Method for dehydrating industrial-grade dimethyl carbonate by adopting modified molecular sieve

Through the ion exchange modification of hydrophilic molecular sieve and helium purge technology, the problems of low efficiency and environmental pollution in the water removal process of industrial-grade dimethyl carbonate are solved, and efficient water removal and purity improvement are achieved, which is suitable for industrial production.

CN118903883AActive Publication Date: 2024-11-08GUANGXI UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411203074.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The prior art has problems of low efficiency, long reaction time and environmental pollution in the water removal process of industrial grade dimethyl carbonate, and it is difficult to achieve large-scale industrial production.

Method used

Hydrophilic molecular sieve is used to change the potassium ions in the skeleton of the molecular sieve through ion exchange, enhance the polarity of the molecular sieve, and use helium purge and gas chromatography to achieve efficient water removal of industrial-grade dimethyl carbonate.

Benefits of technology

It improves the purity of dimethyl carbonate, simplifies the synthesis process, avoids environmental pollution, and has a short reaction time, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118903883A_ABST
    Figure CN118903883A_ABST
Patent Text Reader

Abstract

The invention provides a method for dewatering industrial-grade dimethyl carbonate by adopting a hydrophilic molecular sieve. The invention aims to provide the molecular sieve with good water absorption performance and stability, and the preparation method is high in efficiency, safe, green and environment-friendly and can be used for preparing the hydrophilic molecular sieve on a large scale. The method comprises the following steps: dispersing potassium hydroxide and aluminum hydroxide into a solvent, then adding strontium nitrate and silica sol to obtain a reaction solution A, and transferring the reaction solution A into a stainless steel reaction kettle with a polytetrafluoroethylene lining; reacting at 80-140 DEG C for 20-24 hours to obtain a product hydrophilic molecular sieve; soaking the molecular sieve with a silver nitrate solution to obtain a silver modified molecular sieve; belongs to the technical field of fine chemical engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fine chemical industry, and in particular to a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate and a preparation method and application of the modified hydrophilic molecular sieve. Background Art

[0002] Dimethyl carbonate (DMC) is an important organic compound with a wide range of applications in industry and laboratories. Since its molecules contain functional groups such as methyl, methoxy, carbonyl and carbonylmethyl, it can react with a variety of alcohols, phenols, amines, hydrazines, esters, etc., has a variety of reactivity, and is widely used. It was registered as a non-toxic solvent in Europe in 1992 and is an environmentally friendly organic chemical raw material that meets the requirements of modern "clean technology". DMC has excellent physical properties such as good compatibility, high dielectric constant, and low viscosity. It is widely used as a solvent for lithium-ion battery electrolytes, which enables the battery to have high current density and good anti-oxidation and reduction properties, as well as good conductivity and long battery life.

[0003] The production processes of DMC at home and abroad are mainly divided into three categories: phosgene method, methanol liquid / gas phase oxidation carbonyl method, and ester exchange method. However, industrially produced DMC may contain impurities such as water, acid, alkali or other organic matter, which may affect its performance and effect in various applications. Therefore, purifying DMC to 99.99% electronic grade is of great significance for the green transformation of new energy.

[0004] Traditional separation technologies mainly include distillation, extraction, absorption, crystallization, etc. With the development of the chemical industry, their separation efficiency and processing capacity are constantly improving; and modern separation technologies such as supercritical extraction technology, new adsorption technology, membrane separation technology, etc. are also constantly developing. Compared with other methods, adsorption separation does not require high temperature or high pressure conditions. It only achieves precise control of the separation process by adjusting parameters such as temperature and flow rate. It is low-cost, low-energy consumption, and easy to operate.

[0005] Molecular sieve is a porous material with a regular pore structure that can be used for adsorption separation. Its molecular size and shape determine its selectivity for adsorption separation. By selecting molecular sieves with different pore sizes, it is possible to achieve efficient separation of molecules of different sizes, shapes and polarities. It has a wide range of applications in petrochemicals, gas separation, environmental protection and biopharmaceuticals. Its advantages such as high selectivity, controllability and reproducibility make it an important tool in the adsorption separation process.

