Composite hygroscopic material and preparation method thereof, composite hygroscopic agent and preparation method and application thereof

The composite hygroscopic material linked by hydrogen bonds solves the problem of high energy consumption in the adsorption and desorption processes of existing hygroscopic materials, achieving low-temperature high-efficiency adsorption and low-energy desorption, and utilizing low-grade waste heat for regeneration, thereby improving the utilization efficiency of the hygroscopic material.

CN118904043AActive Publication Date: 2024-11-08UNIV OF SCI & TECH BEIJING
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410999833.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing moisture-absorbing materials present contradictions in the adsorption and desorption processes. Physically adsorbed materials require high-temperature desorption, while chemically adsorbed materials require high-energy regeneration and are prone to saturation, making it difficult to efficiently utilize low-grade waste heat.

Method used

The composite hygroscopic material that uses hydrogen bonds to adsorb water molecules adsorbs water molecules in a bound water state through the hydrogen bond dendritic connection between organic matter and substrate, avoiding aggregation and accumulation. During desorption, only the energy to break the hydrogen bonds is required, and desorption is carried out using low-temperature waste heat.

Benefits of technology

It achieves efficient adsorption of water molecules at low temperatures, low-energy desorption, and can utilize low-grade waste heat for regeneration, thus reducing material regeneration costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904043A_ABST
    Figure CN118904043A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hygroscopic materials, in particular to a composite hygroscopic material and a preparation method thereof, and a composite hygroscopic agent and a preparation method and application thereof. The composite moisture absorption material comprises a base material and an organic matter loaded on the base material, wherein the organic matter is an organic matter containing an amino group or a sulfonic acid group; the base material comprises a molecular sieve; the moisture absorption material is formed by compounding an organic material and an inorganic material and adsorbs water molecules to form bound water, so that the water molecules are effectively prevented from being condensed into liquid water in pore channels, the moisture absorption material can be desorbed at 70 DEG C, the adsorption depth is below-40 DEG C, and the adsorption capacity is above 300g / kg.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of hygroscopic materials, and in particular to a composite hygroscopic material and a preparation method thereof, a composite hygroscopic agent and a preparation method and application thereof. Background Art

[0002] Hygroscopic materials are materials that absorb water or moisture. They are widely used in many fields, such as in the construction industry to regulate indoor humidity, thereby preventing mold and corrosion; in medical devices to absorb blood or other body fluids; in food packaging to keep food fresh, etc.

[0003] The hygroscopic principles of existing hygroscopic materials include physical adsorption of water or chemical adsorption of water; physical adsorption is the use of pore action for adsorption, which has a contradiction between balancing the adsorption capacity and desorption capacity of a specific substance. For the dehumidification process, water molecules condense and accumulate in the pores, which will cause a higher pore adsorption potential, and thus the desorption temperature required for traditional physical adsorption materials during desorption is higher; chemical adsorption is the reaction of hygroscopic materials with water to form corresponding salts or salts containing crystal water. Although it has a higher adsorption performance, the desorption energy consumption required during desorption is higher. Chemical hygroscopic materials can usually only absorb a certain amount of water or moisture. Once they reach a saturated state, they need to be replaced or regenerated. Regeneration requires a chemical reaction to break the chemical bonds. The process of breaking the chemical bonds requires a very high reaction temperature, which increases the regeneration cost of the material. Summary of the invention

[0004] In order to solve the above problems, the present application proposes a hygroscopic material and preparation method, a composite hygroscopic agent and preparation method and application. The hygroscopic material uses hydrogen bonds to adsorb water molecules, and only the energy of "breaking bonds" of hydrogen bonds is required to achieve desorption dendritic connection during desorption. Therefore, the minimum desorption temperature of the hygroscopic material is 70°C.

[0005] This application is implemented through the following technical solutions:

[0006] One of the purposes of the present application is to provide a composite hygroscopic material, comprising a substrate and an organic substance loaded on the substrate;

[0007] Wherein, the organic matter is an organic matter containing an amino group or a sulfonic acid group;

[0008] The mass ratio of the organic matter to the substrate is 1:(0.2-20).

[0009] The composite hygroscopic material provided by the present application, the molecular sieve is the substrate, and the organic matter is the main material for absorbing water molecules. The organic matter is firmly connected to the substrate in a hydrogen bond dendrite, so that when the composite hygroscopic material adsorbs water molecules, the water molecules are adsorbed on the main chain and side chains of the organic matter in a bound water state, and the form of combined adsorption mainly includes the amino functional group and / or sulfonic acid functional group in the organic matter and the water molecules connected by hydrogen bonds or van der Waals forces, and the organic matter is staggered in the pores of the substrate, so that the bound water molecules cannot condense and accumulate in the composite hygroscopic material. The dehumidification depth of the composite hygroscopic material is -80℃~-40℃, and the desorption temperature is above 70℃. The saturated adsorption capacity of the composite hygroscopic material for water is 300g / kg~700g / kg.

[0010] In some possible implementations, the substrate includes one or more of mesoporous silica, nano-silica, mesoporous alumina, nano-alumina, MOFs, activated carbon, and resin.

[0011] The second object of the present application is to provide a method for preparing the composite hygroscopic material provided in the present application, comprising the following steps:

[0012] Drying the mixed slurry to obtain the composite hygroscopic material;

[0013] Wherein, the mixed slurry contains an organic solution and a substrate.

[0014] The preparation method of the composite hygroscopic material provided by the present application comprises the following steps: the organic matter and the substrate in the mixed slurry are fully mixed and then dried to remove the solvent in the mixed slurry to obtain the dried composite hygroscopic material.

[0015] In some possible implementations, the mass fraction of organic matter in the organic solution is 30% to 80%.

[0016] In some possible implementations, the mass ratio of the organic solution to the substrate is: (1-10):3.

[0017] In some possible implementations, the viscosity of the mixed slurry is 10 mPa·s to 1000 mPa·s.

[0018] In some possible implementations, the drying step includes at least two drying steps.

[0019] The third object of the present application is to provide a composite hygroscopic agent, the composite hygroscopic agent comprising a carrier and a composite hygroscopic material provided by an embodiment of the present application loaded on the carrier;

[0020] The loading capacity of the composite hygroscopic material is 20 kg / m 3~350kg / m 3 .

[0021] The composite hygroscopic agent provided by the present application, because it includes the composite hygroscopic material provided by the embodiment of the present application, has a dehumidification depth of -80°C to -40°C and a desorption temperature of above 70°C. The composite hygroscopic material is loaded on a carrier and can be directly formed for adsorption or used for filling bed adsorption, which provides convenience for engineering applications.

[0022] In some possible implementations, the carrier includes: one or more of glass fiber, cordierite, and honeycomb ceramics.

[0023] In some possible implementations, the particle size of the composite moisture absorbent is 50 nm to 200 nm.

