BN) or a polymer material of the siloxane series. For example, the atomic arrangement of boron nitride (BN) is similar to that of graphene. Therefore, when boron nitride (BN) is in contact with the two-dimensional material layer 1 composed of graphene, the decrease in the mobility of the electrons of the two-dimensional material layer 1 is suppressed. Therefore, boron nitride (BN) is a material suitable for the first insulating film 3 as a base film arranged under the two-dimensional material layer 1.
[0104] The material of the first insulating film 3 may also be ReNiO 3 (Re represents a rare earth element) or TaS 2 When electromagnetic waves are irradiated to the Mott insulator layer, a phase change occurs in the Mott insulator layer, and the physical properties (e.g., temperature) of the Mott insulator layer change. Therefore, the Mott insulator layer can enhance the change in the spontaneous polarization of the first ferroelectric layer 5 when the electromagnetic waves are irradiated.
[0105] The thickness of the first insulating film 3 is not particularly limited as long as the first electrode pair 2a and the second electrode pair 2b are electrically insulated from the first ferroelectric layer 5 and no tunnel current is generated between the first electrode pair 2a and the first ferroelectric layer 5 and between the second electrode pair 2b and the first ferroelectric layer 5. The insulating layer may not be disposed below the two-dimensional material layer 1.
[0106] <Structure of the First Ferroelectric Layer 5>
[0107] The material of the first ferroelectric layer 5 may be any material as long as it causes a change in spontaneous polarization in the first ferroelectric layer 5 when an electromagnetic wave having a detection wavelength is incident on the first ferroelectric layer 5. The material of the first ferroelectric layer 5 includes, for example, barium titanate (BaTiO 3 ), lithium niobate (LiNbO 3 ), lithium tantalate (LiTaO 3 ), SrTiO 3 ), lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), zinc oxide (ZnO), hafnium oxide (HfO 2 ) and at least any one of polyvinylidene fluoride-based ferroelectrics (PVDF, P(VDF-TrFE), P(VDF-TrFE-CTFE), etc.) as an organic polymer. In addition, the first ferroelectric layer 5 can also be formed by stacking or mixing multiple different ferroelectric materials.
[0108] The material of the first ferroelectric layer 5 is not limited to the above-mentioned materials as long as it is a pyroelectric that exerts a thermoelectric effect. Specifically, the material of the first ferroelectric layer 5 can be any ferroelectric that produces a change in spontaneous polarization in response to a change in thermal energy inside the first ferroelectric layer 5. In addition, in the thermoelectric effect, electromagnetic waves only act as a heat source. Therefore, there is basically no wavelength dependence in the thermoelectric effect, and there is basically no wavelength dependence in the first ferroelectric layer 5. Therefore, the first ferroelectric layer 5 is sensitive to electromagnetic waves over a wide bandwidth.
[0109] The material of the first ferroelectric layer 5 has spontaneous polarization. When the temperature of the first ferroelectric layer 5 rises due to irradiation with electromagnetic waves, the spontaneous polarization of the first ferroelectric layer 5 decreases. Therefore, the electric field applied from the first ferroelectric layer 5 to the two-dimensional material layer 1 decreases. A resistance change occurs in the two-dimensional material layer 1 due to the change in the spontaneous polarization of the first ferroelectric layer 5. Therefore, the electromagnetic wave detector 100 including the two-dimensional material layer 1 and the first ferroelectric layer 5 is able to detect electromagnetic waves.
[0110] By constructing the first ferroelectric layer 5 in such a way that the speed of change of the spontaneous polarization in the first ferroelectric layer 5 is as fast as possible, the response speed of the electromagnetic wave detector 100 can be improved. Specifically, regarding the thickness of the first ferroelectric layer 5, it is desirable to be as thin as possible within a range that can impart an effect of the change of the spontaneous polarization of the first ferroelectric layer 5 caused by the irradiation of electromagnetic waves to the two-dimensional material layer 1. Specifically, it is desirable that the first ferroelectric layer 5 is a ferroelectric thin film having a thickness of 10 μm or less.
[0111] The thickness of the first ferroelectric layer 5 is preferably such that the two-dimensional material layer 1 can be subjected to the largest possible change in resistance due to a change in spontaneous polarization of the first ferroelectric layer 5 when the first ferroelectric layer 5 is irradiated with electromagnetic waves.
[0112] A protective film (not shown) may also be provided on the first ferroelectric layer 5. The protective film may also be provided in a manner covering the two-dimensional material layer 1, the first electrode pair 2a, and the second electrode pair 2b. The material of the protective film may be, for example, an insulator such as an oxide or a nitride. The material of the protective film may be, for example, silicon oxide (SiO 2 ), silicon nitride (SiN), hafnium oxide (HfO 2 ), aluminum oxide (Al 2 O 3 ) or boron nitride (BN), etc.
[0113] <Method of Manufacturing Electromagnetic Wave Detector 100>
[0114] An example of a method for manufacturing the electromagnetic wave detector 100 according to the present embodiment will be described.
[0115] An example of a method for manufacturing the electromagnetic wave detector 100 of the present embodiment mainly includes a preparation step, a back electrode forming step, an insulating film forming step, an electrode forming step, and a two-dimensional material layer forming step.
[0116] First, a preparation step is performed. In the preparation step, a ferroelectric substrate is prepared as the first ferroelectric layer 5. The material of the ferroelectric substrate is a material having sensitivity to a predetermined detection wavelength.
[0117] Next, a back electrode forming process is implemented. In the back electrode forming process, a protective film is formed on the surface of the first ferroelectric layer 5 (except the second main surface 5b). The protective film is, for example, an anti-etching agent. In a state where the surface of the first ferroelectric layer 5 is protected by the protective film, a back electrode 4 is formed on the second main surface 5b of the first ferroelectric layer 5. It is also possible to form a bonding layer (not shown) on the second main surface 5b of the first ferroelectric layer 5 before forming the back electrode 4. In addition, with regard to the back electrode forming process, as long as the surface of the first ferroelectric layer 5 is protected by the protective film, the back electrode forming process can also be implemented after any process from the insulating film forming process to the two-dimensional material layer forming process. After the back electrode 4 is formed, the protective film is removed from the surface of the first ferroelectric layer 5.
[0118] Next, an insulating film forming process is performed. In the insulating film forming process, a first insulating film 3 is formed on the first main surface 5a of the first ferroelectric layer 5. The film forming method of the first insulating film 3 can also be a CVD (Chemical Vapor Deposition) method or a sputtering method. For example, the first insulating film 3 can also be formed by forming tetraethoxysilane on the first main surface 5a of the first ferroelectric layer 5 using a plasma CVD method or the like.
[0119] Next, an electrode forming step is performed. In the electrode forming step, the first electrode pair 2a and the second electrode pair 2b are formed on the first insulating film 3. Before forming the first electrode pair 2a and the second electrode pair 2b, a bonding layer (not shown) may be formed in the first insulating film 3 in the region where the first electrode pair 2a and the second electrode pair 2b are to be formed. The bonding layer improves the bonding between the first electrode pair 2a and the first insulating film 3 and the bonding between the second electrode pair 2b and the first insulating film 3.
[0120] As a method for forming the first electrode pair 2a and the second electrode pair 2b, for example, the following process is used. First, a resist mask is formed on the first insulating film 3. The resist mask is patterned by photolithography or electron beam (EB) drawing method to form an opening in the region of the resist mask where the first electrode pair 2a and the second electrode pair 2b are to be formed. Then, a conductive film such as a metal film to be the first electrode pair 2a and the second electrode pair 2b is formed on the resist mask by evaporation or sputtering. The conductive film is formed in the opening of the resist mask and on the upper surface of the resist mask. Afterwards, the resist mask is removed together with a portion of the conductive film. The conductive film in the opening of the resist mask remains on the first insulating film 3, and becomes the first electrode pair 2a and the second electrode pair 2b on the first insulating film 3. The above-mentioned method for forming the first electrode pair 2a and the second electrode pair 2b is generally referred to as a lift-off method.
[0121] As a method for forming the first electrode pair 2a and the second electrode pair 2b, other methods may also be used. For example, a conductive film such as a metal film to be the first electrode pair 2a and the second electrode pair 2b is formed on the first insulating film 3. Then, a resist mask is formed on the conductive film. The resist mask is patterned by photolithography or electron beam (EB) drawing method to form an opening in the resist mask. The resist mask covers the area where the first electrode pair 2a and the second electrode pair 2b are to be formed, and the opening is formed in the area where the first electrode pair 2a and the second electrode pair 2b are not formed. Next, the resist mask is used as an etching mask to partially remove the conductive film by wet etching or dry etching. The conductive film exposed from the resist mask is removed. The conductive film covered by the resist mask remains on the first insulating film 3 and becomes the first electrode pair 2a and the second electrode pair 2b. Finally, the resist mask is removed. The first electrode pair 2a and the second electrode pair 2b may also be formed in this way.
[0122] Next, a two-dimensional material layer forming process is implemented. In the two-dimensional material layer forming process of the present embodiment, a two-dimensional material film is formed in such a manner that the first electrode pair 2a, the second electrode pair 2b, and the first insulating film 3 are covered by the two-dimensional material layer 1. There is no particular limitation on the method for forming the two-dimensional material film. The two-dimensional material film can be formed, for example, by epitaxial growth or by screen printing. In addition, with respect to the two-dimensional material film, the two-dimensional material film can also be formed by transferring a two-dimensional material film previously formed by a CVD method and pasting it on the first insulating film 3. The two-dimensional material film can also be formed by transferring a film-like two-dimensional material film that has been peeled off by mechanical peeling or the like and pasting it on the first insulating film 3.
[0123] Next, a resist mask is formed on the two-dimensional material film. The resist mask is patterned by photolithography or electron beam (EB) drawing method. The resist mask covers the area in the two-dimensional material film where the first electrode pair 2a and the second electrode pair 2b are to be formed. The area in the two-dimensional material film where the first electrode pair 2a and the second electrode pair 2b are not formed is exposed from the resist mask. The two-dimensional material film is etched using the resist mask as an etching mask. The etching method of the two-dimensional material film is, for example, dry etching using oxygen plasma. Finally, the resist mask is removed. In this way, a two-dimensional material layer 1 is formed.
[0124] Through the above steps, the electromagnetic wave detector 100 of this embodiment is manufactured.
[0125] In addition, in one example of the above-mentioned manufacturing method, the two-dimensional material layer 1 is formed on the first electrode pair 2a and the second electrode pair 2b, but the two-dimensional material layer 1 can also be formed on the first insulating film 3 or the first ferroelectric layer 5, and then the first electrode pair 2a and the second electrode pair 2b are formed on the two-dimensional material layer 1. However, when forming the first electrode pair 2a and the second electrode pair 2b, it is necessary to be careful to avoid the two-dimensional material layer 1 from being damaged by the formation process of the first electrode pair 2a and the second electrode pair 2b. For example, after covering the area of the two-dimensional material layer 1 where the first electrode pair 2a and the second electrode pair 2b are not formed with a protective film, the first electrode pair 2a and the second electrode pair 2b are formed on the two-dimensional material layer 1 exposed from the protective film. In this way, the two-dimensional material layer 1 is prevented from being damaged by the formation process of the first electrode pair 2a and the second electrode pair 2b.
[0126] <Operation Principle of Electromagnetic Wave Detector 100>
[0127] Reference Figures 1 to 3 The operating principle of the electromagnetic wave detector 100 according to this embodiment will be described.
[0128] In the dark state, the first voltage source 31 included in the first operating circuit 30 applies a bias voltage V between the first electrode 21 and the second electrode 22. d1 The second voltage source 34 included in the second operation circuit 33 applies a bias voltage V between the third electrode 25 and the fourth electrode 26. d2 A current I flows in the two-dimensional material layer 1 (the first elongated portion 11) between the first electrode 21 and the second electrode 22. d1 A current I flows in the two-dimensional material layer 1 (the second elongated portion 12) between the third electrode 25 and the fourth electrode 26. d2 The first ammeter included in the first signal detector 41 detects the current I flowing through the two-dimensional material layer 1 (the first elongated portion 11) between the first electrode 21 and the second electrode 22. d1The second ammeter included in the second signal detector 42 detects the current I flowing through the two-dimensional material layer 1 (the second elongated portion 12) between the third electrode 25 and the fourth electrode 26. d2 . Adjust the bias voltage V d1 and bias voltage V d2 So that in the dark state the current I d1 With current I d2 are equal to each other.
[0129] Next, the first ferroelectric layer 5 is irradiated with electromagnetic waves. The first ferroelectric layer 5 has a pyroelectric effect, which causes a change in the spontaneous polarization of the first ferroelectric layer 5. The second direction in which the first electrode 21 and the second electrode 22 face each other is different from the first direction (y direction) perpendicular to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. Therefore, the change in the spontaneous polarization in the first ferroelectric layer 5 causes a gradient of charge density to be generated in the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22, thereby imparting an electric field change to the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22. Specifically, a change in the spontaneous polarization of the first ferroelectric layer 5 is generated in the x direction, and a potential difference is generated between the first electrode 21 and the second electrode 22. As a result, the two-dimensional material layer 1 becomes in a state where a pn junction is falsely formed, and the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 changes. It is also called a photo-gating effect. Due to the change in the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22, the current I flowing through the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 d1 The current flowing through the two-dimensional material layer 1 when the first ferroelectric layer 5 is irradiated with electromagnetic waves is sometimes referred to as photocurrent.