[0006] Chinese patent CN118026198A reports a method for synthesizing a hydrophilic molecular sieve, which introduces silanol groups to adjust the framework of the molecular sieve and improve the hydrophilicity of the molecular sieve. It also performs ion exchange to further improve the hydrophilicity, but this method has a long reaction time, low efficiency, uses a large amount of organic reagents, and is difficult to achieve industrial large-scale production. Summary of the invention

[0007] In view of the above-mentioned shortcomings, the object of the present invention is to provide a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve.

[0008] To this end, the technical solution provided by the present invention is as follows:

[0009] A method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve comprises the following steps in sequence:

[0010] 1) Place the hydrophilic molecular sieve into the adsorption column and fill both sides with quartz wool;

[0011] 2) Add deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3-5 sccm with the mass flow controller, and connect the helium for purging;

[0012] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry the deionized water through the adsorption column in step 1);

[0013] 4) Turn on the gas chromatograph and pass the tail gas described in step 3) into the gas chromatograph for real-time detection.

[0014] The hydrophilic molecular sieve structure is as follows:

[0015]

[0016] Furthermore, in the above method of removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, the ratio of the hydrophilic molecular sieve to deionized water is: 0.4-1g:30-100mL.

[0017] Furthermore, in the above method of removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, the hydrophilic molecular sieve is synthesized by the following method:

[0018] 3) Dispersing potassium hydroxide and aluminum hydroxide in a solvent, adding strontium nitrate and silica sol to mix to obtain a reaction solution, transferring the reaction solution into a reaction kettle, and reacting at 80 to 140° C. for 20 to 24 hours to obtain a product hydrophilic molecular sieve;

[0019] 4) immersing the hydrophilic molecular sieve prepared in step 1) in a silver nitrate solution for ion exchange to obtain a silver-modified hydrophilic molecular sieve;

[0020] The molar ratio of the aluminum hydroxide, silica sol, potassium hydroxide and strontium nitrate in step 1) is 0.25-0.6:1-3:0.66:0.01.

[0021] Furthermore, in the above method of removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, the solvent in step 1) is deionized water.

[0022] Furthermore, in the above method of removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, the concentration of silver nitrate in step 2) is 0.01 to 0.05 mol / L.

[0023] Furthermore, in the above method of removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, 2) the mass ratio of the hydrophilic molecular sieve to the silver nitrate solution is 1:20-50.

[0024] Furthermore, in the above method of removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, the ion exchange time in step 2) is 40 to 80 minutes.

[0025] Furthermore, in the above method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, the reactor is a stainless steel reactor lined with polytetrafluoroethylene.

[0026] Furthermore, in the above-mentioned method for preparing the hydrophilic molecular sieve for removing water from industrial-grade dimethyl carbonate, the pressure of the reaction system is normal pressure.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The technical solution molecular sieve provided in this application has no organic template, which effectively avoids environmental pollution, and the synthesis process is simple and convenient, easy to operate, and has a short reaction time.

[0029] 2. The technical solution provided in the present application is to change the potassium ions in the molecular sieve framework through ion exchange, thereby enhancing the polarity of the molecular sieve and further improving the hydrophilicity of the molecular sieve.

[0030] 3. The technical solution provided by the present invention adopts a hydrophilic molecular sieve for water removal, which can efficiently remove trace moisture in industrial-grade dimethyl carbonate, thereby improving the purity of dimethyl carbonate and meeting the demand for high-quality dimethyl carbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD pattern of the molecular sieve obtained in Example 1;

[0032] Figure 2 This is a SEM image of the molecular sieve obtained in Example 1;

[0033] Figure 3 The molecular sieve obtained in Example 1 is used as an adsorbent in the design diagram of a dynamic water adsorption device;

[0034] Figure 4 The molecular sieve obtained in implementation case 1 is used as an adsorbent in a dynamic water adsorption breakthrough diagram. DETAILED DESCRIPTION

[0035] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0036] Example 1

[0037] The present embodiment provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0038] 1) Place 0.4 g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0039] 2) Add 30 mL of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm with the mass flow controller, and connect the helium gas for purging;

[0040] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0041] 4) turning on the gas chromatograph, and passing the tail gas described in step 3) into the gas chromatograph for real-time detection;

[0042] Through real-time gas chromatography detection and analysis, water began to elute through the adsorption bed at 250 min / g for molecular sieve K-4, and water began to elute through the adsorption bed at 400 min / g for silver-modified molecular sieve AgK-0.025.