[0024] The fourth object of the present application is to provide a method for preparing a composite moisture absorbent, comprising the following steps:

[0025] The mixed slurry and the carrier are subjected to loading treatment and then drying treatment to obtain the composite moisture absorbent;

[0026] The components of the mixed slurry include the composite hygroscopic material, solvent, binder and additive provided in the present application.

[0027] The preparation method of the composite desiccant provided in the present application comprises the steps of loading the mixed slurry and the carrier so that the composite desiccant material in the mixed slurry is uniformly loaded on the carrier; and drying to remove excess impurities such as moisture.

[0028] In some possible implementations, the mass ratio of the composite hygroscopic material, the solvent, the binder and the auxiliary agent is (1-4): (10-20): (3-7): 0.01.

[0029] In some possible implementations, the viscosity of the mixed slurry is 10 mPa·s to 400 mPa·s. The composite moisture absorbent prepared within this viscosity range has a high loading amount and is less likely to have pore blocking.

[0030] In some possible implementations, the solid-liquid ratio of the carrier to the mixed slurry is 10 g:(400 ml-1000 ml). Within this solid-liquid ratio range, the adsorbent loading can meet the requirements, which avoids the pore blocking phenomenon that is easy to occur due to a large amount of liquid.

[0031] The fifth object of the present application is to provide an application of the composite hygroscopic material provided by the present application or the composite hygroscopic agent provided by the present application in at least one field of lithium battery preparation, crude oil purification, fuel utilization, chemical synthesis, air water capture, flue gas dehydration, blast furnace dehumidification, warehousing and logistics, food processing, automobile aviation, building environment, electronic product processing, HVAC, and indoor dehumidification.

[0032] The application of the composite hygroscopic material or the composite hygroscopic agent provided in the present application can achieve room temperature adsorption under the dew point temperature requirement of -80°C to -40°C (i.e., dehumidification depth) and low temperature regeneration (i.e., desorption) of the composite hygroscopic material or the composite hygroscopic agent at a minimum of 70°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic diagram of the preparation method of the composite hygroscopic material of the embodiment of the present application;

[0034] Figure 2 This is a schematic diagram of the structure of the composite hygroscopic material after absorbing water according to an embodiment of the present application;

[0035] Figure 3 This is a schematic diagram of the structure of the composite moisture absorbent of the embodiment of the present application;

[0036] Figure 4 This is a schematic diagram of the preparation method of the composite moisture absorbent according to the embodiment of the present application;

[0037] Figure 5 The water vapor isothermal hygroscopic lines of the composite hygroscopic materials of Examples 1 to 5 of the present application, the composite hygroscopic agent of Example 6, and the hygroscopic materials of Comparative Examples 1 to 4;

[0038] Figure 6 Desorption curves of the composite hygroscopic materials of Examples 1 to 5 of the present application, the composite hygroscopic agent of Example 6, and the hygroscopic materials of Comparative Examples 1 to 4;

[0039] Figure 7 This is a schematic diagram of the condensation state of water when the hygroscopic material of the comparative example of the present application absorbs water;

[0040] Figure 8 This is a schematic diagram of the penetration adsorption curve of the composite desiccant of Example 6 of the present application. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present application clearer, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0042] On the contrary, the present application covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present application as defined by the claims. Further, in order to make the public have a better understanding of the present application, some specific details are described in detail in the detailed description of the present application below. Those skilled in the art can fully understand the present application without the description of these details.

[0043] The following examples serve to illustrate the present application. In the examples, unless otherwise indicated, parts are by weight, percentages are by weight, and temperatures are in degrees Celsius. The relationship between parts by weight and parts by volume is the same as the relationship between grams and cubic centimeters.

[0044] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0045] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0046] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0047] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0048] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0049] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0050] Hygroscopic materials are widely used in many fields. For example, in the preparation process of lithium batteries, if the moisture content is higher than 0.06kPa, it will cause the lithium salt to decompose, so the required dehumidification depth must be lower than -25°C. For another example, as a raw material for the alkylation reaction, the mixed carbon four needs to reduce the water vapor partial pressure in the environment from 0.075kPa to 0.0484kPa~0.0499kPa, that is, the required dehumidification depth must be lower than -28°C. Similar to this industry, there are requirements for the humidity of the environment. If molecular sieves, silica gel, MOFs, lithium chloride, alumina and other materials are used, the adsorption depth can reach below -30°C, but the desorption temperature during regeneration is high, which will cause more energy consumption and economic losses. For example, the desorption temperature of silica gel is between 90°C and 120°C, and the desorption temperature of molecular sieves is between 120°C and 150°C.

[0051] The adsorption process of materials such as molecular sieves and silica gel generally utilizes their microporous structure to adsorb and screen water molecules. During the adsorption process, water molecules form liquid free water and condense and accumulate. The desorption process utilizes the fact that when the temperature rises, the movement of molecules becomes more intense, and the chance of collision between molecules increases, making it easier for the originally adsorbed water molecules to be released from the pores; however, the adsorption potential problem cannot be avoided during the desorption process, and a higher desorption temperature and desorption time are required, resulting in more energy consumption.

[0052] In order to effectively take into account the adsorption and desorption problems of hygroscopic materials. The embodiments of the present application propose a composite hygroscopic material and a composite hygroscopic agent. The composite hygroscopic material uses an inorganic oxide as a substrate and combines organic matter containing amino or sulfonic acid functional groups to make the dehumidification depth of the composite hygroscopic material be -80°C to -40°C and the desorption temperature be above 70°C. The composite hygroscopic material is combined with a carrier to form a composite hygroscopic agent, which can not only increase the surface area of ​​the composite hygroscopic material, but also avoid the agglomeration of the hygroscopic material that occurs during the adsorption process of the composite hygroscopic material.

[0053] For the convenience of description, the following embodiments of the present application are described by taking composite hygroscopic materials and preparation methods, composite hygroscopic agents and preparation methods, and applications as examples.

[0054]

Composite hygroscopic material

[0055] One of the purposes of the embodiments of the present application is to provide a composite hygroscopic material, such as Figure 1 As shown, it includes a substrate and an organic matter loaded on the substrate;

[0056] Wherein, the organic matter is an organic matter containing an amino group or a sulfonic acid group;

[0057] The mass ratio of the organic matter to the substrate is 1:(0.2-20).

[0058] The composite hygroscopic material provided in the embodiment of the present application has a molecular sieve as a substrate and an organic substance as the main material for absorbing water molecules. The organic substance and the substrate are connected in a branched manner by hydrogen bonds, so that the substrate and the organic substance are firmly connected. When the composite hygroscopic material absorbs water molecules, the amino functional groups and / or sulfonic acid functional groups in the organic substance are hydrogen-bonded with the water molecules for adsorption, so that the water molecules will not condense and accumulate in the composite hygroscopic material. The dehumidification depth of the composite hygroscopic material is -80°C to -40°C, and the desorption temperature is above 70°C. The penetration adsorption capacity of the composite hygroscopic material is 50g / kg to 300g / kg, and the saturated adsorption capacity is 300g / kg to 700g / kg.