[0130] In contrast, the first direction in which the third electrode 25 and the fourth electrode 26 face each other is perpendicular to the first polarization direction (x direction) of the spontaneous polarization of the first ferroelectric layer 5. Therefore, in the first direction, no polarization change of the first ferroelectric layer 5 occurs. No potential difference is generated between the third electrode 25 and the fourth electrode 26, and no electric field change occurs in the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26. The current I flowing through the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26 is d2 There is no change between the dark state and the bright state. That is, when the electromagnetic wave is irradiated, only the current I d1 Therefore, by detecting the current I by the signal detection circuit 40 d1 With current I d2 The differential signal of can make the dark current zero and can extract the photocurrent only when the electromagnetic wave is irradiated. In other words, by detecting the current I d1 With current I d2The differential signal can detect the electromagnetic waves irradiated to the electromagnetic wave detector 100.
[0131] <Operation of Electromagnetic Wave Detector 100>
[0132] Reference Figures 1 to 3 The specific operation of the electromagnetic wave detector 100 of this embodiment is described below. For example, a case where graphene is used as the two-dimensional material layer 1 and lithium niobate (LiNbO 3 ) as the operation of the electromagnetic wave detector 100 of the first ferroelectric layer 5.
[0133] like Figure 1 As shown, when a voltage is applied to the first electrode pair 2 a and the second electrode pair 2 b , a current flows in the two-dimensional material layer 1 .
[0134] When an electromagnetic wave of a detection wavelength is incident on the first ferroelectric layer 5, a change in spontaneous polarization is generated in the first ferroelectric layer 5 through the pyroelectric effect. Specifically, a change in spontaneous polarization is generated in the orientation (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. Due to the change in spontaneous polarization in the first ferroelectric layer 5, a gradient of charge density is generated in the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22, and an electric field change is generated in the two-dimensional material layer 1. As described above, the graphene constituting the two-dimensional material layer 1 has a high mobility and can obtain a large displacement current for a small electric field change. Therefore, the Fermi level of the two-dimensional material layer 1 changes significantly through the pyroelectric effect of the first ferroelectric layer 5, and a pn junction is falsely formed in the plane of the two-dimensional material layer 1. As a result, a potential difference is generated between the first electrode 21 and the second electrode 22, and a current flows in the two-dimensional material layer 1. In this way, in the electromagnetic wave detector 100 involved in this embodiment, the current generated does not depend on the quantum efficiency of the absorbing material. Therefore, the quantum efficiency of the electromagnetic wave detector 100 exceeds 100%, and the sensitivity of the electromagnetic wave detector 100 can be increased.
[0135] Furthermore, if the design is performed in such a way that the speed of change of the spontaneous polarization of the first ferroelectric layer 5 is as fast as possible, the time from the time when the electromagnetic wave is incident on the electromagnetic wave detector 100 to the time when the resistance change occurs in the two-dimensional material layer 1 is shortened. According to such an electromagnetic wave detector 100, the delay of amplification caused by the optical gating effect is eliminated, and the high-speed response of the electromagnetic wave detector 100 can be achieved.
[0136] (Variation Example)
[0137] like Figure 4 As shown, in the electromagnetic wave detector 101 according to the first modified example of the present embodiment, the first insulating film 3 is omitted, and the first electrode pair 2 a and the second electrode pair 2 b are formed on the first ferroelectric layer 5 .
[0138] In the electrode forming process in the manufacturing method of the electromagnetic wave detector 101 of the first variant of the present embodiment, the first electrode pair 2a and the second electrode pair 2b are formed on the first ferroelectric layer 5. Before forming the first electrode pair 2a and the second electrode pair 2b, a bonding layer (not shown) may be formed in the region where the first electrode pair 2a and the second electrode pair 2b are to be formed in the first main surface 5a of the first ferroelectric layer 5. The bonding layer improves the bonding between the first electrode pair 2a and the first ferroelectric layer 5 and the bonding between the second electrode pair 2b and the first ferroelectric layer 5.
[0139] like Figure 5 As shown, the electromagnetic wave detector 102 involved in the second variant of the present embodiment is constructed in the same manner as the electromagnetic wave detector 101 involved in the first variant of the present embodiment, but further includes a substrate 6. The substrate 6 is arranged between the first ferroelectric layer 5 and the back electrode 4. The substrate 6 includes a main surface 6a and a main surface 6b on the opposite side of the main surface 6a. The first ferroelectric layer 5 is formed on the main surface 6a of the substrate 6. The second main surface 5b of the first ferroelectric layer 5 is opposite to the main surface 6a of the substrate 6. The back electrode 4 is formed on the main surface 6b. In the case where the substrate 6 is formed of a semiconductor material such as silicon, for example, the first action circuit 30, the second action circuit 33 and the signal detection circuit 40 can also be formed on the substrate 6.
[0140] In the preparation process of the manufacturing method of the electromagnetic wave detector 102 of the second variant of the present embodiment, the substrate 6 is prepared. In the manufacturing method of the electromagnetic wave detector 102 of the second variant of the present embodiment, the ferroelectric layer forming process is performed after the preparation process. In the ferroelectric layer forming process, the first ferroelectric layer 5 is formed on the substrate 6. There is no particular limitation on the method for forming the first ferroelectric layer 5.
[0141] For example, when the first ferroelectric layer 5 is formed of a ferroelectric polymer material, a ferroelectric polymer film is formed on the main surface 6a of the substrate 6 by spin coating or the like. Then, the ferroelectric polymer film is patterned by photolithography. In this way, the first ferroelectric layer 5 is formed.
[0142] In the case where the material of the first ferroelectric layer 5 is a material different from the ferroelectric polymer material, the first ferroelectric layer 5 is formed by sputtering, evaporation, metal organic decomposition method (MOD coating method, MOD: Metal Organic Composition) or ALD (Atomic Layer Deposition) method. Then, the first ferroelectric layer 5 is patterned by photolithography. In this way, the first ferroelectric layer 5 is formed. The lift-off method can also be used in the patterning of the first ferroelectric layer 5. In the lift-off method, a patterned resist mask is formed on the main surface 6a of the substrate 6. Next, the first ferroelectric layer 5 is formed on the resist mask and on the main surface 6a of the substrate 6 exposed from the resist mask. The resist mask is removed. In this way, the first ferroelectric layer 5 is patterned.
[0143] Alternatively, the first ferroelectric layer 5 may be formed by bonding a ferroelectric substrate to the substrate 6. For example, SiO is formed on the substrate 6 and the ferroelectric substrate. 2 The oxide film formed on the substrate 6 and the oxide film formed on the ferroelectric substrate are made to face each other, and the substrate 6 formed with the oxide film and the ferroelectric substrate formed with the oxide film are combined with each other by thermal compression bonding or the like. A first ferroelectric layer 5 including a substrate 6 and a ferroelectric substrate joined to the substrate 6 is obtained. In addition, after the ferroelectric substrate is joined to the substrate 6, the ferroelectric substrate can be ground to make the ferroelectric substrate thinner, thereby obtaining the first ferroelectric layer 5.
[0144] like Fig. 6A As shown, in the electromagnetic wave detector 103a according to the third modified example of the present embodiment, in the plan view of the first main surface 5a, the first elongated portion 11 has a shape that gradually tapers toward the common portion 13. In the plan view of the first main surface 5a, the second elongated portion 12 has a shape that gradually tapers toward the common portion 13. Therefore, the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 is d1 The third electrode 25 and the fourth electrode 26 are not easily flown into the common portion 13. The current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 d2 The current I is less likely to flow into the first electrode 21 and the second electrode 22 in the common portion 13. In the signal detection circuit 40, the current I can be detected more accurately and easily. d1 With current I d2 By doing so, the sensitivity of the electromagnetic wave detector 103a is improved. The OFF action of the electromagnetic wave detector 103a is further improved.
[0145] like Figure 6BAs shown, in the electromagnetic wave detector 103b involved in the fourth variant of the present embodiment, in the plan view of the first main surface 5a, the first slender portion 11 has a tapered shape that gradually becomes thinner as it moves from the first electrode 21 toward the second electrode 22. Therefore, the contact area between the first electrode 21 and the first slender portion 11 is different from the contact area between the second electrode 22 and the first slender portion 11. The contact resistance between the first electrode 21 and the first slender portion 11 is different from the contact resistance between the second electrode 22 and the first slender portion 11. In the second direction in which the first electrode 21 and the second electrode 22 face each other, a temperature gradient is generated in the two-dimensional material layer 1. As a result, a temperature gradient is generated in the first ferroelectric layer 5 in the second direction. When a photocurrent is generated when an electromagnetic wave is irradiated, the polarization change of the first ferroelectric layer 5 in the second direction is enhanced.
[0146] In contrast, the first direction in which the third electrode 25 and the fourth electrode 26 face each other is perpendicular to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. When irradiated with electromagnetic waves, no polarization change of the first ferroelectric layer 5 occurs in the first direction. The current I flowing through the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26 is d2 There is no change between when electromagnetic waves are irradiated (bright state) and when electromagnetic waves are not irradiated (dark state). Therefore, the current I d1 With current I d2 In the signal detection circuit 40, the current I can be detected more accurately and easily. d1 With current I d2 By doing so, the sensitivity of the electromagnetic wave detector 103b is improved. The OFF action of the electromagnetic wave detector 103b is further improved.
[0147] The second elongated portion 12 preferably has the same shape as the first elongated portion 11. For example, in a plan view of the first main surface 5a, the second elongated portion 12 has a tapered shape that gradually becomes thinner from the third electrode 25 toward the fourth electrode 26. Therefore, the current I d2 Equal to the current I when no electromagnetic wave is irradiated d1 When electromagnetic waves are not irradiated (dark state), the signal output from the signal detection circuit 40 can be made zero. The influence of dark current can be eliminated from the signal output from the signal detection circuit 40 in the bright state. The OFF operation of the electromagnetic wave detector 100 is improved.
[0148] The shape of the first elongated portion 11 is not limited to a triangle as long as it generates a temperature gradient in the two-dimensional material layer 1 in the second direction in which the first electrode 21 and the second electrode 22 face each other. For example, a hole may be provided in the first elongated portion 11 to generate a temperature gradient in the two-dimensional material layer 1 in the second direction.
[0149] In the fifth variation of the present embodiment, the first action circuit 30 may also include, for example, a first current source (not shown) for applying a bias current between the first electrode 21 and the second electrode 22. The first current source applies a bias current to the first elongated portion 11 of the two-dimensional material layer 1. The second action circuit 33 may also include, for example, a second current source (not shown) for applying a bias current between the third electrode 25 and the fourth electrode 26. The second current source applies a bias current to the second elongated portion 12 of the two-dimensional material layer 1. The first current source and the second current source are, for example, constant current sources. The first signal detector 41 includes, for example, a first voltmeter. The first voltmeter detects a voltage generated in the first electrode pair 2a by applying a bias current between the first action circuit 30 and the second electrode 22. The second signal detector 42 includes, for example, a second voltmeter. The second voltmeter detects a voltage generated in the second electrode pair 2b by applying a bias current between the third electrode 25 and the fourth electrode 26 by the second action circuit 33. The differentiator 44 outputs a differential signal between the voltage generated in the first electrode pair 2a and the voltage generated in the second electrode pair 2b.
[0150] In the sixth variation of the present embodiment, the electromagnetic wave detector 100 is configured in the same manner as the electromagnetic wave detector 100 of the present embodiment, but the first action circuit 30 and the second action circuit 33 can be omitted. Therefore, the electromagnetic wave detector 100 generates a change in the current flowing in the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 only when the electromagnetic wave is irradiated. Therefore, the dark current can be made zero. The noise of the electromagnetic wave detector 100 can be suppressed. However, in the sixth variation of the present embodiment, the current flowing through the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 is smaller than the current flowing through the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 in the electromagnetic wave detector 100 of the present embodiment including the first action circuit 30 and the second action circuit 33. In the sixth variation of the present embodiment, the signal output from the signal detection circuit 40 becomes smaller than that of the electromagnetic wave detector 100 of the present embodiment.
[0151] In the seventh variation of the present embodiment, the configuration is the same as the fifth variation of the present embodiment, but the first action circuit 30 and the second action circuit 33 can be omitted. Therefore, the electromagnetic wave detector 100 generates a change in the voltage generated in the first electrode pair 2a only when the electromagnetic wave is irradiated. Therefore, the dark current can be made zero. The noise of the electromagnetic wave detector 100 can be suppressed. However, in the seventh variation of the present embodiment, the voltage generated in the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 is smaller than the voltage generated in the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 in the seventh variation of the present embodiment including the first action circuit 30 and the second action circuit 33. In the seventh variation of the present embodiment, the signal output from the signal detection circuit 40 becomes smaller than that in the fifth variation of the present embodiment.
[0152] <Effects>
[0153] The effects of this embodiment will be described.
[0154] In the electromagnetic wave detectors 100, 101, 102, 103a, 103b according to the present embodiment, Figures 1 to 3 As shown, on the first ferroelectric layer 5, the first electrode pair 2a and the second electrode pair 2b are electrically connected to the two-dimensional material layer 1. Therefore, when the spontaneous polarization of the first ferroelectric layer 5 changes due to the pyroelectric effect, the resistance of the two-dimensional material layer 1 between the first electrode 21 and the second electrode 22 may change. As a result, the conductivity of the two-dimensional material layer 1 is modulated by the above-mentioned photo-gating effect, and the photocurrent can be amplified in the two-dimensional material layer 1.
