Method for mineralizing CO2 in gas

By establishing a functional relationship between mineralized raw materials and gas performance parameters, and determining the surface renewal frequency, the low efficiency and safety issues of CO2 capture and storage in existing technologies have been resolved. This has enabled efficient mineralization of CO2 in the air, improving the utilization rate and absorption rate of mineralized raw materials.

CN118904066APending Publication Date: 2024-11-08YUANCHU TECH (BEIJING) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411195542.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing technologies, direct air capture of CO2 has problems such as amine volatilization, large gas phase loss, and high capture cost. Furthermore, geological CO2 sequestration is difficult to monitor and carries the risk of geological structural damage, resulting in low utilization rate of industrial solid waste mineralization raw materials.

Method used

By using mineralized raw materials to directly mineralize CO2 in the gas into a stable carbonate structure, and by establishing a functional relationship between the mineralized raw materials and the gas performance parameters, the surface renewal frequency can be determined, thereby improving the absorption rate and utilization rate of CO2 by the mineralized raw materials.

Benefits of technology

It achieves efficient mineralization of CO2 in the air, improves the utilization rate of CO2-fixable components in mineralized raw materials, with an absorption rate of over 20 g/m2/h and a utilization rate of over 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904066A_ABST
    Figure CN118904066A_ABST
Patent Text Reader

Abstract

The invention provides a method for mineralizing CO2 in gas, which comprises the following steps: mineralizing CO2 in gas by using a mineralizing raw material, and carrying out surface updating on the mineralizing raw material according to a preset updating frequency in the mineralizing process; the updating frequency is determined according to a function relationship between the physical performance parameters of the mineralization raw material and the physical performance parameters of the gas. According to the method, the function relationship among the performance parameters of the mineralization raw material, the performance parameters of the to-be-mineralized gas and the surface updating frequency of the mineralization raw material is established, and the surface updating is performed on the mineralization raw material according to the calculated frequency, so that the CO2 absorption rate of the mineralization raw material is increased, and the utilization rate of fixable CO2 components in the mineralization raw material is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of CO2 treatment, and in particular to a method for mineralizing CO2 in gas. Background Art

[0002] In order to reduce CO2 in the atmosphere, the mainstream method of direct air capture technology (DAC) is to use solution absorption and solid adsorption. The chemical absorption process based on ethanolamine organic amine solution has been widely used in the field of flue gas capture, but the high gas processing volume and low liquid-gas ratio of direct air capture make the organic amine absorption technology have problems such as large volatilization of amine liquid, large gas phase loss, and significantly increased capture cost. Solid adsorption technology can effectively solve the problems of amine volatilization and water loss. Solid adsorbents mainly include alkali / alkaline earth metal-based adsorbents, metal organic framework adsorbents, loaded amine-based adsorbents, variable humidity adsorbents, etc., but there are still problems such as high energy consumption and high cost. Moreover, DAC technology only completes the capture of CO2 in the air. If we want to achieve the stable storage of CO2, that is, to achieve the goal of "carbon neutrality", the current practice is to transport the captured carbon dioxide and then inject it into a specific geological structure for storage. However, such operations are difficult to monitor, the groundwater under the geological layer is at risk of being contaminated, and the damage to the geological structure is at risk of causing seismic activity and secondary leakage of high-concentration CO2.

[0003] Direct Air Mineralization (DAM) is a process whereby CO2 in the air is directly mineralized into a stable carbonate structure using mineralized raw materials containing calcium, magnesium, etc., without the need for capture and concentration of CO2 in the air. For example, the prior art discloses that industrial solid waste can be used to mineralize CO2 in the air, etc. However, in the currently disclosed methods, the utilization rate of raw materials such as industrial solid waste or alkali metal minerals is low. Summary of the invention

[0004] In view of this, the present invention provides a method for mineralizing CO2 in gas. The method provided by the present invention directly uses mineralized raw materials to directly mineralize the CO2 in the gas into a stable carbonate structure, and can improve the utilization rate of the fixable CO2 component in the mineralized raw materials.