[0059] In the embodiment, the desorption temperature of the hygroscopic material is above 70°C. Since the composite hygroscopic material has a lower desorption temperature (minimum 70°C), industrial medium-temperature waste heat can be used for heating and desorption during desorption, and no heat source needs to be introduced for heating. For example, harmful flue gas needs to be separated and treated during boiler exhaust. The presence of water in this separation process will seriously affect the separation effect. Therefore, before the flue gas treatment process, a composite hygroscopic material needs to be used to absorb water. After that, the low-grade waste heat in the boiler flue gas can be used to desorb and regenerate the hygroscopic material after water absorption. In this way, there is no need to introduce an external heat source for heating and desorption, and the low-grade waste heat is effectively utilized. In addition to boiler flue gas, waste gas emitted by high-temperature furnaces in the steel, glass, ceramics and other industries also belongs to low-grade waste heat. While the hygroscopic material of the embodiment of the present application is used to effectively absorb water, the low-grade waste heat of these waste gases can also be effectively utilized.

[0060] In some embodiments, the substrate includes one or more of mesoporous silica, nano-silica, mesoporous alumina, nano-alumina, MOFs, activated carbon, and resin. In this case, these substrates have abundant pores, which can not only accommodate the organic matter, but also the hydroxyl groups on the surface of the substrate form stable hydrogen bonds with the organic matter, strengthen the combination of the organic matter and the substrate, and the special pore structure of the substrate makes the organic matter regularly confined in the substrate; when absorbing moisture, the substrate provides a high-concentration water molecule environment for the organic matter, promotes the adsorption and binding of the organic matter to water molecules to form bound water, and under the synergistic effect of the abundant pores of the substrate and the organic matter, the dehumidification depth of the hygroscopic material is improved.

[0061] In some embodiments, the particle size of mesoporous silica is 50nm to 200nm. In the exemplary embodiment, it can be a typical but non-restrictive particle size such as 50nm, 100nm, 150nm, 200nm, or a range between any two particle sizes. In this particle size range, mesoporous silica has a larger specific surface area and more pores, which helps to increase the amount of organic matter attached to mesoporous silica and its adsorption capacity for water molecules, and provides more moisture environment for organic matter to absorb water. The dispersibility and stability of mesoporous silica at this particle size are relatively high. In the subsequent molding process, mesoporous silica at this particle size is not easy to agglomerate, is easier to disperse in the solvent, and is easier to mold.

[0062] In some embodiments, the pore size of mesoporous silica is 2nm to 50nm. In the exemplary embodiment, it can be a typical but non-limiting pore size such as 2nm, 10nm, 20nm, 30nm, 40nm, 50nm, or a range between any two pore sizes. In this pore size range, high molecular organic matter can more easily enter the pores, and can effectively achieve a regular arrangement of organic matter in the pores, avoiding the problem of organic matter accumulation in the pores due to excessive pore size; secondly, in this pore size range, it is ensured that after the organic matter enters the pores, there is still space, which ensures the movement of water molecules in the pores and avoids adsorption kinetics problems.

[0063] In some embodiments, the pore volume of the mesoporous silica is 0.3 cm 3 / g~4cm 3 / g, in the example, it can be 0.3cm 3 / g, 1cm 3 / g, 2cm 3 / g, 3cm 3 / g, 4cm 3 / g and other typical but non-limiting pore volumes or the range between any two pore volumes. In this pore volume range, the substrate is fully and effectively loaded with organic matter, which improves the dehumidification capacity of the composite material; secondly, the pore volume also improves the transmission and release rate of water molecules in the pores.

[0064] Pore ​​volume unit: cm 3 / g refers to the total volume of pores contained in each gram of substrate.

[0065] In some embodiments, the specific surface area of ​​the mesoporous silica is 100 m 2 / g~500m 2 / g, in the example, it can be 100m 2 / g, 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g or any range between two specific surface areas. Within this specific surface area range, mesoporous silica has more binding sites, which directly increases the amount of organic matter attached and improves the moisture absorption capacity of the composite material.

[0066] In some embodiments, the particle size of nano-silicon dioxide is 7nm to 40nm. In the exemplary embodiment, it can be a typical but non-restrictive particle size such as 7nm, 10nm, 20nm, 30nm, 40nm, or a range between any two particle sizes. In this particle size range, nano-silicon dioxide has a larger specific surface area and more pores, which helps to increase the amount of organic matter attached to nano-silicon dioxide and the adsorption capacity of water molecules, and provides more moisture environment for the organic matter to absorb water. At this particle size, the dispersibility and stability of nano-silicon dioxide are relatively high. In the subsequent molding process, nano-silicon dioxide at this particle size is not easy to agglomerate, is easier to disperse in the solvent, and is easier to mold.

[0067] In some embodiments, the pore size of the nano-silicon dioxide is less than 2 nm. In the exemplary embodiment, the pore size may be 0.1 nm, 0.5 nm, 0.8 nm, 1 nm, 1.5 nm, 1.9 nm, etc., which are typical but non-limiting pore sizes, or a range between any two pore sizes. Within this pore size range, the specific surface area of ​​the material is increased, and the pore volume of the nano-silicon dioxide is increased, providing contact sites and space for the subsequent entry of organic matter.

[0068] In some embodiments, the specific surface area of ​​nano-silicon dioxide is 300 m 2 / g~600m 2 / g, in the example, it can be 300m 2 / g, 400m 2 / g、500m 2 / g、600m 2 / g or any range between two specific surface areas. In this specific surface area range, more contact sites can be provided for the recombination of organic matter and substrate.

[0069] In some embodiments, the pore volume of nano-silica is 0.8 cm 3 / g~5cm 3 / g, in the example, it can be 0.8cm 3 / g, 1cm 3 / g, 2cm 3 / g, 3cm 3 / g, 4cm 3 / g, 5cm 3 / g or any range between two pore volumes. In this pore volume range, more space can be provided for organic matter to enter the substrate.

[0070] In some embodiments, the particle size of mesoporous alumina is 50nm to 200nm. In the exemplary embodiment, it can be a typical but non-limiting particle size such as 50nm, 150nm, 200nm, or a range between any two particle sizes. In this particle size range, mesoporous alumina has a larger specific surface area and more pores, which helps to increase the amount of organic matter attached to the mesoporous alumina and the adsorption capacity of water molecules, and provides more moisture environment for the organic matter to absorb water. At this particle size, the dispersibility and stability of mesoporous alumina are relatively high. In the subsequent molding process, the mesoporous alumina at this particle size is not easy to agglomerate, is easier to disperse in the solvent, and is easier to mold.