[0155] The change in current in the two-dimensional material layer 1 caused by the change in the spontaneous polarization of the first ferroelectric layer 5 is larger than the change in current in a normal semiconductor. In particular, in the two-dimensional material layer 1, a large current change occurs for a small potential change compared to a normal semiconductor. For example, when a single layer of graphene is used as the two-dimensional material layer 1, the thickness of the two-dimensional material layer 1 is the thickness of an atomic layer, which is extremely thin. In addition, the mobility of carriers (for example, electrons or holes) in a single layer of graphene is large. In this case, the change in current in the two-dimensional material layer 1 calculated based on the mobility of carriers in the two-dimensional material layer 1 and the thickness of the two-dimensional material layer 1 is about hundreds to thousands of times the change in current in a normal semiconductor.
[0156] Therefore, by utilizing the optical gating effect, the efficiency of extracting current from the two-dimensional material layer 1 is greatly improved. Such an optical gating effect does not directly enhance the quantum efficiency of the photoelectric conversion material as in ordinary semiconductors, but increases the current change in the two-dimensional material layer 1 caused by electromagnetic wave irradiation. Therefore, the equivalent quantum efficiency of the electromagnetic wave detectors 100, 101, 102, 103a, 103b calculated based on the differential current caused by electromagnetic wave irradiation can exceed 100%. Therefore, the electromagnetic wave detectors 100, 101, 102, 103a, 103b involved in this embodiment have a higher detection sensitivity to electromagnetic waves than the detection sensitivity of conventional semiconductor electromagnetic wave detectors to electromagnetic waves and the detection sensitivity of graphene electromagnetic wave detectors to electromagnetic waves without applying the optical gating effect.
[0157] In the electromagnetic wave detectors 100, 101, 102, 103a, and 103b according to the present embodiment, the current I d1 With current I d2 are equal to each other, and the current I is detected by the signal detection circuit 40 d1 With current I d2 Therefore, in the electromagnetic wave detectors 100, 101, 102, 103a, 103b, the dark current can be made zero, and the electrical signal can be detected only when the electromagnetic wave is irradiated. In the electromagnetic wave detector including graphene, it is difficult to perform the OFF action, so the dark current becomes large, which becomes a cause of noise. In the present embodiment, the dark current can be made zero, so even if the electromagnetic wave detectors 100, 101, 102, 103a, 103b include graphene, the noise can be reduced from the detection signal output by the signal detection circuit 40.
[0158] In addition, by using the same graphene layer as the two-dimensional material layer 1 (first elongated portion 11) between the first electrode 21 and the second electrode 22 and the two-dimensional material layer 1 (second elongated portion 12) between the third electrode 25 and the fourth electrode 26, the variation in the resistance of the two-dimensional material layer 1, which depends on the quality of graphene, can be reduced. In addition, even when different graphene layers are used between the two-dimensional material layer 1 (first elongated portion 11) between the first electrode 21 and the second electrode 22 and the two-dimensional material layer 1 (second elongated portion 12) between the third electrode 25 and the fourth electrode 26, the damage to the graphene layer caused by the manufacturing process can be made the same between the two-dimensional material layer 1 (first elongated portion 11) between the first electrode 21 and the second electrode 22 and the two-dimensional material layer 1 (second elongated portion 12) between the third electrode 25 and the fourth electrode 26. Therefore, the signal output from the signal detection circuit 40 in the dark state can be reduced.
[0159] As described above, the quantum efficiency of the electromagnetic wave detectors 100, 101, 102, 103a, 103b according to this embodiment exceeds 100%, and the sensitivity of the electromagnetic wave detectors 100, 101, 102, 103a, 103b to electromagnetic waves can be improved. In addition, the OFF operation of the electromagnetic wave detectors 100, 101, 102, 103a, 103b is improved.
[0160] Implementation method 2.
[0161] Reference Figure 7 The electromagnetic wave detector 104 according to Embodiment 2 will be described. The electromagnetic wave detector 104 according to this embodiment has the same structure as the electromagnetic wave detector 100 according to Embodiment 1 and achieves the same effects, but is different from the electromagnetic wave detector 100 according to Embodiment 1 mainly in the following points.
[0162] In the electromagnetic wave detector 104, the fourth electrode 26 included in the second electrode pair 2b is the second electrode 22 included in the first electrode pair 2a. The first electrode pair 2a and the second electrode pair 2b share one common electrode (the second electrode 22, the fourth electrode 26).
[0163] In the present embodiment, the common portion 13 of the first elongated portion 11 and the second elongated portion 12 is the end of the first elongated portion 11 close to the second electrode 22, and is the end of the second elongated portion 12 close to the fourth electrode 26. In the plan view of the first main surface 5a, the end of one side of the first elongated portion 11 overlaps the end of one side of the second elongated portion 12. In the plan view of the first main surface 5a, the shape of the two-dimensional material layer 1 is L-shaped.
[0164] The two-dimensional material layer 1 (first elongated portion 11) between the first electrode 21 and the second electrode 22 may also be formed of a material different from that of the two-dimensional material layer 1 (second elongated portion 12) between the third electrode 25 and the fourth electrode 26. In addition, as long as a common electrode (second electrode 22, fourth electrode 26) shared by the first electrode pair 2a and the second electrode pair 2b is electrically connected to the two-dimensional material layer 1 (first elongated portion 11) between the first electrode 21 and the second electrode 22 and the two-dimensional material layer 1 (second elongated portion 12) between the third electrode 25 and the fourth electrode 26, the two-dimensional material layer 1 (first elongated portion 11) between the first electrode 21 and the second electrode 22 may also be separated from the two-dimensional material layer 1 (second elongated portion 12) between the third electrode 25 and the fourth electrode 26.
[0165] <Effects>
[0166] The electromagnetic wave detector 104 according to this embodiment can reduce the number of electrodes compared to the electromagnetic wave detector 100 according to Embodiment 1. Therefore, the electromagnetic wave detector 104 can achieve a simpler structure.
[0167] Implementation method 3.
[0168] Reference Figure 8 and Fig. 9 The electromagnetic wave detector 105 according to Embodiment 3 will be described. The electromagnetic wave detector 105 according to this embodiment has the same structure as the electromagnetic wave detector 100 according to Embodiment 1 and achieves the same effects, but is different from the electromagnetic wave detector 100 according to Embodiment 1 mainly in the following points.
[0169] The electromagnetic wave detector 105 of this embodiment further includes a first semiconductor layer 7a and a second semiconductor layer 7b. The first semiconductor layer 7a is disposed between the two-dimensional material layer 1 (the first elongated portion 11) and the second electrode 22. The second semiconductor layer 7b is disposed between the two-dimensional material layer 1 (the second elongated portion 12) and the fourth electrode 26. The first semiconductor layer 7a preferably has the same structure as the second semiconductor layer 7b. The electromagnetic wave detector 105 may also include only one of the first semiconductor layer 7a and the second semiconductor layer 7b.
[0170] <Structure of the First Semiconductor Layer 7a and the Second Semiconductor Layer 7b>
[0171] The material of the first semiconductor layer 7a and the second semiconductor layer 7b is, for example, a semiconductor material such as silicon (Si). Specifically, the first semiconductor layer 7a and the second semiconductor layer 7b are silicon doped with impurities. The material of the first semiconductor layer 7a and the second semiconductor layer 7b may also be, for example, germanium (Ge) or a compound semiconductor. Compound semiconductors are, for example, silicon carbide (SiC), III-V semiconductors (gallium nitride (GaN), gallium phosphide (GaP), indium gallium arsenide (InGaAs), indium arsenide (InAs) or iridium antimonide (InSb), or II-V semiconductors (mercury cadmium telluride (HgCdTe), lead selenium (PbSe), lead sulfur (PbS) or cadmium sulfur (CdS)). The semiconductor layer 7 may also be formed by a material combining at least two of these semiconductor materials.
[0172] The first semiconductor layer 7a and the second semiconductor layer 7b may also have a multilayer structure. The semiconductor layer 7 may also include a quantum well or a quantum dot. The material of the semiconductor layer 7 may also include a Type II superlattice. The first semiconductor layer 7a and the second semiconductor layer 7b may also be a pn junction photodiode, a pin photodiode, a Schottky photodiode or an avalanche photodiode. The first semiconductor layer 7a and the second semiconductor layer 7b may also be a phototransistor.
[0173] It is desirable to dope the first semiconductor layer 7a and the second semiconductor layer 7b with impurities in such a manner that the resistivity of the first semiconductor layer 7a and the second semiconductor layer 7b is less than 100 Ω·cm. By doping the first semiconductor layer 7a and the second semiconductor layer 7b with impurities at a high concentration, the mobility of carriers (holes or electrons) in the first semiconductor layer 7a and the second semiconductor layer 7b is improved. Therefore, the response speed of the electromagnetic wave detector 105 is improved.
[0174] The thickness of the first semiconductor layer 7a and the second semiconductor layer 7b is preferably 10 μm or less. As the thickness of the first semiconductor layer 7a and the second semiconductor layer 7b decreases, deactivation of carriers (holes or electrons) in the first semiconductor layer 7a and the second semiconductor layer 7b decreases.
[0175] In order to improve the adhesion between the second electrode 22 and the first semiconductor layer 7a, a bonding layer (not shown) may be provided between the second electrode 22 and the first semiconductor layer 7a. In order to improve the adhesion between the fourth electrode 26 and the second semiconductor layer 7b, a bonding layer (not shown) may be provided between the fourth electrode 26 and the second semiconductor layer 7b. The material of the bonding layer includes, for example, a metal material such as chromium (Cr) or titanium (Ti).
[0176] <Effects>
[0177] In the electromagnetic wave detector 105 according to the present embodiment, a Schottky junction is formed between the first semiconductor layer 7a and the two-dimensional material layer 1 (the first elongated portion 11). A Schottky junction is formed between the second semiconductor layer 7b and the two-dimensional material layer 1 (the second elongated portion 12). The bias voltage V of the first voltage source 31 is adjusted. d1 and the bias voltage V of the second voltage source 34 d2 , to apply a reverse bias voltage to the Schottky junction. In this way, the current flowing through the two-dimensional material layer 1 in the dark state can be made zero. In other words, the dark current can be reduced, and the OFF operation of the electromagnetic wave detector 105 can be improved.
[0178] When electromagnetic waves are irradiated to the first ferroelectric layer 5, the spontaneous polarization of the first ferroelectric layer 5 changes due to the pyroelectric effect, and the Fermi level of the two-dimensional material layer 1 is modulated. Therefore, the energy barrier between the two-dimensional material layer 1 and the first semiconductor layer 7a decreases. As a result, only when the electromagnetic wave detector 105 is irradiated with electromagnetic waves, current flows through the first semiconductor layer 7a, and the current I is detected by the first ammeter. d1 .
[0179] When the electromagnetic wave detector 105 is irradiated with electromagnetic waves, the current I d1The change in current includes the change in the current caused by the change in the resistance of the two-dimensional material layer 1 caused by the change in the spontaneous polarization of the first ferroelectric layer 5 and the change in the current caused by the change in the energy barrier between the two-dimensional material layer 1 and the first semiconductor layer 7a. That is, in the electromagnetic wave detector 105 involved in this embodiment, in addition to being able to detect the current generated by the above-mentioned photogating effect due to the incidence of electromagnetic waves, it is also possible to detect the photocurrent caused by the change in the energy barrier between the two-dimensional material layer 1 and the first semiconductor layer 7a. A larger signal can be taken out from the signal detection circuit 40.
[0180] Implementation method 4.
[0181] Reference Fig.10 The electromagnetic wave detector 106 according to Embodiment 4 will be described. The electromagnetic wave detector 106 of this embodiment has the same structure as the electromagnetic wave detector 100 of Embodiment 1 and achieves the same effects, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following points.
[0182] In the electromagnetic wave detector 106 involved in this embodiment, a gap 8 is provided between the first insulating film 3 and the two-dimensional material layer 1. The two-dimensional material layer 1 has a portion configured separately from the first insulating film 3. The two-dimensional material layer 1 has a surface facing the gap 8. The gap 8 is provided between the first electrode 21 and the second electrode 22, and between the third electrode 25 and the fourth electrode 26. A support (not shown) for supporting the two-dimensional material layer 1 may also be provided between the two-dimensional material layer 1 and the first insulating film 3. Therefore, the gap 8 can be formed more reliably between the two-dimensional material layer 1 and the first insulating film 3.
[0183] Reference Fig.11 In the electromagnetic wave detector 107 according to the first variation of the present embodiment, the first insulating film 3 is omitted in the same manner as the electromagnetic wave detector 101 according to the first variation of the first embodiment. The gap 8 is provided between the first ferroelectric layer 5 and the two-dimensional material layer 1. A support (not shown) for supporting the two-dimensional material layer 1 may also be provided between the two-dimensional material layer 1 and the first ferroelectric layer 5. Therefore, the gap 8 can be formed more reliably between the two-dimensional material layer 1 and the first insulating film 3.
[0184] The two-dimensional material layer 1 preferably faces the gap 8 as much as possible. As long as the gap 8 can be used to suppress the influence of scattering of carriers on the surface of the first ferroelectric layer 5 or the influence of scattering of carriers on the surface of the first insulating film 3, the thickness of the gap 8 is not particularly limited. However, in order to maximize the influence of the electric field from the first ferroelectric layer 5 on the two-dimensional material layer 1, the thickness of the gap 8 is preferably as thin as possible. The thinner the thickness of the gap 8, the greater the influence of the electric field from the first ferroelectric layer 5, and the greater the change in the resistance of the two-dimensional material layer 1.