[0043] The preparation method of the hydrophilic molecular sieve used in this embodiment comprises the following steps:

[0044] (1) Add 0.7 g potassium hydroxide and 0.4 g aluminum hydroxide to 2 mL deionized water and heat at 100 °C for 10 min to obtain a clear solution.

[0045] (2) After the solution obtained in step (1) was cooled to room temperature, 0.05 g of strontium nitrate was added, and then 4.6 g of silica sol and 5 mL of deionized water were added, and the mixture was stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0046] (3) The molecular sieve gel obtained in step (2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0047] (4) The liquid after the reaction obtained in step (3) is filtered, washed, and dried to obtain the hydrophilic molecular sieve K-4.

[0048] (5) The hydrophilic molecular sieve K-4 obtained in step (4) is ion exchanged in a 0.025 mol / L silver nitrate solution in the dark for 1 hour. The solution after the reaction is filtered, washed, and dried overnight to obtain the silver-modified molecular sieve AgK-0.025.

[0049] Example 2

[0050] The present embodiment provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0051] 1) Place 0.4 g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0052] 2) Add 30 mL of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm with the mass flow controller, and connect the helium gas for purging;

[0053] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0054] 4) turning on the gas chromatograph, and passing the tail gas described in step 3) into the gas chromatograph for real-time detection; through real-time detection and analysis by gas chromatography, water begins to elute through the adsorption bed of the silver-modified molecular sieve AgK-0.05 at 250 min / g. Although the elution point in Example 1 is the same as that in the unmodified state, the mass transfer area slope of the silver-modified molecular sieve AgK-0.05 is higher, and the diffusion coefficient of water molecules inside the pores is stronger.

[0055] A method for preparing a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate comprises the following steps:

[0056] 1) Add 0.7 g potassium hydroxide and 0.4 g aluminum hydroxide to 2 mL deionized water and heat at 100°C for 10 min to obtain a clear solution.

[0057] 2) After the solution obtained in step 1) is cooled to room temperature, 0.05 g of strontium nitrate is added, and then 4.6 g of silica sol and 5 mL of deionized water are added, and the mixture is stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0058] 3) The molecular sieve gel obtained in step 2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0059] 4) The liquid after the reaction obtained in step 3) is filtered, washed and dried to obtain the hydrophilic molecular sieve K-4.

[0060] 5) The hydrophilic molecular sieve K-4 obtained in step 4) was ion exchanged in a 0.05 mol / L silver nitrate solution for 1 h in the dark. The solution after the reaction was filtered, washed, and dried overnight to obtain the silver-modified molecular sieve AgK-0.05.

[0061] Example 3

[0062] The present embodiment provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0063] 1) Place 0.4 g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0064] 2) Add 30 mL of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm with the mass flow controller, and connect the helium gas for purging;

[0065] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0066] 4) Turn on the gas chromatograph, and pass the tail gas in step 3) into the gas chromatograph for real-time detection; through real-time detection and analysis by gas chromatography, water begins to elute through the adsorption bed of the silver-modified molecular sieve at 270 min / g.

[0067] A method for preparing a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate comprises the following steps:

[0068] 1) Add 0.7 g potassium hydroxide and 0.4 g aluminum hydroxide to 2 mL deionized water and heat at 100°C for 10 min to obtain a clear solution.

[0069] 2) After the solution obtained in step 1) is cooled to room temperature, 0.05 g of strontium nitrate is added, and then 4.6 g of silica sol and 5 mL of deionized water are added, and the mixture is stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0070] 3) The molecular sieve gel obtained in step 2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0071] 4) The liquid after the reaction obtained in step 3) is filtered, washed and dried to obtain the hydrophilic molecular sieve K-4.

[0072] 5) The hydrophilic molecular sieve K-4 obtained in step 4) was ion exchanged in a 0.01 mol / L silver nitrate solution for 1 h in the dark, and the solution after the reaction was filtered, washed, and dried overnight to obtain the silver-modified molecular sieve AgK-0.01.