[0071] In some embodiments, the pore size of mesoporous alumina is 2nm to 20nm. In the exemplary embodiment, it can be a typical but non-limiting pore size such as 2nm, 10nm, 15nm, 20nm, or a range between any two pore sizes. In this pore size range, high molecular organic matter can more easily enter the pores, and can effectively achieve a regular arrangement of organic matter in the pores, avoiding the problem of organic matter accumulation in the pores due to excessive pore size; secondly, in this pore size range, it is ensured that after the organic matter enters the pores, there is still space, which ensures the movement of water molecules in the pores and avoids adsorption kinetics problems.

[0072] In some embodiments, the specific surface area of ​​the mesoporous alumina is 100 m 2 / g~500m 2 / g, in the example, it can be 100m 2 / g, 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g or any range between two specific surface areas. Within this specific surface area range, the loading amount of organic matter on the substrate can be increased, thereby improving the dehumidification capacity of the composite material; secondly, the pore volume also increases the transmission and release rate of water molecules in the pores.

[0073] In some embodiments, the pore volume of the mesoporous alumina is 0.3 cm 3 / g~5cm 3 / g, in the example, it can be 0.3cm 3 / g, 1cm 3 / g, 2cm 3 / g, 3cm 3 / g, 4cm 3 / g, 5cm 3 / g or any range between two pore volumes. In this pore volume range, the loading amount of organic matter on the substrate can be increased, thereby improving the dehumidification capacity of the composite material; secondly, the pore volume also increases the transmission and release rate of water molecules in the pores.

[0074] In some embodiments, the particle size of nano-alumina is 5nm to 100nm. In the exemplary embodiment, it can be a typical but non-limiting particle size such as 5nm, 10nm, 40nm, 80nm, 100nm, or a range between any two particle sizes. In this particle size range, nano-alumina has a larger specific surface area and more pores, which helps to increase the amount of organic matter attached to nano-alumina and its adsorption capacity for water molecules, and provides more moisture environment for organic matter to absorb water. At this particle size, the dispersibility and stability of nano-alumina are relatively high. In the subsequent molding process, nano-alumina at this particle size is not easy to agglomerate, is easier to disperse in the solvent, and is easier to mold.

[0075] In some embodiments, the pore size of the nano-alumina is 0.3nm to 2nm. In the exemplary embodiment, it can be a typical but non-limiting pore size of 0.3nm, 0.6nm, 0.8nm, 1nm, 1.5nm, 2nm, etc., or a range between any two pore sizes. In this pore size range, the specific surface area of ​​the material is increased, and the pore volume of the nano-alumina is increased, providing contact sites and space for the subsequent entry of organic matter.

[0076] In some embodiments, the specific surface area of ​​nano-alumina is 300 m 2 / g~700m 2 / g, in the example, it can be 300m 2 / g, 400m 2 / g、500m 2 / g、600m 2 / g、700m 2 / g and other typical but non-limiting specific surface areas or the range between any two specific surface areas. In this specific surface area range, not only can more contact sites be provided for the composite of organic matter and substrate, but also the number of hydroxyl groups on the surface of mesoporous alumina is less than that of nano-silica, which will reduce the loading amount of organic matter and thus affect the hygroscopic effect of the composite hygroscopic material.

[0077] In some embodiments, the pore volume of nano-alumina is 0.6 cm 3 / g~5cm 3 / g. In this pore volume range, more space can be provided for organic matter to enter the substrate.

[0078] In some embodiments, the organic material comprises polyethylenediamine, monoethanolamine, diethanolamine, tetraethylenepentamine, polyethyleneimine, polyaminopropyltrimethoxysilane, polyethyleneimine-trimethoxysilane, polyamide, polytetraethylenepentamine, polydiethylenetriamine, polybenzenesulfonic acid, polymethanesulfonic acid, polyp-toluenesulfonic acid, polyethylenediaminesulfonyl halide derivatives, polyethylenediaminesulfonate derivatives, polymonoethanolaminesulfonyl halide derivatives, polymonoethanolaminesulfonate derivatives, polydiethanolaminesulfonyl halide derivatives, polydiethanolaminesulfonate derivatives, polyethyleneiminesulfonyl halide derivatives, polyethyleneiminesulfonate derivatives, polyaminopropyltrimethoxysilanesulfonyl halide derivatives. One or more of the group consisting of biological, polyaminopropyl trimethoxysilane sulfonate derivatives, polyethylene imine-trimethoxysilane sulfonyl halide derivatives, polyethylene imine-trimethoxysilane sulfonate derivatives, polyamide sulfonyl halide derivatives, polyamide sulfonate derivatives, tetraethylene pentamine sulfonyl halide derivatives, polytetraethylene pentamine sulfonate derivatives, polydiethylene triamine sulfonyl halide derivatives, polydiethylene triamine sulfonate derivatives, polybenzene sulfonyl halide derivatives, polybenzene sulfonate derivatives, polymethane sulfonyl halide derivatives, polymethane sulfonate derivatives, poly-p-toluene sulfonyl halide derivatives, and poly-p-toluene sulfonate derivatives. These organic substances have at least one amino functional group and / or sulfonic acid functional group, which can form strong hydrogen bonding with the substrate, so that the prepared composite has stronger stability; in the process of combining with water molecules, such organic substances can form strong chemical affinity with water molecules, and the water molecules are confined in the pores by the pore structure, thereby increasing the contact space between the organic substances and water molecules. The van der Waals force on the pore surface provides the initial driving force for the initial adsorption of water molecules, and the highly electronegative molecules on the surface of the organic substances provide traction force, and polar molecules are dipole-connected with each other, and some molecules are hydrogen-bonded. With the joint promotion of multiple connection modes and multiple interaction forces, the adsorption amount of water molecules is increased.

[0079] In some embodiments, the relative molecular weight of the organic compound is 100 to 25,000. In exemplary embodiments, the relative molecular weight may be 100, 600, 1,000, 1,800, 8,000, 10,000, 20,000, 25,000, or any range between any two relative molecular weights. Within this molecular weight range, the organic compound can effectively compound with the substrate without blocking the pores of the substrate.

[0080]

Preparation method of composite hygroscopic material

[0081] The second purpose of the embodiment of the present application is to provide a method for preparing the composite hygroscopic material provided in the embodiment of the present application, such as Figure 1 As shown, the following steps are included:

[0082] S1. The mixed slurry is dried to obtain a composite hygroscopic material;

[0083] The mixed slurry contains an organic solution and a substrate.

[0084] The preparation method of the composite hygroscopic material provided by the present application comprises the following steps: the organic matter and the substrate in the mixed slurry are fully mixed and then dried to remove the solvent in the mixed slurry to obtain the dried composite hygroscopic material.

[0085] In some embodiments, in the above step S1, the organic solution includes an organic substance and a solvent; the mass fraction of the organic substance is 30% to 80%, and in the exemplary embodiment, it can be 30%, 40%, 50%, 60%, 70%, 80% and other typical but non-limiting mass fractions or a range between any two mass fractions. In this case, the organic substance can be fully and effectively loaded on the substrate.