[0185] <Effects>
[0186] In the electromagnetic wave detectors 106 and 107 according to the present embodiment, between the first insulating film 3 and the two-dimensional material layer 1 (see Fig.10 ) or between the first ferroelectric layer 5 and the two-dimensional material layer 1 (refer to Fig.11 ) is provided with a gap 8. Therefore, the influence of scattering of carriers caused by the contact between the two-dimensional material layer 1 and the first insulating film 3 or the first ferroelectric layer 5 can be reduced. As a result, the decrease in the mobility of carriers in the two-dimensional material layer 1 can be suppressed. Therefore, the sensitivity of the electromagnetic wave detectors 106 and 107 can be improved.
[0187] Implementation method 5.
[0188] Reference Fig.12 The electromagnetic wave detector 108 according to Embodiment 5 will be described. The electromagnetic wave detector 108 according to this embodiment has the same structure and effects as the electromagnetic wave detector 102 according to the second variation of Embodiment 1, but is different from the electromagnetic wave detector 102 according to the second variation of Embodiment 1 mainly in the following aspects.
[0189] In the electromagnetic wave detector 108 involved in this embodiment, a hole 8b is provided in the substrate 6. The hole 8b extends from the main surface 6a to the main surface 6b, and penetrates the substrate 6 along the thickness direction (z direction) of the substrate 6. At least a part of the second main surface 5b of the first ferroelectric layer 5 is exposed from the substrate 6 at the hole 8b, and is exposed to the surrounding atmosphere of the electromagnetic wave detector 108. In the plan view of the first main surface 5a, the hole 8b overlaps with the two-dimensional material layer 1. The hole 8b is provided below the two-dimensional material layer 1.
[0190] Reference Fig.13 In the electromagnetic wave detector 108b involved in the modification of the present embodiment, the substrate 6 is omitted in the same manner as the electromagnetic wave detector 101 of the first modification of the embodiment 1. A recess 8c is provided on the second principal surface 5b of the first ferroelectric layer 5. At least a portion of the second principal surface 5b of the first ferroelectric layer 5 is exposed from the back electrode 4 at the recess 8c and is exposed to the surrounding atmosphere of the electromagnetic wave detector 108b. In the plan view of the first principal surface 5a, the recess 8c overlaps with the two-dimensional material layer 1. The recess 8c is provided below the two-dimensional material layer 1.
[0191] <Effects>
[0192] In the electromagnetic wave detector 108, a hole 8b is provided in the substrate 6, so that the contact area between the first ferroelectric layer 5 and the substrate 6 is reduced. Therefore, heat is not easily dissipated from the first ferroelectric layer 5 to the substrate 6. In the electromagnetic wave detector 108b, a recess 8c is provided in the second main surface 5b of the first ferroelectric layer 5, so that the contact area between the first ferroelectric layer 5 and the back electrode 4 is reduced. Therefore, heat is not easily dissipated from the first ferroelectric layer 5 to the back electrode 4. According to the electromagnetic wave detector 108, 108b involved in this embodiment, the thermal insulation performance of the first ferroelectric layer 5 is improved, and the heat dissipation after electromagnetic wave irradiation can be suppressed. As a result, the change in the spontaneous polarization of the first ferroelectric layer 5 can be increased. Therefore, the sensitivity of the electromagnetic wave detector 108, 108b can be improved.
[0193] Implementation method 6.
[0194] Reference Fig.14 The electromagnetic wave detector 109 according to Embodiment 6 will be described. The electromagnetic wave detector 109 according to this embodiment has the same effects as the electromagnetic wave detector 102 according to the second modification of Embodiment 1, but is different from the electromagnetic wave detector 102 according to the second modification of Embodiment 1 mainly in the following aspects.
[0195] The thickness of the first ferroelectric layer 5 varies between the first electrode 21 and the second electrode 22. The height of the first principal surface 5a varies between the first electrode 21 and the second electrode 22. Specifically, the first ferroelectric layer 5 includes a first ferroelectric layer portion 51 and a second ferroelectric layer portion 52. In a plan view of the first principal surface 5a, the first ferroelectric layer portion 51 is arranged on the first electrode 21 side, and the second ferroelectric layer portion 52 is arranged on the second electrode 22 side. The first ferroelectric layer portion 51 and the second ferroelectric layer portion 52 are arranged in a second direction (for example, the x direction) in which the first electrode 21 and the second electrode 22 face each other. The thickness of the second ferroelectric layer portion 52 is different from that of the first ferroelectric layer portion 51. For example, the second ferroelectric layer portion 52 is thinner than the first ferroelectric layer portion 51. A step 55 is formed at the boundary between the first ferroelectric layer portion 51 and the second ferroelectric layer portion 52. The second main surface 5 b of the first ferroelectric layer 5 is flush with the first ferroelectric layer portion 51 and the second ferroelectric layer portion 52 .
[0196] The first elongated portion 11 of the two-dimensional material layer 1 is disposed on the first ferroelectric layer portion 51 and the second ferroelectric layer portion 52. The two-dimensional material layer 1 covers the step 55.
[0197] The first ferroelectric layer 5 is preferably constructed to avoid changes in spontaneous polarization between the third electrode 25 and the fourth electrode 26. Therefore, for example, the first ferroelectric layer 5 located between the third electrode 25 and the fourth electrode 26 in a planar view of the first principal surface 5a may have a constant structure in a direction in which the third electrode 25 and the fourth electrode 26 are separated from each other, and may have a symmetrical structure in the polarization direction of the spontaneous polarization of the first ferroelectric layer. In addition, as long as the first ferroelectric layer 5 is constructed in a manner to avoid changes in spontaneous polarization between the third electrode 25 and the fourth electrode 26, the polarization directions of the first ferroelectric layer portion 51 and the second ferroelectric layer portion 52 may not be in the x direction, and may be in the z direction, for example. Furthermore, between the first electrode 21 and the second electrode 22, the first ferroelectric layer 5 may include three or more ferroelectric layer portions having different thicknesses. The thickness of the first ferroelectric layer 5 may continuously change between the first electrode 21 and the second electrode 22 , and the first principal surface 5 a of the first ferroelectric layer 5 may be inclined with respect to the second principal surface 5 b of the first ferroelectric layer 5 .
[0198] <Effects>
[0199] In the electromagnetic wave detector 109 involved in the present embodiment, the thickness of the first ferroelectric layer 5 varies between the first electrode 21 and the second electrode 22. If the thickness of the first ferroelectric layer 5 varies, the voltage change amount generated in the two-dimensional material layer 1 by the thermoelectric effect of the first ferroelectric layer 5 also varies. That is, the voltage change amount generated in the two-dimensional material layer 1 on the portion of the first ferroelectric layer 5 having a larger thickness (the first ferroelectric layer portion 51) is different from the voltage change amount generated in the two-dimensional material layer 1 on the portion of the first ferroelectric layer 5 having a smaller thickness (the second ferroelectric layer portion 52). Therefore, the voltage applied to the two-dimensional material layer 1 on the portion of the first ferroelectric layer 5 having a larger thickness (the first ferroelectric layer portion 51) is different from the voltage applied to the two-dimensional material layer 1 on the portion of the first ferroelectric layer 5 having a smaller thickness (the second ferroelectric layer portion 52). A pn junction is falsely formed in the two-dimensional material layer 1, and the efficiency of extracting current from the two-dimensional material layer 1 is improved. In addition, the influence of the change in the spontaneous polarization of the first ferroelectric layer 5 of the two-dimensional material layer 1 upon irradiation with electromagnetic waves becomes greater. Therefore, the detection sensitivity of the electromagnetic wave detector 109 is improved.
[0200] Implementation method 7.
[0201] Reference Fig.15 The electromagnetic wave detector 110 according to Embodiment 7 will be described. The electromagnetic wave detector 110 of this embodiment has the same structure and effects as the electromagnetic wave detector 100 of Embodiment 1, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following points.
[0202] The dielectric constant of the first ferroelectric layer 5 changes between the first electrode 21 and the second electrode 22. Specifically, the first ferroelectric layer 5 includes a first ferroelectric layer portion 51 and a second ferroelectric layer portion 52. In a plan view of the first principal surface 5a, the first ferroelectric layer portion 51 is arranged on the first electrode 21 side, and the second ferroelectric layer portion 52 is arranged on the second electrode 22 side. The first ferroelectric layer portion 51 and the second ferroelectric layer portion 52 are arranged in a second direction (for example, the x direction) in which the first electrode 21 and the second electrode 22 face each other. The dielectric constant of the first ferroelectric layer portion 51 is different from the dielectric constant of the second ferroelectric layer portion 52. For example, the ferroelectric material forming the first ferroelectric layer portion 51 is different from the ferroelectric material forming the second ferroelectric layer portion 52. The absorption wavelength range of the first ferroelectric layer portion 51 may also be different from the absorption wavelength range of the second ferroelectric layer portion 52.
[0203] The first elongated portion 11 of the two-dimensional material layer 1 is disposed on the first ferroelectric layer portion 51 and the second ferroelectric layer portion 52 .
[0204] The first ferroelectric layer 5 is preferably constructed to avoid changes in spontaneous polarization between the third electrode 25 and the fourth electrode 26. The first ferroelectric layer 5 may also include three or more ferroelectric layer portions having different polarizabilities. In addition, as long as the first ferroelectric layer 5 is constructed in a manner to avoid changes in spontaneous polarization between the third electrode 25 and the fourth electrode 26, the polarization directions of the first ferroelectric layer portion 51 and the second ferroelectric layer portion 52 may not be in the x direction, but may be in the z direction, for example.
[0205] <Effects>
[0206] In the electromagnetic wave detector 110 involved in the present embodiment, the dielectric constant of the first ferroelectric layer portion 51 is different from the dielectric constant of the second ferroelectric layer portion 52. If the dielectric constants of the ferroelectrics are different, the voltage change amount generated in the two-dimensional material layer 1 by the thermoelectric effect of the ferroelectrics is also different. That is, the voltage change amount generated in the two-dimensional material layer 1 located on the first ferroelectric layer portion 51 is different from the voltage change amount generated in the two-dimensional material layer 1 located on the second ferroelectric layer portion 52. Therefore, the voltage applied to the two-dimensional material layer 1 located on the first ferroelectric layer portion 51 is different from the voltage applied to the two-dimensional material layer 1 located on the second ferroelectric layer portion 52, and a pn junction is falsely formed in the two-dimensional material layer 1. The efficiency of extracting current from the two-dimensional material layer 1 is improved. In addition, the influence of the change in the spontaneous polarization of the first ferroelectric layer 5 of the two-dimensional material layer 1 when irradiated with electromagnetic waves becomes larger. Therefore, the detection sensitivity of the electromagnetic wave detector 110 is improved.
[0207] By making the absorption wavelength range of the first ferroelectric layer portion 51 different from the absorption wavelength range of the second ferroelectric layer portion 52, the electromagnetic wave detector 110 has sensitivity in a plurality of wavelength ranges. The detection band of the electromagnetic wave detector 110 for electromagnetic waves can be expanded.
[0208] Implementation method 8.
[0209] Reference Figures 16 to 18 The electromagnetic wave detector 111 according to Embodiment 8 will be described. The electromagnetic wave detector 111 of this embodiment has the same structure and effects as the electromagnetic wave detector 100 of Embodiment 1, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following points.
[0210] In the electromagnetic wave detector 111 according to the present embodiment, the first electrode 21 is formed of a metal material different from that of the second electrode 22. The third electrode 25 is formed of a metal material different from that of the fourth electrode 26. The first electrode 21 may be formed of the same material as that of the third electrode 25. The second electrode 22 may be formed of the same material as that of the fourth electrode 26.
[0211] <Effects>
[0212] In the electromagnetic wave detector 111 according to the present embodiment, the first electrode 21 is formed of a metal material different from that of the second electrode 22 . The third electrode 25 is formed of a metal material different from that of the fourth electrode 26 .
[0213] When the two-dimensional material layer 1 and the metal are in contact with each other, carriers (holes or electrons) are doped from the metal into the two-dimensional material layer 1 due to the difference between the work function of the metal and the work function of the material (e.g., graphene) forming the two-dimensional material layer 1. The Fermi level of the two-dimensional material layer 1 changes, or the contact resistance between the two-dimensional material layer 1 and the metal changes.
[0214] Therefore, if the first electrode 21 is formed of a metal material different from that of the second electrode 22, the energy gap of the first portion of the two-dimensional material layer 1 in contact with the first electrode 21 is different from the energy gap of the second portion of the two-dimensional material layer 1 in contact with the second electrode 22. If the third electrode 25 is formed of a metal material different from that of the fourth electrode 26, the energy gap of the third portion of the two-dimensional material layer 1 in contact with the third electrode 25 is different from the energy gap of the fourth portion of the two-dimensional material layer 1 in contact with the fourth electrode 26. The two-dimensional material layer 1 is in a state where a pn junction is falsely formed. Thus, the efficiency of taking out an electrical signal (e.g., current) from the first electrode pair 2a and the efficiency of taking out an electrical signal (e.g., current) from the second electrode pair 2b are improved. The sensitivity of the electromagnetic wave detector 111 can be improved.
[0215] Implementation method 9.
[0216] Reference Figures 19 to 21A The electromagnetic wave detector 112a according to Embodiment 9 will be described. The electromagnetic wave detector 112a of this embodiment has the same structure as the electromagnetic wave detector 100 of Embodiment 1 and achieves the same effects, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following points.