[0073] Example 4

[0074] The present embodiment provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0075] 1) Place 1g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0076] 2) Place 100 mL of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm using the mass flow controller, and connect the helium gas for purging;

[0077] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0078] 4) turning on the gas chromatograph, and passing the tail gas described in step 3) into the gas chromatograph for real-time detection;

[0079] A method for preparing a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate comprises the following steps:

[0080] 1) Add 0.7 g potassium hydroxide and 0.4 g aluminum hydroxide to 2 mL deionized water and heat at 100°C for 10 min to obtain a clear solution.

[0081] 2) After the solution obtained in step 1) is cooled to room temperature, 0.05 g of strontium nitrate is added, and then 4.6 g of silica sol and 5 mL of deionized water are added, and the mixture is stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0082] 3) The molecular sieve gel obtained in step 2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0083] 4) filtering, washing and drying the liquid after the reaction obtained in step 3) to obtain a hydrophilic molecular sieve K-4;

[0084] 5) The hydrophilic molecular sieve K-4 obtained in step 4) was ion exchanged in a 0.01 mol / L silver nitrate solution for 1 h in the dark, and the solution after the reaction was filtered, washed, and dried overnight to obtain the silver-modified molecular sieve AgK-0.01.

[0085] Through real-time gas chromatography analysis, water began to elute through the adsorption bed at 330 min / g of the molecular sieve.

[0086] Comparative Example 1

[0087] The present embodiment provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0088] 1) Place 0.4 g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0089] 2) Add 30 ml of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm with the mass flow controller, and connect the helium gas for purging;

[0090] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0091] 4) Turn on the gas chromatograph, and pass the tail gas in step 3) into the gas chromatograph for real-time detection; through real-time detection and analysis by the gas chromatograph, water begins to elute through the adsorption bed at 280 min / g of the molecular sieve.

[0092] A method for preparing a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate comprises the following steps:

[0093] 1) Add 0.7 g potassium hydroxide and 0.2 g aluminum hydroxide to 2 mL deionized water and heat at 100°C for 10 min to obtain a clear solution.

[0094] 2) After the solution obtained in step 1) is cooled to room temperature, 0.05 g of strontium nitrate is added, and then 2.3 g of silica sol and 5 mL of deionized water are added, and the mixture is stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0095] 3) The molecular sieve gel obtained in step 2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0096] 4) The liquid after the reaction obtained in step 3) is filtered, washed and dried to obtain the hydrophilic molecular sieve K-2.

[0097] Comparative Example 2

[0098] This comparative example provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0099] 1) Place 0.4 g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0100] 2) Add 30 mL of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm with the mass flow controller, and connect the helium gas for purging;

[0101] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0102] 4) Turn on the gas chromatograph, and pass the tail gas in step 3) into the gas chromatograph for real-time detection; through real-time detection and analysis by the gas chromatograph, water begins to elute through the adsorption bed at 250 min / g of the molecular sieve.

[0103] A method for preparing a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate comprises the following steps:

[0104] 1) Add 0.7 g potassium hydroxide and 0.2 g aluminum hydroxide to 2 mL deionized water and heat at 100°C for 10 min to obtain a clear solution.

[0105] 2) After the solution obtained in step 1) is cooled to room temperature, 0.05 g of strontium nitrate is added, and then 4.6 g of silica sol and 5 mL of deionized water are added, and the mixture is stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0106] 3) The molecular sieve gel obtained in step 2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0107] 4) The liquid after the reaction obtained in step 3) is filtered, washed and dried to obtain the hydrophilic molecular sieve K-1.

[0108] Comparative Example 3

[0109] This comparative example provides a method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve. The method comprises the following steps in sequence:

[0110] 1) Place 0.4 g of molecular sieve into the adsorption column and fill both sides with quartz wool;

[0111] 2) Add 30 mL of deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3 sccm with the mass flow controller, and connect the helium gas for purging;

[0112] 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry dimethyl carbonate and methanol through the adsorption column in step 1);

[0113] 4) Turn on the gas chromatograph and pass the tail gas in step 3) into the gas chromatograph for real-time detection; 5) Through real-time detection and analysis by the gas chromatograph, water begins to elute through the adsorption bed at 170 min / g of the molecular sieve.