[0086] In some embodiments, the solvent includes one or more of water, methanol, ethanol, propanol, and n-butanol. In this case, these solvents are easy to remove by drying and will not introduce new impurities.

[0087] In some embodiments, in the above step S1, the step of preparing the organic solution includes:

[0088] S10. Obtain the masses of the organic matter and the solvent respectively.

[0089] S11. Perform a first mixing of the organic matter and the solvent to obtain an organic solution.

[0090] In some embodiments, in the above step S11, the first mixing includes mechanical mixing or ultrasonic mixing; the mixing conditions of mechanical mixing are: stirring for 30 min to 300 min at a temperature of 20° C. to 30° C. and a rotation speed of 200 rpm to 500 rpm; the mixing conditions of ultrasonic mixing are: ultrasonication for 10 min to 60 min at a temperature of 20° C. to 30° C., an ultrasonic frequency of 10 KHz to 60 KHz, and a power of 50 W to 500 W. Under this first mixing condition, the organic matter can be evenly dispersed in the solvent.

[0091] In some embodiments, mechanical mixing includes centrifugal stirring, turbine stirring, or magnetic stirring.

[0092] In some embodiments, in the above step S1, the substrate is pretreated and then subjected to a first mixing treatment with the organic solution; the pretreatment step includes: vacuum drying the substrate at a temperature of 50°C to 110°C for 1h to 5h. After the substrate is pretreated, water combined with the substrate can be further removed, and vacuum drying at an appropriate temperature can avoid collapse and damage of the substrate pores due to rapid water loss.

[0093] In some embodiments, the vacuum degree of the above pretreatment step during vacuum drying is less than 1 mmHg. In this case, vacuum drying helps to remove free water and bound water in the substrate and avoids the influence of material damage caused by relying solely on temperature drying.

[0094] In some embodiments, in the above step S1, the mass ratio of the organic solution to the substrate is: (1-10): 3. In this case, the organic solution can fully immerse the substrate, so that the organic matter can fully enter the internal pores of the substrate and be loaded.

[0095] In some embodiments, in the above step S1, the step of preparing the mixed slurry includes: adding the substrate to the organic solution, and then adding 20 to 80 parts by volume of the solvent, stirring until viscous, and obtaining the mixed slurry. In this case, the solvent can assist the organic matter to enter the pores of the substrate, and the solution is removed in the subsequent drying process, which can play a role in opening the pores, providing conditions for subsequent water molecules to enter the pores for adsorption, and will not affect the adsorption performance of the original organic matter.

[0096] In some embodiments, the solvent includes one or more of water, methanol, ethanol, propanol, and n-butanol. In this case, these solvents are easy to remove by drying and will not introduce new impurities.

[0097] In other embodiments, in the above step S1, the step of preparing the mixed slurry includes: mixing the substrate and the solvent to obtain a substrate mixed solution; mixing the substrate mixed solution with the organic solution and stirring until viscous to obtain a mixed slurry. In this case, the composite stability and loading capacity of the organic matter can be enhanced.

[0098] In other specific embodiments, the mass fraction of the substrate in the substrate mixed solution is 40% to 80%. In the exemplary examples, it can be 40%, 50%, 60%, 70%, 80% and other typical but non-limiting mass fractions or a range between any two mass fractions. Within this mass fraction range, the viscosity of the prepared mixed slurry meets the requirements.

[0099] In some embodiments, in the above step S1, the viscosity of the mixed slurry is 10mPa·s to 1000mPa·s. In the exemplary embodiment, it can be 10mPa·s, 100mPa·s, 400mPa·s, 800mPa·s, 1000mPa·s, etc., which are typical but non-limiting viscosities, or a range between any two viscosities. In this viscosity range, not only the organic matter is evenly dispersed in the substrate, but also the mixed slurry has strong dispersibility and stability.

[0100] In some embodiments, in the above step S1, the drying step includes at least two dryings. In this case, the first drying removes free water and alcohol solvents in the mixed slurry, and the second drying removes bound water and solvents inside the mixed slurry to obtain a completely dried and internally transparent composite hygroscopic material.

[0101] In some embodiments, in the above step S1, the drying step includes:

[0102] S12. Dry the mixed slurry at 40°C to 100°C for 2h to 24h to obtain a first dried product.

[0103] S13. The first dried product is vacuum dried at a temperature of 80°C to 110°C for 1h to 5h to obtain a composite hygroscopic material.

[0104] In the above drying treatment step, the mixed slurry is first dried at a temperature of 40°C to 100°C for 2h to 24h to remove free water and alcohol solvents in the mixed slurry; then vacuum drying is performed to remove bound water and solvent inside the first dried product; and finally a completely dried composite hygroscopic material is obtained.

[0105] In some embodiments, in the above step S12, the mixed slurry is dried using one of a drying oven, an oven, a hot plate, a heating mantle, a muffle furnace, and a tube furnace to obtain a first dried product. In this case, the drying equipment used is a common device to dry and remove free water and alcohol solution in the mixed slurry.

[0106] In some embodiments, in the above step S13, the vacuum degree when the first dried product is dried under vacuum is less than 1 mmHg. In this case, the bound water in the material can be completely removed without damaging the pore structure of the material.

[0107] In some embodiments, in the above step S13, the first dried product is vacuum dried using a box-type vacuum drying oven or a microwave vacuum drying oven. In this case, the box-type vacuum drying oven or the microwave vacuum drying oven provides a vacuum condition to the drying environment to remove bound water and alcohol in the first dried product.

[0108] In some other embodiments, in the above step S1, the drying step includes:

[0109] S14. Dry the mixed slurry by microwave at a power of 100w to 1000w for 30s to 30min to obtain a first dried product.

[0110] S15. The first dried product is vacuum dried at a temperature of 50°C to 110°C for 1h to 5h to obtain a composite hygroscopic material.

[0111] In some embodiments, in the above step S14, the mixed slurry is dried in a microwave drying oven to obtain a first dried product. In this case, the drying device used is a common device to dry and remove free water and alcohol in the mixed slurry.

[0112]

Compound moisture absorbent

[0113] The third object of the present application embodiment is to provide a composite moisture absorbent, such as Figure 3 As shown, the composite hygroscopic agent includes a carrier and a composite hygroscopic material provided by an embodiment of the present application loaded on the carrier;

[0114] The loading capacity of the composite hygroscopic material is 20kg / m 3 ~350kg / m 3 .

[0115] The composite hygroscopic agent provided in the embodiment of the present application comprises the composite hygroscopic material provided in the embodiment of the present application, and its dehumidification depth is -80°C to -40°C, and the desorption temperature is above 70°C. The composite hygroscopic material is loaded on a carrier, and can be directly formed for adsorption, or used for filling bed adsorption, which provides convenience for engineering applications.