[0217] The electromagnetic wave detector 112 a according to the present embodiment further includes a first contact layer 9 a and a second contact layer 9 b . The first contact layer 9 a and the second contact layer 9 b are in contact with the two-dimensional material layer 1 .
[0218] Specifically, the first contact layer 9a contacts the first elongated portion 11 of the two-dimensional material layer 1. The first contact layer 9a is arranged at a portion of the first elongated portion 11 close to the second electrode 22. The first contact layer 9a is arranged at a position of the first elongated portion 11 closer to the second electrode 22 than the common portion 13 of the first elongated portion 11 and the second elongated portion 12. The second contact layer 9b contacts the second elongated portion 12 of the two-dimensional material layer 1. The second contact layer 9b is arranged at a portion of the second elongated portion 12 close to the fourth electrode 26. The second contact layer 9b is arranged at a position of the second elongated portion 12 closer to the fourth electrode 26 than the common portion 13 of the first elongated portion 11 and the second elongated portion 12. Preferably, the relative position of the first contact layer 9a with respect to the first elongated portion 11 is the same as the relative position of the second contact layer 9b with respect to the second elongated portion 12.
[0219] The first contact layer 9a contacts the first elongated portion 11 of the two-dimensional material layer 1 and supplies carriers (holes or electrons) to the first elongated portion 11. The first elongated portion 11 is doped by the first contact layer 9a. The second contact layer 9b contacts the second elongated portion 12 of the two-dimensional material layer 1 and supplies carriers (holes or electrons) to the second elongated portion 12. The second elongated portion 12 is doped by the second contact layer 9b.
[0220] Therefore, the energy gap of the first portion in the two-dimensional material layer 1 that contacts the first electrode 21 is different from the energy gap of the second portion in the two-dimensional material layer 1 that contacts the second electrode 22. The energy gap of the third portion in the two-dimensional material layer 1 that contacts the third electrode 25 is different from the energy gap of the fourth portion in the two-dimensional material layer 1 that contacts the fourth electrode 26. The two-dimensional material layer 1 is in a state where a pn junction is falsely formed. Therefore, the efficiency of taking out an electrical signal (e.g., current) from the first electrode pair 2a and the efficiency of taking out an electrical signal (e.g., current) from the second electrode pair 2b are improved. The sensitivity of the electromagnetic wave detector 112a can be improved.
[0221] The first contact layer 9a and the second contact layer 9b need to have a thickness sufficient to dope carriers (holes or electrons) into the two-dimensional material layer 1. However, in order to prevent the electromagnetic wave from being absorbed by the first contact layer 9a and the second contact layer 9b and excessively attenuated from reaching the two-dimensional material layer 1, the first insulating film 3, and the first ferroelectric layer 5 when the electromagnetic wave is irradiated onto the two-dimensional material layer 1, the thickness of the first contact layer 9a and the thickness of the second contact layer 9b are preferably thin.
[0222] The first contact layer 9a and the second contact layer 9b only need to be configured to form a gradient of charge density in the two-dimensional material layer 1. Each of the first contact layer 9a and the second contact layer 9b may also include a plurality of contact portions. The plurality of contact portions may be stacked on the two-dimensional material layer 1 or arranged in parallel on the two-dimensional material layer 1. The plurality of contact portions may be formed of the same material or different materials.
[0223] Hereinafter, the first contact layer 9a and the second contact layer 9b will be described in detail.
[0224] The material of the first contact layer 9a and the second contact layer 9b may be any material as long as it generates charge bias and polarization, for example, it may be an organic substance, a metal, a semiconductor, an insulator or a two-dimensional material, or a mixture of any of these materials.
[0225] In the case where the materials of the first contact layer 9a and the second contact layer 9b are inorganic substances, the two-dimensional material layer 1 is doped as follows through the first contact layer 9a and the second contact layer 9b. If the work function of the first contact layer 9a and the second contact layer 9b is greater than the work function of the two-dimensional material layer 1, the two-dimensional material layer 1 is doped to a p-type through the first contact layer 9a and the second contact layer 9b. If the work function of the first contact layer 9a and the second contact layer 9b is less than the work function of the two-dimensional material layer 1, the two-dimensional material layer 1 is doped to an n-type.
[0226] In contrast, organic matter does not have a clear work function. Therefore, when the materials of the first contact layer 9a and the second contact layer 9b are organic matter, the manner in which the first contact layer 9a and the second contact layer 9b dope the two-dimensional material layer 1 is determined based on the polar groups of the materials of the first contact layer 9a and the second contact layer 9b. The polar groups of the materials of the first contact layer 9a and the second contact layer 9b are determined based on the polarity of the molecules of the organic matter constituting the materials of the first contact layer 9a and the second contact layer 9b.
[0227] The material of the first contact layer 9a and the second contact layer 9b is, for example, a positive photoresist. The positive photoresist is, for example, a composition containing a photosensitive agent having a quinone diazide group and a phenolic varnish resin. In the case where the material of the first contact layer 9a and the second contact layer 9b is a positive photoresist, the area in the two-dimensional material layer 1 where the positive photoresist is formed becomes a p-type area. The positive photoresist is formed on the two-dimensional material layer 1, for example, by a photolithography process. Thus, there is no need for a process of forming a mask in contact with the two-dimensional material layer 1. It is possible to suppress the two-dimensional material layer 1 from being damaged by the mask formation process, and the process can be simplified.
[0228] The material of the first contact layer 9a and the second contact layer 9b may be, for example, a material having a polar group. More specifically, the material of the first contact layer 9a and the second contact layer 9b may be, for example, a material having an electron-withdrawing group. The material having an electron-withdrawing group reduces the electron density of the two-dimensional material layer 1. The material having an electron-withdrawing group is, for example, a material having a halogen, a nitrile, a carboxyl or a carbonyl group. The material of the first contact layer 9a and the second contact layer 9b may be, for example, a material having an electron-donating group. The material having an electron-donating group increases the electron density of the two-dimensional material layer 1. The material having an electron-donating group is, for example, a material having an alkyl, a hydroxyl or an amino group.
[0229] The material of the first contact layer 9a and the second contact layer 9b may also be a material that undergoes a polarity change when the first contact layer 9a and the second contact layer 9b are irradiated with electromagnetic waves. In this specification, polarity change refers to the phenomenon that a polar group changes chemically. Polarity change refers to, for example, the phenomenon that an electron-withdrawing group changes into an electron-donating group, the phenomenon that an electron-donating group changes into an electron-withdrawing group, the phenomenon that a polar group changes into a non-polar group, or the phenomenon that a non-polar group changes into a polar group. The electromagnetic wave that produces the polarity change may have a detection wavelength or may not have a detection wavelength. There is no particular limitation on the material that produces the polarity change, and it may be, for example, a photoresist. By producing a polarity change in the first contact layer 9a and the second contact layer 9b, the carriers (holes or electrons) generated during the polarity change are supplied to the two-dimensional material layer 1. The portion of the two-dimensional material layer 1 that is in contact with the first contact layer 9a and the second contact layer 9b is doped with carriers (holes or electrons).
[0230] As the material of the first contact layer 9a and the second contact layer 9b, a material that undergoes polarity change by being irradiated with an electromagnetic wave having a detection wavelength may also be selected. Therefore, polarity change occurs in the first contact layer 9a and the second contact layer 9b only when being irradiated with an electromagnetic wave having a detection wavelength. Carriers are doped in the two-dimensional material layer 1 only when being irradiated with an electromagnetic wave having a detection wavelength, and the photocurrent flowing through the two-dimensional material layer 1 can be increased.
[0231] As the material of the first contact layer 9a and the second contact layer 9b, a material that undergoes a polarity change by being irradiated with an electromagnetic wave that does not have a detection wavelength can also be selected. In this case, the first contact layer 9a and the second contact layer 9b can also be removed after the electromagnetic wave that does not have a detection wavelength is irradiated to the first contact layer 9a and the second contact layer 9b. Even after the first contact layer 9a and the second contact layer 9b are removed, the portion of the two-dimensional material layer 1 that has been in contact with the first contact layer 9a and the second contact layer 9b is still doped with carriers (holes or electrons). In addition, by removing the first contact layer 9a and the second contact layer 9b, the area of the two-dimensional material layer 1, the area of the first insulating film 3, and the area of the first ferroelectric layer 5 that are irradiated with electromagnetic waves having a detection wavelength increase. Therefore, the detection sensitivity of the electromagnetic wave detector 112a can be improved.
[0232] The materials of the first contact layer 9a and the second contact layer 9b may also be materials that produce a redox reaction when the first contact layer 9a and the second contact layer 9b are irradiated with electromagnetic waves. Thus, carriers (holes or electrons) generated by the redox reaction are doped into the two-dimensional material layer 1. The electromagnetic wave that produces the redox reaction may have a detection wavelength or may not have a detection wavelength.
[0233] The electromagnetic wave that causes the first contact layer 9a and the second contact layer 9b to produce a redox reaction may also be an electromagnetic wave having a detection wavelength. Only when the electromagnetic wave having a detection wavelength is irradiated, carriers are doped in the two-dimensional material layer 1, and the photocurrent flowing through the two-dimensional material layer 1 can be increased. The electromagnetic wave that causes the first contact layer 9a and the second contact layer 9b to produce a redox reaction may also be an electromagnetic wave without a detection wavelength. In the case where the electromagnetic wave that causes the first contact layer 9a and the second contact layer 9b to produce a redox reaction is an electromagnetic wave without a detection wavelength, the first contact layer 9a and the second contact layer 9b may also be removed after the electromagnetic wave without a detection wavelength is irradiated to the first contact layer 9a and the second contact layer 9b.
[0234] The first contact layer 9a and the second contact layer 9b may also be formed of a material that supplies molecules to the two-dimensional material layer 1. For example, the first contact layer 9a and the second contact layer 9b may also be a liquid layer or a gas layer containing molecules, and the two-dimensional material layer 1 is immersed in the liquid layer or exposed to the gas layer. Carriers can be supplied from the liquid layer or the gas layer to the two-dimensional material layer 1 at the molecular level.
[0235] <Effects>
[0236] In the electromagnetic wave detector 112a involved in this embodiment, the first contact layer 9a and the second contact layer 9b are in contact with the two-dimensional material layer 1, and carriers (holes or electrons) are supplied to the two-dimensional material layer 1. The portion of the two-dimensional material layer 1 in contact with the first contact layer 9a and the portion of the two-dimensional material layer 1 in contact with the second contact layer 9b are doped to n-type or p-type. Therefore, the energy gap of the first portion of the two-dimensional material layer 1 in contact with the first electrode 21 is different from the energy gap of the second portion of the two-dimensional material layer 1 in contact with the second electrode 22. The energy gap of the third portion of the two-dimensional material layer 1 in contact with the third electrode 25 is different from the energy gap of the fourth portion of the two-dimensional material layer 1 in contact with the fourth electrode 26. The efficiency of taking out an electrical signal (for example, a current) from the first electrode pair 2a and the efficiency of taking out an electrical signal (for example, a current) from the second electrode pair 2b are improved. The sensitivity of the electromagnetic wave detector 112a can be improved.
[0237] Implementation method 10.
[0238] Reference Fig. 21B and Fig. 21C The structure of the electromagnetic wave detector 112b according to Embodiment 10 will be described. The electromagnetic wave detector 112b of this embodiment has the same structure and effects as the electromagnetic wave detector 100 of Embodiment 1, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following points.
[0239] The electromagnetic wave detector 112b also includes an electromagnetic wave shielding member 60. The electromagnetic wave shielding member 60 shields electromagnetic waves to prevent electromagnetic waves from being incident on a portion of the first ferroelectric layer 5. Therefore, in the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5, a gradient of polarizability is generated in the first ferroelectric layer 5. The electromagnetic wave shielding member 60 is formed of a material that shields electromagnetic waves having an absorption wavelength of the first ferroelectric layer 5. The electromagnetic wave shielding member 60 is formed of, for example, a metal such as a black body, aluminum (Al) or gold (Au), or a material processed by aluminum oxide.
[0240] In the present embodiment, the electromagnetic wave is incident on the electromagnetic wave detector 112b from the first electrode pair 2a side relative to the first ferroelectric layer 5, so the electromagnetic wave shielding member 60 is arranged on the side opposite to the first ferroelectric layer 5 side (above the first electrode 21) relative to the first electrode 21. The electromagnetic wave shielding member 60 is arranged separately from the two-dimensional material layer 1. Therefore, the electromagnetic wave shielding member 60 does not deteriorate the mobility of the two-dimensional material layer 1.
[0241] The electromagnetic wave shielding member 60 covers only one side of the first ferroelectric layer 5 relative to the center of the first ferroelectric layer 5 in the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5 in the plan view of the first main surface 5a. Therefore, the electromagnetic wave shielding member 60 shields electromagnetic waves only on one side of the first ferroelectric layer 5. One side can be Fig. 21B and Fig. 21C As shown, it is the first electrode 21 side, but it may be the second electrode 22 side.
[0242] When electromagnetic waves are incident on the electromagnetic wave detector 112b from the back electrode 4 side relative to the first ferroelectric layer 5, the electromagnetic wave shielding member 60 is arranged on the side opposite to the first ferroelectric layer 5 side (below the back electrode 4) relative to the back electrode 4. The electromagnetic wave shielding member 60 may be in contact with the two-dimensional material layer 1 as long as the mobility of the two-dimensional material layer 1 is not degraded.