[0114] A method for preparing a hydrophilic molecular sieve for dehydrating industrial-grade dimethyl carbonate comprises the following steps:

[0115] 1) Add 0.7 g potassium hydroxide and 0.2 g aluminum hydroxide to 2 mL deionized water and heat at 100°C for 10 min to obtain a clear solution.

[0116] 2) After the solution obtained in step 1) is cooled to room temperature, 0.05 g of strontium nitrate is added, and then 6.9 g of silica sol and 5 mL of deionized water are added, and the mixture is stirred at room temperature for 60 min to obtain a molecular sieve gel.

[0117] 3) The molecular sieve gel obtained in step 2) was transferred into a reaction vessel for crystallization reaction at 140° C. for 24 h.

[0118] 4) The liquid after the reaction obtained in step 3) is filtered, washed and dried to obtain the hydrophilic molecular sieve K-8.

[0119] Through X-ray diffraction pattern ( Figure 1 ) It can be seen that the synthesized molecular sieve belongs to the KFI type molecular sieve; Figure 3 The device shown in the figure was subjected to a dynamic water penetration test. By comparing Examples 1 to 3, it can be seen that the hydrophilicity of the silver-modified molecular sieve is affected compared with that of the unmodified molecular sieve. Although the elution point of water passing through the adsorption column is increased in Comparative Examples 1 and 2 compared with Example 1, the diffusion coefficient of Example 1 is larger than that of Comparative Examples 1 and 2. The morphology and size of the modified molecular sieve ( Figure 2 ) had no significant change, and water was eluted through the adsorption column at 400 min / g, which was significantly enhanced compared to the elution at 250 min / g before modification.

Claims

1. A method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve, characterized in that: The steps are as follows: 1) Place the hydrophilic molecular sieve into the adsorption column and fill both sides with quartz wool; 2) Add deionized water into the bubbler, open the air valve, close the adsorption column valve, control the helium flow rate to 3-5 sccm with the mass flow controller, and connect the helium for purging; 3) After the helium gas in step 2) is stabilized, the air valve is closed, and the adsorption column valve is opened to allow the helium gas to carry the deionized water through the adsorption column in step 1); 4) Turn on the gas chromatograph and pass the tail gas described in step 3) into the gas chromatograph for real-time detection.

2. The method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 1, characterized in that: The ratio of the hydrophilic molecular sieve to deionized water is: 0.4-1g: 30-100mL.

3. The method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 1, characterized in that: The hydrophilic molecular sieve is synthesized by the following method: 1) Dispersing potassium hydroxide and aluminum hydroxide in a solvent, adding strontium nitrate and silica sol to mix to obtain a reaction solution, transferring the reaction solution into a reaction kettle, and reacting at 80 to 140° C. for 20 to 24 hours to obtain a product hydrophilic molecular sieve; 2) immersing the hydrophilic molecular sieve prepared in step 1) in a silver nitrate solution for ion exchange to obtain a silver-modified hydrophilic molecular sieve; The molar ratio of the aluminum hydroxide, silica sol, potassium hydroxide and strontium nitrate in step 1) is 0.25-0.6:1-3:0.66:0.

01.

4. The method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 2, characterized in that: The solvent in step 1) is deionized water.

5. The method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 2, characterized in that: The concentration of silver nitrate in step 2) is 0.02-0.4 mol / L.

6. The method for removing water from industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 2, characterized in that: The mass ratio of the hydrophilic molecular sieve to the silver nitrate solution in step 2) is 1:20-50.

7. The method for dewatering industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 2, characterized in that: The ion exchange time in step 2) is 40 to 80 minutes.

8. The method for dewatering industrial-grade dimethyl carbonate using a hydrophilic molecular sieve according to claim 2, characterized in that: The reactor is a stainless steel reactor lined with polytetrafluoroethylene.

Citation Information

Patent Citations

  • Integral molecular sieve preparation method

    CN106390925A

  • Method for preparing molecular sieve-type dehydrating agent of coal tar

    CN107937018A

  • Synthesis method of nano KFI molecular sieve

    CN112479225A

  • Cu-ZK-5 molecular sieve synthesized by organic template-free method as well as preparation method and application of Cu-ZK-5 molecular sieve

    CN118084009A

  • Double-component modified molecular sieve with improved hydrothermal stability and production method thereof

    US20120275994A1