[0116] In some embodiments, the carrier includes: one or more of glass fiber, cordierite, and honeycomb ceramics. These carriers contain abundant pores and have a large specific surface area, and can accommodate enough composite hygroscopic materials, that is, increase the loading amount of the composite hygroscopic materials in the carrier, thereby improving the hygroscopic capacity of the composite hygroscopic materials.

[0117] In some embodiments, the particle size of the composite moisture absorbent is 50 nm to 200 nm. In the exemplary embodiment, it can be a typical but non-limiting particle size such as 50 nm, 150 nm, 200 nm, or a range between any two particle sizes. Within this particle size range, the dispersibility and stability of the slurry can be improved, the strength of the carrier can be enhanced, and the powder loss rate can be reduced.

[0118] [Preparation method of composite moisture absorbent]

[0119] The fourth object of the present application embodiment is to provide a method for preparing a composite moisture absorbent, such as Figure 4 As shown, the following steps are included:

[0120] X1. The mixed slurry and the carrier are loaded and dried to obtain a composite moisture absorbent;

[0121] The components of the mixed slurry include the composite hygroscopic material, solvent, binder and additive provided in the embodiments of the present application.

[0122] The preparation method of the composite desiccant provided in the embodiment of the present application is to load the mixed slurry and the carrier so that the composite desiccant material in the mixed slurry is evenly loaded on the carrier; and drying can remove excess impurities such as moisture.

[0123] In some embodiments, in the above step X1, the mass ratio of the composite hygroscopic material, the solvent, the binder and the auxiliary agent is (1-4): (10-20): (3-7): 0.01, and can be, for example, a typical but non-limiting mass ratio such as 2:12:5:0.01 or a range between any two mass ratios. Within this mass ratio range, the composite hygroscopic material, the solvent, the binder and the auxiliary agent are mixed to form a mixed slurry with a viscosity of 10mPa·s to 400mPa·s. The composite hygroscopic material prepared within this mass ratio range has a high loading capacity, a high loading strength, a low powder loss rate after loading, and a good comprehensive evaluation of loading performance.

[0124] In some embodiments, in the above step X1, the solvent is one or more of water, methanol, ethanol, propanol, and n-butanol. In this case, the solvent adjusts the viscosity of the mixed slurry so that the viscosity of the mixed slurry meets the requirements.

[0125] In some embodiments, in the above step X1, the binder includes one or more of silica sol, polyethylene, polypropylene, acrylic acid, acrylamide, and 2-acrylamide-2-methylpropanesulfonic acid. These binders can enhance the bonding between different materials and enhance the bonding between the original powder and the carrier. The binder can improve the overall mechanical strength and stability of the material after loading.

[0126] In some embodiments, the auxiliary agent includes at least one of a dispersant and a defoaming agent.

[0127] In some embodiments, the dispersant includes one or more of acrylic acid copolymer and polyvinyl alcohol. These dispersants are mainly used to adjust the interaction between molecules to avoid agglomeration and sedimentation caused by mutual attraction between molecules.

[0128] In some embodiments, in the above step X1, the step of preparing the mixed slurry includes: mixing and stirring the raw materials including the composite hygroscopic material, the solvent, the binder and the auxiliary agent at a temperature of 20°C to 30°C and a rotation speed of 200rpm to 500rpm for 5h to 24h to obtain a mixed slurry. In this case, the composite hygroscopic material in the mixed slurry obtained after mixing is mixed uniformly and the viscosity of the slurry is 10mPa·s to 400mPa·s.

[0129] In some embodiments, in the above step X1, the viscosity of the mixed slurry is 100mPa·s to 400mPa·s, and can be, for example, 10mPa·s, 100mPa·s, 200mPa·s, 300mPa·s, 400mPa·s, or any other typical but non-limiting viscosity or a range between any two viscosities. The composite desiccant prepared within this viscosity range has a high loading capacity and is not prone to pore blocking.

[0130] In some embodiments, in the above step X1, the carrier is calcined and then mixed with the mixed slurry for loading treatment. In some specific embodiments, the calcination step includes: calcining at a temperature of 200° C. to 600° C. for 2 h to 4 h. Under this calcination condition, impurities such as binders and crosslinking agents in the carrier can be fully removed.

[0131] In some embodiments, the carrier is calcined using one of a drying oven, an oven, a hot plate, a heating mantle, a muffle furnace, and a tube furnace. These calcination equipments are commonly used devices and can meet the requirements of carrier calcination.

[0132] In some embodiments, in the above step X1, the solid-liquid ratio of the carrier and the mixed slurry is 10g:(400ml-1000ml), and in exemplary examples, it can be 10g:400ml, 10g:500ml, 10g:600ml, 10g:700ml, 10g:800ml, 10g:900ml, 10g:1000ml, etc., typical but non-limiting solid-liquid ratios or ranges between any two solid-liquid ratios. Within this solid-liquid ratio range, the adsorbent loading amount can meet the requirements, which avoids the pore blocking phenomenon that is easy to occur due to a large amount of liquid.

[0133] In some embodiments, in the above step X1, the loading treatment includes the steps of: placing the carrier in the mixed slurry and immersing it to obtain a wet composite hygroscopic agent. In some embodiments, the immersion time is 5 minutes to 30 minutes, and can be, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, etc., which are typical but non-limiting times or a range between any two times. Within this immersion time range, the composite hygroscopic material can be fully loaded, avoiding problems such as decreased solution dispersibility, decreased wettability, and accumulation inside the pores due to long-term standing.

[0134] In some embodiments, the number of dipping is 1 to 3 times.

[0135] In some embodiments, in the above step X1, after the mixed slurry and the carrier are loaded, a static treatment is also performed before drying, including the steps of taking out the composite moisture absorbent obtained after impregnation from the mixed slurry and hanging it for static treatment. In this case, the static treatment can avoid uneven distribution of the moisture absorbent, which may cause the solution to solidify and block the inside of the pores after subsequent drying.

[0136] In some embodiments, the static treatment time is 2 hours to 10 hours, and can be, for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, or any range between two times. Within this static treatment time range, the pores can be fully dredged, the uniformity of the distribution of the moisture absorbent can be enhanced, and the subsequent drying and pore blocking phenomenon can be avoided.

[0137] In some embodiments, in the above step X1, the drying step includes: vacuum drying the impregnated composite moisture absorbent at a temperature of 50° C. to 110° C. for 5 to 10 hours to obtain a dried composite moisture absorbent. Under this vacuum drying condition, the water content of the dried composite moisture absorbent is 1 mg / g to 10 mg / g.

[0138] In some embodiments, the composite moisture absorbent after impregnation is dried using a box vacuum drying oven or a microwave vacuum drying oven, and the vacuum degree is less than 1 mmHg. In this case, the free and bound water in the composite moisture absorbent can be removed using a vacuum degree less than 1 mmHg.