[0243] In the case where electromagnetic waves are incident on the electromagnetic wave detector 112b from the first electrode pair 2a side relative to the first ferroelectric layer 5, and the first electrode pair 2a is not transparent to the electromagnetic waves, one of the first electrode 21 and the second electrode 22 may be enlarged and the enlarged portion of one of the first electrode 21 and the second electrode 22 may function as an electromagnetic wave shielding member for the electromagnetic waves, instead of providing the electromagnetic wave shielding member 60. In the case where electromagnetic waves are incident on the electromagnetic wave detector 112b from the back electrode 4 side relative to the first ferroelectric layer 5, and the back electrode 4 is not transparent to the electromagnetic waves, the back electrode 4 may function as an electromagnetic wave shielding member for the electromagnetic waves, instead of providing the electromagnetic wave shielding member 60.
[0244] The electromagnetic wave shielding member 60 is disposed, for example, so as not to shield the two-dimensional material layer 1 from electromagnetic waves. The electromagnetic wave shielding member 60 may be disposed so as to completely shield the two-dimensional material layer 1 from electromagnetic waves.
[0245] <Effects>
[0246] The electromagnetic wave shielding member 60 covers only one side of the first ferroelectric layer 5 relative to the center of the first ferroelectric layer 5 in the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5 in the plan view of the first main surface 5a. Therefore, the electromagnetic wave is not irradiated to one side of the first ferroelectric layer 5 due to the electromagnetic wave shielding member 60, but is irradiated to the other side of the first ferroelectric layer 5. In the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5, the polarizability of the first ferroelectric layer 5 changes. Specifically, on one side of the first ferroelectric layer 5, the polarizability of the first ferroelectric layer 5 does not change, while on the other side of the first ferroelectric layer 5, the polarizability of the first ferroelectric layer 5 changes. As a result, a polarization change occurs in the first ferroelectric layer 5 in the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. As a result, a charge density gradient is formed in the two-dimensional material layer 1, and the resistance of the two-dimensional material layer 1 changes between the first electrode 21 and the second electrode 22. As a result, the photocurrent extracted from the first electrode pair 2a increases, thereby improving the sensitivity of the electromagnetic wave detector 112b.
[0247] Implementation method 11.
[0248] Reference Fig. 22 and Fig.23 The structure of the electromagnetic wave detector 113 according to Embodiment 11 will be described. The electromagnetic wave detector 113 of this embodiment has the same structure and effects as the electromagnetic wave detector 100 of Embodiment 1, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following aspects.
[0249] In the electromagnetic wave detector 113 involved in this embodiment, the first elongated portion 11 and the second elongated portion 12 are different layers and are stacked on each other. The second elongated portion 12 is stacked on the first elongated portion 11. The second elongated portion 12 is arranged on the side opposite to the first ferroelectric layer 5 relative to the first elongated portion 11. The first elongated portion 11 is arranged between the second elongated portion 12 and the first ferroelectric layer 5.
[0250] For example, the two-dimensional material layer 1 is formed by the following method. The two-dimensional material film is transferred onto the first insulating film 3, the first electrode pair 2a and the second electrode pair 2b. The two-dimensional material film is patterned by a photolithography process and an etching process to form the first elongated portion 11. Then, the second elongated portion 12 is also formed by the same process as the first elongated portion 11. In order to prevent the first elongated portion 11 from being damaged when the second elongated portion 12 is patterned, a protective film (not shown) may also be formed on the first elongated portion 11 after the first elongated portion 11 is formed and before the second elongated portion 12 is formed.
[0251] <Effects>
[0252] In the electromagnetic wave detector 113 according to the present embodiment, the first elongated portion 11 and the second elongated portion 12 are stacked on each other. The second elongated portion 12 is arranged on the side of the first elongated portion 11 opposite to the first ferroelectric layer 5 .
[0253] The resistance between adjacent two-dimensional material layers is much greater than the resistance within the plane of the two-dimensional material layer 1. Therefore, in the electromagnetic wave detector 113 according to the present embodiment, the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 is greater than that in the electromagnetic wave detector 100 according to the first embodiment. d1 The path of the current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 is d2 The current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 is d1 Furthermore, it is difficult to flow into the third electrode 25 and the fourth electrode 26. The current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 d2 Furthermore, it is less likely to flow into the first electrode 21 and the second electrode 22. In addition, the second elongated portion 12 is less likely to be affected by the change in the spontaneous polarization of the first ferroelectric layer 5 when the electromagnetic wave is irradiated. The current I between the time of irradiation and the time of non-irradiation of the electromagnetic wave d1 The change in the current I between when the electromagnetic wave is irradiated and when it is not irradiated increases. d2 The change is reduced.
[0254] Therefore, in the signal detection circuit 40, the current I d1 With current I d2 The sensitivity of the electromagnetic wave detector 113 is improved. The OFF action of the electromagnetic wave detector 113 is further improved.
[0255] The first elongated portion 11 and the second elongated portion 12 are respectively stacked bodies of a plurality of graphene layers, and a moiré superlattice, a magic angle, or random stacking may be formed by adjusting the rotation angle of the lattice in each of the plurality of graphene layers.
[0256] By using the moiré superlattice in the first elongated portion 11 and the second elongated portion 12, a band gap corresponding to the stacking angle of a plurality of graphene layers can be formed. Therefore, the sensitivity of the electromagnetic wave detector 113 to an arbitrary wavelength can be enhanced.
[0257] By stacking adjacent graphene layers among a plurality of graphene layers so as to be offset by a magic angle (a rotation angle of a lattice of about 1.1 degrees), superconductivity exhibited in the first elongated portion 11 and the second elongated portion 12 can be controlled with a small voltage change. Therefore, the dark current of the electromagnetic wave detector 113 can be reduced.
[0258] If multiple graphene layers are lattice mismatched and randomly stacked, the interaction between the multiple graphene layers is reduced, and each of the multiple graphene layers behaves equally to a single layer of graphene. Therefore, it is possible to suppress the decrease in mobility caused by stacking multiple graphene layers. The sensitivity of the electromagnetic wave detector 113 is improved.
[0259] Implementation method 12.
[0260] Reference Fig.24 and Fig.25 The electromagnetic wave detector 114 according to Embodiment 12 will be described. The electromagnetic wave detector 114 according to this embodiment has the same structure and effects as the electromagnetic wave detector 113 according to Embodiment 11, but is different from the electromagnetic wave detector 113 according to Embodiment 11 mainly in the following respects.
[0261] The electromagnetic wave detector 114 according to the present embodiment further includes a second insulating film 3b. The second insulating film 3b is disposed between the first elongated portion 11 and the second elongated portion 12. The second insulating film 3b electrically insulates the second elongated portion 12 from the first elongated portion 11. The second insulating film 3b is formed after the first elongated portion 11 is formed and before the second elongated portion 12 is formed.
[0262] <Effects>
[0263] The electromagnetic wave detector 114 according to the present embodiment further includes a second insulating film 3 b. The second insulating film 3 b is disposed between the first elongated portion 11 and the second elongated portion 12.
[0264] Therefore, in the electromagnetic wave detector 114 according to the present embodiment, the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 is greater than that in the electromagnetic wave detector 113 according to the eleventh embodiment. d1 The path of the current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 is further d2 Prevent the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 from flowing. d1 The current I of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 is prevented from flowing. d2The second elongated portion 12 is further less susceptible to the change in the spontaneous polarization of the first ferroelectric layer 5 when the electromagnetic wave is irradiated. The current I between the time of irradiation and the time of non-irradiation of the electromagnetic wave d1 The change in the current I between when the electromagnetic wave is irradiated and when it is not irradiated increases. d2 The change is reduced.
[0265] Therefore, in the signal detection circuit 40, the current I d1 With current I d2 The sensitivity of the electromagnetic wave detector 114 is improved. The OFF action of the electromagnetic wave detector 114 is further improved.
[0266] Implementation method 13.
[0267] Reference Fig.26 and Fig. 27 The electromagnetic wave detector 115 according to Embodiment 13 will be described. The electromagnetic wave detector 115 according to this embodiment has the same structure and effects as the electromagnetic wave detector 114 according to Embodiment 12, but is different from the electromagnetic wave detector 114 according to Embodiment 12 mainly in the following respects.
[0268] The electromagnetic wave detector 115 according to the present embodiment further includes gate insulating films 3 c and 3 d and gate electrodes 28 and 29 .
[0269] The gate insulating film 3c is disposed on the first elongated portion 11. The gate insulating film 3c is in contact with the first elongated portion 11. The gate insulating film 3c may be disposed between the first elongated portion 11 and the second elongated portion 12, or may electrically insulate the first elongated portion 11 from the second elongated portion 12. In a plan view of the first main surface 5a, the gate insulating film 3c includes a portion exposed from the second elongated portion 12.
[0270] The gate electrode 28 is disposed on the gate insulating film 3c. Specifically, the gate electrode 28 is disposed on a portion of the gate insulating film 3c that is exposed from the second elongated portion 12. In a plan view of the first main surface 5a, at least a portion of the gate electrode 28 overlaps with a portion of the two-dimensional material layer 1 that is located between the first electrode 21 and the second electrode 22. The first electrode 21 is, for example, a drain electrode, and the second electrode 22 is, for example, a source electrode.
[0271] The gate insulating film 3d is disposed on the second elongated portion 12. Specifically, the gate insulating film 3d is disposed on the surface opposite to the surface facing the first ferroelectric layer 5. The gate insulating film 3d is in contact with the second elongated portion 12.
[0272] The gate electrode 29 is disposed on the gate insulating film 3d. In a plan view of the first main surface 5a, at least a portion of the gate electrode 29 overlaps with a portion of the two-dimensional material layer 1 located between the third electrode 25 and the fourth electrode 26. The third electrode 25 is, for example, a drain electrode, and the fourth electrode 26 is, for example, a source electrode.
[0273] (Variation Example)
[0274] There is no particular limitation on the shape and number of the gate insulating film 3c and the gate electrode 28. There is no particular limitation on the shape and number of the gate insulating film 3d and the gate electrode 29. The gate insulating films 3c, 3d and the gate electrodes 28, 29 may also be provided on the two-dimensional material layer 1 of the first embodiment.
[0275] The electromagnetic wave detector 115 may also include one of the gate insulating films 3c and 3d and one of the gate electrodes 28 and 29, and omit the other of the gate insulating films 3c and 3d and the other of the gate electrodes 28 and 29. That is, the electromagnetic wave detector 115 may also include the gate insulating film 3c and the gate electrode 28 provided on the two-dimensional material layer 1, but not include the gate insulating film 3d and the gate electrode 29. The electromagnetic wave detector 115 may also include the gate insulating film 3d and the gate electrode 29 provided on the two-dimensional material layer 1, but not include the gate insulating film 3c and the gate electrode 28.
[0276] <Effects>
[0277] According to the electromagnetic wave detector 115 of this embodiment, a gate voltage can be applied to the two-dimensional material layer 1 from the gate electrodes 28 and 29. Therefore, the resistance and mobility of the two-dimensional material layer 1 can be controlled. d1 and current I d2 Therefore, in the signal detection circuit 40, the current I can be easily detected. d1 With current I d2 The performance of the electromagnetic wave detector 115 can be improved.
[0278] Implementation method 14.
[0279] Reference Fig.28 and Fig.29 The electromagnetic wave detector 116 according to Embodiment 14 will be described. The electromagnetic wave detector 116 according to this embodiment has the same effects as the electromagnetic wave detector 113 according to Embodiment 11, but is different from the electromagnetic wave detector 113 according to Embodiment 11 mainly in the following respects.
[0280] The electromagnetic wave detector 116 involved in this embodiment also has a second ferroelectric layer 5c with spontaneous polarization. The second ferroelectric layer 5c is formed on the second slender portion 12. The second ferroelectric layer 5c is arranged on the side opposite to the first ferroelectric layer 5 relative to the second slender portion 12. The second ferroelectric layer 5c is arranged on the side opposite to the first ferroelectric layer 5 relative to the first slender portion 11. The second polarization direction of the spontaneous polarization of the second ferroelectric layer 5c is parallel to the first direction (y direction) perpendicular to the first polarization direction (+x direction) of the spontaneous polarization of the first ferroelectric layer 5. The second polarization direction of the spontaneous polarization of the second ferroelectric layer 5c is parallel to the first direction (y direction) in which the third electrode 25 and the fourth electrode 26 face each other or the long side direction (y direction) of the second slender portion 12. In the planar view of the first main surface 5a, the second ferroelectric layer 5c preferably covers the two-dimensional material layer 1 between the third electrode 25 and the fourth electrode 26.
[0281] (Variation Example)
[0282] The second ferroelectric layer 5c may also be disposed on the second elongated portion 12 of the two-dimensional material layer 1 of embodiment 1. As long as the second elongated portion 12 is electrically connected to the second electrode pair 2b, the second ferroelectric layer 5c may also be disposed below the second elongated portion 12 (for example, between the first elongated portion 11 and the second elongated portion 12).
[0283] <Effects>
[0284] When the electromagnetic wave detector 116 involved in this embodiment is irradiated with electromagnetic waves, the spontaneous polarization of the first ferroelectric layer 5 and the spontaneous polarization of the second ferroelectric layer 5c change. The first polarization direction of the spontaneous polarization of the first ferroelectric layer 5 is parallel to the second direction (x direction) in which the first electrode 21 and the second electrode 22 are facing each other, so the first slender portion 11 between the first electrode 21 and the second electrode 22 is affected by the change in the spontaneous polarization of the first ferroelectric layer 5. The second polarization direction of the spontaneous polarization of the second ferroelectric layer 5c is parallel to the first direction (y direction) in which the third electrode 25 and the fourth electrode 26 are facing each other, so the second slender portion 12 between the third electrode 25 and the fourth electrode 26 is affected by the change in the spontaneous polarization of the second ferroelectric layer 5c.