[0139] In other embodiments, in the above step X1, the drying step includes: placing the impregnated composite desiccant in a tube furnace or a muffle furnace, and then introducing an inert gas at a flow rate of 200 ml / min to 5000 ml / min to dry at 50° C. to 110° C. for 5 h to 10 h. In this case, the impregnated composite desiccant is dried under an inert atmosphere to remove free water and bound water in the impregnated composite desiccant.

[0140] In some embodiments, the inert gas is one or more of nitrogen, neon, and argon.

[0141]

application

[0142] The fifth purpose of the embodiments of the present application is to provide applications of the composite hygroscopic material provided by the embodiments of the present application or the composite hygroscopic agent provided by the embodiments of the present application in the fields of lithium battery preparation, crude oil purification, fuel utilization, and chemical synthesis.

[0143] The composite hygroscopic material or composite hygroscopic agent provided in the embodiments of the present application is used in the fields of lithium battery preparation, crude oil purification, fuel utilization, and chemical synthesis. The composite hygroscopic material or composite hygroscopic agent can achieve room temperature adsorption under the dew point temperature requirement of -80°C to -40°C (i.e., dehumidification depth) and low-temperature regeneration (i.e., desorption) of the composite hygroscopic material or composite hygroscopic agent at a minimum of 70°C.

[0144] The following describes the invention in conjunction with specific embodiments.

[0145] Example 1

[0146] This embodiment provides a composite hygroscopic material, including mesoporous alumina and polyethyleneimine;

[0147] The mass fraction of mesoporous alumina is 38.5%, and the mass fraction of polyethyleneimine is 61.5%.

[0148] The particle size of mesoporous alumina is 80nm, the pore size is 11nm, and the specific surface area is 375m 2 / g, pore volume is 1.5cm 3 / g.

[0149] The relative molecular weight of polyethyleneimine is 1800.

[0150] This embodiment also provides a method for preparing a composite hygroscopic material, comprising the steps of:

[0151] (1) Preparation of organic solution: 40 g of polyethyleneimine was dissolved in 50 ml of anhydrous methanol, and stirred for 60 min at room temperature (25° C.) and rotation speed (300 rpm) using a magnetic stirrer to obtain a polyethyleneimine solution.

[0152] (2) Dry mesoporous AL2O3 at a vacuum of less than 1 mmHg for 2 h.

[0153] (3) The polyethyleneimine solution, 25 g of mesoporous AL2O3 and 20 ml of anhydrous methanol were mixed and stirred with a magnetic stirrer at a temperature of 25°C and a rotation speed of 300 rpm for 12 h to obtain a mixed slurry with a viscosity of 153 mPa·s.

[0154] (4) The mixed slurry was placed in a muffle furnace, kept at a constant temperature of 50° C. for 5 h, and then placed in a box-type vacuum drying oven, and dried at a temperature of 80° C. for 2 h at a vacuum degree of less than 1 mmHg to obtain a composite hygroscopic material.

[0155] Example 2

[0156] This embodiment provides a composite hygroscopic material, including mesoporous silica and polyethyleneimine;

[0157] The mass fraction of mesoporous silica is 38.5%, and the mass fraction of polyethyleneimine is 61.5%.

[0158] The particle size of mesoporous silica is 70, the pore size is 5nm, and the specific surface area is 412m 2 / g, pore volume is 1.3cm 3 / g.

[0159] The relative molecular weight of polyethyleneimine is 1800.

[0160] The present application example also proposes a method for preparing a composite hygroscopic material, the steps of which are basically the same as those of Example 1, except that the substrate is mesoporous silica.

[0161] Example 3

[0162] This embodiment provides a composite hygroscopic material, including mesoporous alumina and polyphenylsulfonic acid;

[0163] The mass fraction of the mesoporous alumina is 38.5%, and the mass fraction of the polybenzene sulfonic acid is 61.5%.

[0164] The particle size of mesoporous alumina is 80nm, the pore size is 11nm, and the specific surface area is 375m 2 / g, pore volume is 1.5cm 3 / g.

[0165] The relative molecular weight of polybenzenesulfonic acid is 8000.

[0166] The present application example also proposes a method for preparing a composite hygroscopic material, and the steps are basically the same as those in Example 1, except that the organic matter is polyphenylsulfonic acid, and the relative molecular weight is 8000.

[0167] Example 4

[0168] This embodiment provides a composite hygroscopic material, including mesoporous alumina and tetraethylenepentamine;

[0169] The mass fraction of the mesoporous alumina is 38.5%, and the mass fraction of the tetraethylenepentamine is 61.5%.

[0170] The particle size of mesoporous alumina is 80nm, the pore size is 11nm, and the specific surface area is 375m 2 / g, pore volume is 1.5cm 3 / g.

[0171] The relative molecular weight of tetraethylenepentamine is 189.3.

[0172] The present application example also proposes a method for preparing a composite hygroscopic material, the steps of which are basically the same as those of Example 1, except that the organic substance is tetraethylenepentamine, and the relative molecular weight is 189.3.

[0173] Example 5

[0174] This embodiment provides a composite hygroscopic material and a preparation method thereof. The material and the preparation method thereof are substantially the same as those in Embodiment 1, except that:

[0175] In the preparation method, the mixed slurry is not dried in a muffle furnace, that is, the content of step (4) is: placing the mixed slurry in a box-type vacuum drying oven, and drying it at a constant temperature of 80° C. for 2 hours under a vacuum degree of less than 1 mmHg to obtain a composite hygroscopic material.

[0176] Example 6

[0177] This embodiment provides a composite moisture absorbent, including glass fiber and the composite moisture absorbent material of embodiment 1. The loading amount of the composite moisture absorbent material on the glass fiber is 158 kg / m 3 .

[0178] This embodiment also provides a method for preparing a composite moisture absorbent, comprising the following steps:

[0179] 1) A composite hygroscopic material was prepared according to the preparation method of the composite hygroscopic material in Example 1.

[0180] 2) 60 g of the composite hygroscopic material, 360 g of water, 150 g of silica sol and 0.3 g of polyvinyl alcohol were obtained, and mechanically stirred at 25° C. and 300 rpm for 10 h to obtain a mixed slurry with a viscosity of 183 mPa·s.

[0181] 3) calcining the glass fiber at 550° C. for 2 h to obtain pretreated glass fiber.

[0182] 4) The pretreated glass fiber is mixed with the mixed slurry and coated for 10 minutes, and then the wet material is taken out and allowed to stand for 5 hours to obtain an impregnated composite moisture absorbent.

[0183] 5) Drying the impregnated composite desiccant at a vacuum degree of less than 1 mmHg and a temperature of 50° C. to 110° C. for 8 hours to obtain a composite desiccant.

[0184] Comparative Example 1

[0185] This comparative example provides 65 g of mesoporous AL2O3 as a hygroscopic material.

[0186] Comparative Example 2

[0187] This comparative example provides 65 g of mesoporous silica gel as a hygroscopic material.

[0188] Comparative Example 3

[0189] This comparative example provides 65 g of molecular sieve as a hygroscopic material.