[0285] Therefore, when the electromagnetic wave detector 116 is irradiated with electromagnetic waves, not only the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 d1 changes, and the current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 d2 By making the current I d1 The change of current I d2 The change of the detection current I d1and current I d2 , the current I detected in the signal detection circuit 40 d1 With current I d2 The differential signal between them increases. d1 The change of current I d2 The change of the detection current I d1 and current I d2 This can be achieved, for example, by adjusting the first polarization direction of the spontaneous polarization of the first ferroelectric layer 5, the second polarization direction of the spontaneous polarization of the second ferroelectric layer 5c, the bias voltage V d1 and the bias voltage V d2 Thus, the sensitivity of the electromagnetic wave detector 116 is improved. The OFF action of the electromagnetic wave detector 116 is further improved.
[0286] Implementation method 15.
[0287] Reference Fig.30 The electromagnetic wave detector 117 according to Embodiment 15 will be described. The electromagnetic wave detector 117 of this embodiment has the same structure and effects as the electromagnetic wave detector 100 of Embodiment 1, but is different from the electromagnetic wave detector 100 of Embodiment 1 mainly in the following points.
[0288] The electromagnetic wave detector 117 according to the present embodiment includes an operation circuit 35 and a balance circuit 36 .
[0289] The action circuit 35 is connected to at least one of the first electrode pair 2a and the second electrode pair 2b. In the present embodiment, the action circuit 35 is connected to both the first electrode pair 2a and the second electrode pair 2b. Specifically, the action circuit 35 includes a first action circuit 30 connected to the first electrode pair 2a and a second action circuit 33 connected to the second electrode pair 2b. The first action circuit 30 of the present embodiment is configured in the same manner as the first action circuit 30 of embodiment 1. The second action circuit 33 of the present embodiment is configured in the same manner as the second action circuit 33 of embodiment 1.
[0290] The balancing circuit 36 is connected to the first electrode pair 2a and the second electrode pair 2b. Specifically, the balancing circuit 36 is connected to one of the first electrode 21 and the second electrode 22 and one of the third electrode 25 and the fourth electrode 26. In this embodiment, the balancing circuit 36 is connected to the second electrode 22 and the fourth electrode 26. In this way, the balancing circuit 36 is electrically connected to the two-dimensional material layer 1. Specifically, the balancing circuit 36 is electrically connected to the first elongated portion 11 and the second elongated portion 12. The balancing circuit 36 includes a plurality of resistor elements. The plurality of resistor elements can be either fixed resistors or variable resistors. The balancing circuit 36, the first elongated portion 11 between the first electrode 21 and the second electrode 22, and the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 form a bridge circuit.
[0291] In this embodiment, the signal detection circuit 40 is connected to the second electrode 22 and the fourth electrode 26. The signal detection circuit 40 of this embodiment is configured similarly to the signal detection circuit 40 of Embodiment 1. For example, the signal detection circuit 40 includes a first signal detector 41 (see Figure 1 ) and the second signal detector 42 (refer to Figure 1 ). The first signal detector 41 and the second signal detector 42 may be either an ammeter or a voltmeter.
[0292] The operation circuit 35 and the balance circuit 36 can adjust the first electrical signal output from the first electrode pair 2 a and the second electrical signal output from the second electrode pair 2 b .
[0293] For example, the first operating circuit 30 and the second operating circuit 33 are voltage sources. By adjusting the bias voltage V applied from the first operating circuit 30 to the first elongated portion 11, d1 (Refer to Figure 1 and Figure 2 ), it is possible to adjust the signal provided by the first signal detector 41 (refer to Figure 1 ) is detected as the first electrical signal current I d1 (Refer to Figure 1 and Figure 2 ). By adjusting the bias voltage V applied from the second action circuit 33 to the second elongated portion 12 d2 (Refer to Figure 1 and Figure 3 ), it is possible to adjust the signal provided by the second signal detector 42 (refer to Figure 1 ) is detected as the second electrical signal I d2 (Refer to Figure 1 and Figure 3 The balancing circuit 36 is electrically connected to the first elongated portion 11 and the second elongated portion 12, so that the current I as the first electrical signal can be adjusted. d1 and the current I as the second electrical signald2 .
[0294] In addition, the case where the first action circuit 30 and the second action circuit 33 are current sources is as follows. By adjusting the bias current flowing from the first action circuit 30 to the first elongated portion 11, the current generated by the first signal detector 41 (see Figure 1 ) is detected as a first electrical signal between the first electrode 21 and the second electrode 22. By adjusting the bias current flowing from the second operating circuit 33 through the second elongated portion 12, the voltage detected by the second signal detector 42 (see Figure 1 ) is detected as a voltage between the third electrode 25 and the fourth electrode 26 as the second electrical signal. The balancing circuit 36 is electrically connected to the first elongated portion 11 and the second elongated portion 12, so that the voltage between the first electrode 21 and the second electrode 22 as the first electrical signal and the voltage between the third electrode 25 and the fourth electrode 26 as the second electrical signal can be adjusted.
[0295] The operation circuit 35 and the balance circuit 36 are adjusted so that when no electromagnetic wave is irradiated to the electromagnetic wave detector 117 (dark state), the resistance of the first elongated portion 11 between the first electrode 21 and the second electrode 22 and the resistance of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 are equal to each other. Therefore, when the first signal detector 41 and the second signal detector 42 are ammeters, in the dark state, the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22 is equal to d1 =I = 1, which is equal to the current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26. d2 When the first signal detector 41 and the second signal detector 42 are voltmeters, in the dark state, the voltage of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is equal to the voltage of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26. Therefore, the electrical signal output from the signal detection circuit 40 is zero.
[0296] (Variation Example)
[0297] As long as the resistance of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is equal to the resistance of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26, the electromagnetic wave detector 117 may include only one of the operating circuit 35 and the balancing circuit 36, and not include the other of the operating circuit 35 and the balancing circuit 36. That is, at least one of the operating circuit 35 and the balancing circuit 36 is adjusted so that the resistance of the first elongated portion 11 between the first electrode 21 and the second electrode 22 is equal to the resistance of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 in the dark state.
[0298] <Effects>
[0299] In the electromagnetic wave detector 117 involved in this embodiment, the first electrical signal output from the first electrode pair 2a and the second electrical signal output from the second electrode pair 2b can be adjusted by at least one of the action circuit 35 and the balance circuit 36. Therefore, the resistance of the first elongated portion 11 between the first electrode 21 and the second electrode 22 and the resistance of the second elongated portion 12 between the third electrode 25 and the fourth electrode 26 can be made equal to each other by at least one of the action circuit 35 and the balance circuit 36. The dark current can be reduced. In addition, the first electrical signal output from the first electrode pair 2a in the bright state (for example, the current I flowing through the first elongated portion 11 between the first electrode 21 and the second electrode 22) can be detected by the signal detection circuit 40. d1 ) and a second electrical signal output from the second electrode pair 2b (eg, a current I flowing through the second elongated portion 12 between the third electrode 25 and the fourth electrode 26). d2 ) The OFF action of the electromagnetic wave detector 117 is improved.
[0300] Implementation method 16.
[0301] Reference Fig.31 The electromagnetic wave detector 118 according to Embodiment 16 will be described. The electromagnetic wave detector 118 according to Embodiment 16 has the same structure and effects as the electromagnetic wave detector 100 according to Embodiment 1, but is different from the electromagnetic wave detector 100 according to Embodiment 1 mainly in the following points.
[0302] In the electromagnetic wave detector 118 involved in this embodiment, the signal detection circuit 40 includes a differential amplifier circuit 45. The differential amplifier circuit 45 is connected to one of the first electrode 21 and the second electrode 22 included in the first electrode pair 2a (the first electrode 21 in this embodiment). The signal detection circuit 40 is connected to one of the third electrode 25 and the fourth electrode 26 included in the second electrode pair 2b (the third electrode 25 in this embodiment).
[0303] The differential amplifier circuit 45 may also include an operational amplifier 46. Specifically, the differential amplifier circuit 45 may also be an integration circuit including the operational amplifier 46, a power supply 47, and a capacitor 48. The negative terminal of the operational amplifier 46 is connected to one of the first electrode 21 and the second electrode 22 (the first electrode 21 in this embodiment) and one of the third electrode 25 and the fourth electrode 26 (the third electrode 25 in this embodiment). The power supply 47 is connected to the positive terminal of the operational amplifier 46 and the ground potential. The capacitor 48 is connected in parallel with the operational amplifier 46. Specifically, the capacitor 48 is connected to the negative terminal of the operational amplifier 46 and the output terminal of the operational amplifier 46.
[0304] <Effects>
[0305] The electromagnetic wave detector 118 according to this embodiment includes the differential amplifier circuit 45, and therefore does not require a balancing circuit (see Fig.30 ). Therefore, the electromagnetic wave detector 118 can be miniaturized. In addition, the differential amplifier circuit 45 includes the operational amplifier 46, so that the average value of the differential signal between the first electrical signal and the second electrical signal can be obtained. Therefore, the S / N ratio of the differential signal output from the signal detection circuit 40 is improved. The performance of the electromagnetic wave detector 118 is improved.
[0306] Implementation method 17.
[0307] Reference Fig.32 The electromagnetic wave detector array 120 according to the seventeenth embodiment will be described.
[0308] The electromagnetic wave detector array 120 includes a plurality of electromagnetic wave detectors 121. The plurality of electromagnetic wave detectors 121 are any of the electromagnetic wave detectors 100-118 of Embodiments 1 to 16 and their modifications. The plurality of electromagnetic wave detectors 121 have the same structure as each other. Therefore, the electromagnetic wave detector array 120 has an improved detection sensitivity to electromagnetic waves.
[0309] The plurality of electromagnetic wave detectors 121 are arranged along at least any one of a third direction 126 and a fourth direction 127 different from the third direction 126. The fourth direction 127 is, for example, perpendicular to the third direction 126. In the present embodiment, the plurality of electromagnetic wave detectors 121 are arranged along the third direction 126 and the fourth direction 127, and are configured in a 2×2 array. The number of electromagnetic wave detectors 121 provided by the electromagnetic wave detector array 120 is not limited to four. For example, the number of electromagnetic wave detectors 121 provided by the electromagnetic wave detector array 120 may also be nine, and the plurality of electromagnetic wave detectors 121 may be configured in a 3×3 array. The plurality of electromagnetic wave detectors 121 may be arranged periodically or non-periodically. The plurality of electromagnetic wave detectors 121 may also be configured on the substrate 6.
[0310] Reference Fig.33 The electromagnetic wave detector array 120 according to the modification of the present embodiment includes a plurality of electromagnetic wave detectors 121, 122, 123, and 124. The plurality of electromagnetic wave detectors 121, 122, 123, and 124 are any of the electromagnetic wave detectors 100 to 118 according to Embodiments 1 to 16. The plurality of electromagnetic wave detectors 121, 122, 123, and 124 have mutually different structures.
[0311] For example, the plurality of electromagnetic wave detectors 121, 122, 123, and 124 may have different detection wavelengths. Figure 2 and Figure 3 etc.) or the first semiconductor layer 7a (refer to Figure 8 ) and the second semiconductor layer 7b (refer to Fig. 9 ) is sensitive to electromagnetic waves (i.e., absorbs electromagnetic waves), by making the material of the first ferroelectric layer 5 or the materials of the first semiconductor layer 7a and the second semiconductor layer 7b different among the multiple electromagnetic wave detectors 121, 122, 123, 124, the multiple electromagnetic wave detectors 121, 122, 123, 124 can have different detection wavelengths.
[0312] Therefore, the electromagnetic wave detector array 120 can detect a plurality of electromagnetic waves having different wavelengths. The electromagnetic wave detector array 120 can detect electromagnetic waves in a larger wavelength range. The electromagnetic wave detector array 120 can, for example, identify the wavelength of electromagnetic waves in any wavelength range such as ultraviolet light, infrared light, terahertz waves, or radio waves. For example, when the detection wavelength of a part of the plurality of electromagnetic wave detectors 121, 122, 123, and 124 is visible light, and the detection wavelength of the rest of the plurality of electromagnetic wave detectors 121, 122, 123, and 124 is infrared light, the electromagnetic wave detector 100 can be used as a visible light image camera during the day and as an infrared image camera at night.
[0313] The plurality of electromagnetic wave detectors 121, 122, 123, 124 may have, for example, different polarization sensitivities. For example, the electromagnetic wave detector 121 may be sensitive to electromagnetic waves having a polarization angle of 0°, the electromagnetic wave detector 122 may be sensitive to electromagnetic waves having a polarization angle of 45°, the electromagnetic wave detector 123 may be sensitive to electromagnetic waves having a polarization angle of 90°, and the electromagnetic wave detector 124 may be sensitive to electromagnetic waves having a polarization angle of 135°. For example, in the case where the two-dimensional material layer 1 of the plurality of electromagnetic wave detectors 121, 122, 123, 124 has a structure in which graphene nanoribbons are periodically arranged, the orientation of the periodic arrangement of the graphene nanoribbons may be changed among the plurality of electromagnetic wave detectors 121, 122, 123, 124 so that the plurality of electromagnetic wave detectors 121, 122, 123, 124 have different polarization sensitivities.