[0190] Comparative Example 4

[0191] This comparative example provides 65 g of activated carbon as a hygroscopic material.

[0192] In order to verify the progress of the embodiments of the present application, the composite hygroscopic materials and composite hygroscopic agents provided in the above embodiments 1 to 6 and the hygroscopic materials provided in comparative examples 1 to 4 were subjected to penetration adsorption, saturated adsorption and desorption regeneration experiments, and the experimental steps included:

[0193] The steps for determining the penetration adsorption amount and saturated adsorption amount are as follows: the same mass of experimental materials are loaded into the penetration adsorption column. The penetration adsorption column and the bypass are connected in parallel. Humidity probes are installed in front and behind the two respectively, for a total of four probes. The corresponding humidity conditions are measured. The moisture is taken out by N2 through the steam generator and enters the penetration adsorption table and the bypass. The penetration adsorption table is used for adsorption, and the bypass is used as a comparison. The nitrogen flow rate is 200ml / min. The humidity changes of the humidity probe are recorded, and the penetration adsorption amount and saturated adsorption amount are calculated. The dehumidification depth is calculated based on the humidity that can be achieved after the adsorption.

[0194] Desorption regeneration experiment: Weigh 0.2 mg of the sample after adsorption of water vapor, put it into a hot weight crucible, set the temperature from 0℃ to 120℃, and the heating rate is 2℃ / min. The temperature at which the weight reaches a constant is the desorption regeneration temperature of the sample.

[0195] The penetration adsorption amount, saturated adsorption amount and material agglomeration of the composite hygroscopic materials, composite hygroscopic agents and hygroscopic materials provided in Examples 1 to 6 and Comparative Examples 1 to 4 obtained from the above experiments are shown in Table 1 below; the water vapor isothermal hygroscopic lines of the hygroscopic materials of Examples 1 to 5, the composite hygroscopic agents of Example 6 and the hygroscopic materials of Comparative Examples 1 to 4 are shown in Table 1 below. Figure 5 As shown ( Figure 5 The horizontal axis is P / P0, P represents the current pressure of the environment, P0 represents the atmospheric pressure, and P / P0 is the relative pressure). The desorption curve is shown in Figure 6 As shown; Figure 7 A schematic diagram of the condensed state of water in the pores when the hygroscopic material provided in Comparative Examples 1 to 4 absorbs water; Figure 8 This is the adsorption penetration curve of the composite desiccant of Example 6.

[0196] Table 1

[0197]

[0198] From Table 1 above and Figures 5 to 8 It can be seen that:

[0199] ① Compared with a single inorganic hygroscopic material or an organic hygroscopic material, the composite hygroscopic material of the embodiment of the present application has a low dehumidification depth and can capture moisture with a lower water content in the environment.

[0200] ② Compared with Example 5, since Example 5 is directly vacuum dried without muffle furnace drying, the adsorption penetration and saturated adsorption capacity of the obtained composite hygroscopic material are 188.74 / kg and 401.56g / kg, respectively, which are significantly lower than the composite hygroscopic material of Example 1. This is because the spatial structure collapses due to direct primary drying without secondary drying, which reduces the content of organic matter entering the substrate and affects the adsorption effect.

[0201] ③ In Example 6, glass fiber was added as a carrier of the composite hygroscopic material, and no particle agglomeration phenomenon was found in the experiment.

[0202] ④ The composite hygroscopic materials and composite hygroscopic agents of Examples 1 to 6 of the present application can achieve room temperature adsorption under the dew point temperature requirement of -80°C to -40°C and low temperature regeneration at around 70°C.

[0203] ⑤ By the attached Figure 8 It can be seen that the moisture absorption depth of the composite desiccant of the embodiment of the present application can reach -70°C.

[0204] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A composite hygroscopic material, characterized in that: It includes a substrate and an organic matter supported on the substrate; Wherein, the organic matter is an organic matter containing an amino group or a sulfonic acid group; The mass ratio of the organic matter to the substrate is 1:0.2-20.

2. The composite hygroscopic material according to claim 1, characterized in that: The substrate includes one or more of mesoporous silica, nano-silica, mesoporous alumina, nano-alumina, MOFs, activated carbon and resin.

3. A method for preparing the composite hygroscopic material according to claim 1 or 2, characterized in that: The steps include: Drying the mixed slurry to obtain the composite hygroscopic material; Wherein, the mixed slurry contains an organic solution and a substrate.

4. The method for preparing the composite hygroscopic material according to claim 3, characterized in that: The mass fraction of organic matter in the organic solution is 20% to 80%; And / or, the mass ratio of the organic solution to the substrate is 1 to 10:3; And / or, the viscosity of the mixed slurry is 10 mPa·s to 1000 mPa·s.

5. The method for preparing the composite hygroscopic material according to claim 3 or 4, characterized in that: The drying step includes at least two drying steps.

6. A composite moisture absorbent, characterized in that: The composite hygroscopic agent comprises a carrier and a composite hygroscopic material prepared by the preparation method according to any one of claims 3 to 5 loaded on the carrier; The loading capacity of the composite hygroscopic material is 20 kg / m 3 ~350kg / m 3 .

7. The composite moisture absorbent according to claim 6, characterized in that The carrier includes: one or more of glass fiber, cordierite, and honeycomb ceramics; And / or, the particle size of the composite moisture absorbent is 50nm to 200nm.

8. A method for preparing the composite moisture absorbent according to claim 6 or 7, characterized in that: The steps include: The mixed slurry and the carrier are subjected to loading treatment and then drying treatment to obtain the composite moisture absorbent; The components of the mixed slurry include the composite hygroscopic material, a solvent, a binder and an additive.

9. The method for preparing the composite moisture absorbent according to claim 8, characterized in that: The mass ratio of the composite hygroscopic material, the solvent, the binder and the auxiliary agent is 1-4:10-20:3-7:0.01; And / or, the viscosity of the mixed slurry is 10mPa·s to 400mPa·s; And / or, the solid-liquid ratio of the carrier to the mixed slurry is 10g:400ml-1000ml.

10. An application of a composite hygroscopic material prepared by the preparation method according to any one of claims 3 to 5 or a composite hygroscopic agent prepared by the preparation method according to any one of claims 8 to 9 in at least one of the fields of lithium battery preparation, crude oil purification, fuel utilization, chemical synthesis, air water capture, flue gas dehydration, blast furnace dehumidification, warehousing and logistics, food processing, automobile aviation, building environment, electronic product processing, HVAC, and indoor dehumidification.

Citation Information

Patent Citations

  • Stable efficient composite water absorbing material and preparation method thereof

    CN104353433A

  • Forming process for compound water absorbing material

    CN105214615A

  • Porous ceramic based supported adsorbent and method for preparing same

    CN106237996A

  • Low-temperature regeneration dehumidification material of bacterial cellulose compound moisture absorbent

    CN107262048A

  • Superhydrophobic efficient air filtering material and preparation method thereof