[0314] Reference Fig.34 and Fig.35 , the electromagnetic wave detector array 120 of this embodiment can be used as an image sensor 130.
[0315] For example, the electromagnetic wave detector array 120 having a plurality of electromagnetic wave detectors 121, 122, 123, and 124 having different detection wavelengths can be used as an image sensor capable of detecting a plurality of electromagnetic waves having different wavelengths. Thus, it is possible to detect a plurality of electromagnetic waves having different wavelengths without using a color filter that is conventionally required in a CMOS (Complementary MOS) sensor or the like. In addition, a colorized image can be obtained in which the difference in the wavelength of the electromagnetic wave is represented as a difference in color.
[0316] For example, an electromagnetic wave detector array 120 having a plurality of electromagnetic wave detectors 121, 122, 123, and 124 having different polarization sensitivities can be used as a polarization recognition imaging sensor. For example, by configuring a plurality of electromagnetic wave detectors 121 having sensitivity to electromagnetic waves having a polarization angle of 0°, an electromagnetic wave detector 122 having sensitivity to electromagnetic waves having a polarization angle of 90°, an electromagnetic wave detector 123 having sensitivity to electromagnetic waves having a polarization angle of 45°, and an electromagnetic wave detector 124 having sensitivity to electromagnetic waves having a polarization angle of 135°, a polarization recognition imaging sensor can be formed. The polarization recognition imaging sensor can, for example, realize the recognition of man-made objects and natural objects, the recognition of materials, the recognition of multiple objects having the same temperature in the infrared wavelength range, the recognition of boundaries between multiple objects, or an equivalent improvement in resolution, etc.
[0317] like Fig.34 and Fig.35 As shown, the image sensor 130 may also include a readout circuit 131 in addition to the electromagnetic wave detector array 120 of the present disclosure. The readout circuit 131 is electrically connected to the electromagnetic wave detector array 120. The readout circuit 131 uses a CTIA (Capacitive Transimpedance Amplifier) type, but is not limited to this method and may also be other readout methods.
[0318] The electromagnetic wave detector included in the image sensor 130 (for example, the electromagnetic wave detector 100) further includes an insulating layer 133, extraction electrodes 134, 136, and pads 135, 137. The insulating layer 133 covers the two-dimensional material layer 1. The extraction electrode 134 is electrically connected to the first electrode 21 and is extracted onto the insulating layer 133. The pad 135 is arranged on the extraction electrode 134 and the insulating layer 133. The extraction electrode 136 is electrically connected to the third electrode 25 and is extracted onto the insulating layer 133. The pad 137 is arranged on the extraction electrode 136 and the insulating layer 133. The two-dimensional material layer 1 is electrically insulated from the extraction electrodes 134, 136. The material constituting the pads 135, 137 is a conductive material such as aluminum silicon, nickel or gold.
[0319] The pad 135 is electrically connected to the readout circuit 131 via the bump 138. The pad 137 is electrically connected to the readout circuit 131 via the bump 139. In other words, the readout circuit 131 and the electromagnetic wave detector (for example, the electromagnetic wave detector 100) included in the image sensor 130 are so-called hybrid-connected. The material constituting the bumps 138 and 139 is a conductive material such as indium.
[0320] The electromagnetic wave detector array 120 may also be used as a sensor other than the image sensor 130. The electromagnetic wave detector array 120 can be used, for example, as a position detection sensor that detects the position of an object.
[0321] In the embodiments 1 to 17 and their modifications, the first insulating film 3 (see Figures 1 to 3 etc.), the first semiconductor layer 7a (refer to Figure 8 ) and the second semiconductor layer 7b (refer to Fig. 9 ), and the first contact layer 9a (refer to Fig.19 and Fig. 20 ) and the second contact layer 9b (refer to Fig.19 and Fig.21A ) can be formed of a material whose characteristics change when irradiated with electromagnetic waves, thereby generating a change in potential in the two-dimensional material layer 1. Such materials are, for example, quantum dots, ferroelectric materials, liquid crystal materials, fullerenes, rare earth oxides, semiconductor materials, pn junction materials, metal-semiconductor bonding materials or metal-insulator-semiconductor bonding materials. For example, in the case where the first contact layer 9a and the second contact layer 9b are formed of a material whose characteristics change when irradiated with electromagnetic waves, thereby imparting a change in potential to the two-dimensional material layer 1, the first contact layer 9a and the second contact layer 9b do not need to be in direct contact with the two-dimensional material layer 1, and can be, for example, arranged above or below the two-dimensional material layer 1 via a first insulating film 3.
[0322] It should be considered that the embodiments 1-17 and their modifications disclosed this time are illustrative and not restrictive in all aspects. As long as there is no contradiction, at least two of the embodiments 1-17 and their modifications disclosed this time may be combined. The scope of the present disclosure is not indicated by the above description but by the claims, and is intended to include all changes within the meaning and scope equivalent to the claims.
Claims
1. An electromagnetic wave detector comprising: A first ferroelectric layer includes a first main surface and has a spontaneous polarization; a two-dimensional material layer, disposed on the first main surface of the first ferroelectric layer; A first electrode pair, comprising a first electrode and a second electrode; as well as a second electrode pair including a third electrode and a fourth electrode, The first electrode pair is electrically connected to the two-dimensional material layer, The second electrode pair is electrically connected to the two-dimensional material layer, In a plan view of the first main surface, the third electrode and the fourth electrode are arranged to face each other in a first direction perpendicular to a first polarization direction of the spontaneous polarization of the first ferroelectric layer. In the plan view of the first main surface, the first electrode and the second electrode are arranged to face each other in a second direction different from the first direction.
2. The electromagnetic wave detector according to claim 1, in, In the plan view of the first major surface, the second direction is parallel to the first polarization direction.
3. The electromagnetic wave detector according to claim 1 or 2, in, The two-dimensional material layer comprises a first elongated portion and a second elongated portion, The first long side direction of the first elongated portion is different from the second long side direction of the second elongated portion, In the plan view of the first major face, a portion of the first elongated portion overlaps a portion of the second elongated portion.
4. The electromagnetic wave detector according to claim 3, in, In the plan view of the first major surface, a shape of the first elongated portion between the first electrode and the second electrode is the same as a shape of the second elongated portion between the third electrode and the fourth electrode.
5. The electromagnetic wave detector according to claim 3 or 4, in, The two-dimensional material layer is formed by a single two-dimensional material layer, In the plan view of the first main surface, the first elongated portion has a shape that gradually tapers toward a common portion of the first elongated portion and the second elongated portion, In the plan view of the first main face, the second elongated portion has a shape that tapers toward the common portion.
6. The electromagnetic wave detector according to claim 3 or 4, in, The first elongated portion and the second elongated portion are stacked on top of each other, The second elongated portion is arranged on a side of the first elongated portion opposite to the first ferroelectric layer.
7. The electromagnetic wave detector according to claim 6, in, A second insulating film is further provided and is arranged between the first elongated portion and the second elongated portion.
8. The electromagnetic wave detector according to any one of claims 3 to 7, in, Also available: a first contact layer in contact with the first elongated portion; and a second contact layer in contact with the second elongated portion, The first contact layer is disposed at a portion of the first elongated portion close to the second electrode. The second contact layer is disposed at a portion of the second elongated portion close to the fourth electrode.
9. The electromagnetic wave detector according to any one of claims 3 to 8, in, It also has an electromagnetic wave shielding member, The electromagnetic wave shielding member covers only one side of the first ferroelectric layer with respect to the center of the first ferroelectric layer in the first polarization direction of the spontaneous polarization of the first ferroelectric layer in the plan view of the first main surface.
10. The electromagnetic wave detector according to any one of claims 3 to 9, in, further comprising a second ferroelectric layer having spontaneous polarization, The second ferroelectric layer is formed on the second elongated portion, A second polarization direction of the spontaneous polarization of the second ferroelectric layer is parallel to the first direction.
11. The electromagnetic wave detector according to any one of claims 1 to 4, in, The two-dimensional material layer is formed by a single two-dimensional material layer.
12. The electromagnetic wave detector according to any one of claims 1 to 11, in, The first ferroelectric layer is a ferroelectric thin film having a thickness of 10 μm or less.
13. The electromagnetic wave detector according to any one of claims 1 to 12, in, It also has a back electrode. The first ferroelectric layer includes a second main surface opposite to the first main surface. The back electrode is formed on the second main surface.
14. The electromagnetic wave detector according to any one of claims 1 to 13, in, further comprising a first insulating film, The first insulating film is formed on the first main surface of the first ferroelectric layer and is arranged between the first ferroelectric layer and the two-dimensional material layer.
15. The electromagnetic wave detector according to claim 14, in, A gap is provided between the first insulating film and the two-dimensional material layer.
16. The electromagnetic wave detector according to any one of claims 1 to 13, in, A gap is provided between the first ferroelectric layer and the two-dimensional material layer.
17. The electromagnetic wave detector according to any one of claims 1 to 16, in, The fourth electrode is the second electrode.
18. The electromagnetic wave detector according to any one of claims 1 to 17, in, A substrate is also provided. The first ferroelectric layer includes a second main surface opposite to the first main surface. The first ferroelectric layer is formed on the substrate, The second principal surface of the first ferroelectric layer faces the substrate.
19. The electromagnetic wave detector according to claim 18, in, The substrate is provided with a hole, At least a portion of the second main surface of the first ferroelectric layer is exposed to the surrounding atmosphere of the electromagnetic wave detector at the hole.
20. The electromagnetic wave detector according to any one of claims 1 to 18, in, further comprising at least one of a first semiconductor layer and a second semiconductor layer, The first semiconductor layer is disposed between the two-dimensional material layer and the second electrode. The second semiconductor layer is disposed between the two-dimensional material layer and the fourth electrode.
21. The electromagnetic wave detector according to any one of claims 1 to 20, in, The first ferroelectric layer includes a second main surface opposite to the first main surface. A recess is provided on the second main surface of the first ferroelectric layer. At least a portion of the second main surface of the first ferroelectric layer is exposed to the surrounding atmosphere of the electromagnetic wave detector at the recessed portion.
22. The electromagnetic wave detector according to any one of claims 1 to 21, in, The thickness of the first ferroelectric layer varies between the first electrode and the second electrode.
23. The electromagnetic wave detector according to any one of claims 1 to 22, in, The first ferroelectric layer includes a first ferroelectric layer portion and a second ferroelectric layer portion, The first ferroelectric layer portion and the second ferroelectric layer portion are arranged in the second direction in which the first electrode and the second electrode face each other. The dielectric constant of the first ferroelectric layer portion is different from the dielectric constant of the second ferroelectric layer portion.
24. The electromagnetic wave detector according to any one of claims 1 to 22, in, The first ferroelectric layer includes a first ferroelectric layer portion and a second ferroelectric layer portion, The first ferroelectric layer portion and the second ferroelectric layer portion are arranged in the second direction in which the first electrode and the second electrode face each other. The absorption wavelength range of the first ferroelectric layer portion is different from the absorption wavelength range of the second ferroelectric layer portion.
25. The electromagnetic wave detector according to any one of claims 1 to 24, in, The first electrode is formed of a metal material different from that of the second electrode, The third electrode is formed of a metal material different from that of the fourth electrode.
26. The electromagnetic wave detector according to any one of claims 1 to 25, in, Also available: a gate insulating film, disposed on the two-dimensional material layer; and A gate electrode is formed on the gate insulating film.
27. The electromagnetic wave detector according to any one of claims 1 to 26, in, The two-dimensional material layer is formed of any material selected from the group consisting of graphene, multilayer graphene, turbostratic graphene, transition metal dichalcogenides, black phosphorus, silicene, graphene nanoribbons, and borophene.
28. The electromagnetic wave detector according to any one of claims 1 to 27, in, A signal detection circuit is also provided, wherein the signal detection circuit includes a first signal detector, a second signal detector and a differentiator. The first signal detector is connected to the first electrode pair and detects a first electrical signal output from the first electrode pair. The second signal detector is connected to the second electrode pair and detects a second electrical signal output from the second electrode pair. The differentiator is connected to the first signal detector and the second signal detector, and outputs a differential signal between the first electrical signal and the second electrical signal.
29. The electromagnetic wave detector according to claim 28, in, further comprising at least one of an action circuit and a balance circuit, The action circuit includes a first action circuit connected to the first electrode pair and a second action circuit connected to the second electrode pair. The balancing circuit is connected to the first electrode pair and the second electrode pair, Adjust at least one of the action circuit and the balance circuit so that when no electromagnetic wave is irradiated to the electromagnetic wave detector, the resistance value of the two-dimensional material layer between the first electrode and the second electrode is equal to the resistance value of the two-dimensional material layer between the third electrode and the fourth electrode.
30. The electromagnetic wave detector according to claim 29, in, The balancing circuit includes a plurality of resistance elements. The balancing circuit, the two-dimensional material layer between the first electrode and the second electrode, and the two-dimensional material layer between the third electrode and the fourth electrode form a bridge circuit.
31. The electromagnetic wave detector according to any one of claims 1 to 27, in, It also has a signal detection circuit. The signal detection circuit includes a differential amplifier circuit connected to the first electrode pair and the second electrode pair.
32. An electromagnetic wave detector array, in, A device comprising a plurality of electromagnetic wave detectors according to any one of claims 1 to 31, The plurality of electromagnetic wave detectors are arranged along at least one of a third direction and a fourth direction different from the third direction.
33. An image sensor comprising: The electromagnetic wave detector array as claimed in claim 32; and The readout circuit is hybrid-connected to the electromagnetic wave detector array.