[0005] The present application provides a method for mineralizing CO2 in gas, comprising the following steps:

[0006] The CO2 in the gas is mineralized by using a mineralized raw material, and the surface of the mineralized raw material is updated according to a predetermined update frequency during the mineralization process;

[0007] The updating frequency is determined according to the functional relationship between the physical property parameters of the mineralized raw material and the physical property parameters of the gas;

[0008] The physical property parameters of the mineralized raw material include the moisture content of the mineralized raw material , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials and at least one of the particle size d of the mineralized raw material;

[0009] The physical properties of the gas include the partial pressure of CO2 in the gas and the absolute humidity of the gas At least one of .

[0010] The applicant found in the study that the physical properties of the mineralized raw materials, including the moisture content of the mineralized raw materials , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials and the particle size d of the mineralized raw materials, as well as the physical properties of the gas to be mineralized, including the partial pressure of CO2 in the gas and the absolute humidity of the gas etc. will affect the absorption rate of CO2 by the mineralized raw materials, and further affect the utilization rate of the fixable CO2 components in the mineralized raw materials. Based on this, the applicant establishes a functional relationship between the above-mentioned performance parameters and the surface renewal frequency of the mineralized raw materials, and renews the surface of the mineralized raw materials according to the calculated frequency, thereby increasing the absorption rate of CO2 by the mineralized raw materials and improving the utilization rate of the fixable CO2 components in the mineralized raw materials.

[0011] This application adopts direct air mineralization to mineralize CO2 in gas, specifically, the mineralized raw material is contacted with the gas containing CO2, Ca, Mg, etc. in the mineralized raw material react with CO2 to form stable carbonate, so as to achieve the absorption and stable fixation of CO2. A typical reaction process is as follows:

[0012] 2Ca(Mg)X n (OH) m +2CO2= 2Ca(Mg)CO3+ X 2n O (m+4) + m H2O;

[0013] Wherein, X is other elements in mineralized raw materials such as silicon, iron, aluminum, etc.

[0014] Based on this, the mineralized raw materials described in the present application are magnesium-calcium mineralized raw materials, including but not limited to industrial solid wastes such as carbide slag, steel slag, red mud, concrete, or natural minerals such as serpentine, forsterite, basalt, volcanic ash, and wollastonite. In some specific implementations, the mineralizable CO2 component in the mineralized raw materials is mainly alkaline earth metal compounds such as magnesium hydroxide, calcium hydroxide, magnesium oxide, or calcium oxide. The content of the mineralizable CO2 component is not less than 5% in terms of calcium hydroxide, preferably 10wt%~95wt%, more preferably 20wt%~90wt%, and most preferably 30wt%~85wt%. In some specific implementations, the dry weight of the mineralized raw materials is 10 kg / m 2 ~50kg / m 2 , preferably 15 kg / m 2 ~45kg / m 2 , more preferably 20kg / m 2 ~40kg / m 2 In some specific implementations, the water content of the mineralized raw material is 2wt%~40wt%, preferably 5wt%~35wt%. In some specific implementations, the particle size of the mineralized raw material is 20 mesh~2000 mesh, preferably 50 mesh~1000 mesh, and more preferably 80 mesh~500 mesh.

[0015] The method provided by the present invention can mineralize CO2 in the air, and can also mineralize waste gas, including industrial waste gas, such as CO2 in flue gas from thermal power plants, cement plants, steel plants, and chemical plants. Based on this, the gas described in the present application, i.e., the gas to be mineralized, can be air or waste gas containing CO2. In some specific implementations, the water content of the gas is 2 g / kg dry gas to 40 g / kg dry gas, preferably 5 g / kg dry gas to 35 g / kg dry gas.

[0016] The present application has no special restrictions on the specific method of mineralizing CO2 in gas by using mineralized raw materials, and the mineralized raw materials can be directly contacted with gas. In some specific implementations, in order to improve the mineralization efficiency, gas can be introduced under the condition that the mineralized raw materials move. The present application has no special restrictions on the method of movement of the mineralized raw materials, for example, the mineralized raw materials can be loaded on a carrier, such as a transmission belt, etc., and the movement of the mineralized raw materials is realized by the reciprocating motion of the carrier. In some specific implementations, the movement of the mineralized raw materials is translation, and the moving speed of the mineralized raw materials is preferably 0.05m / s~1m / s, preferably 0.1m / s~0.8m / s. While the mineralized raw materials are moving, gas is introduced to contact the mineralized raw materials, for example, the gas is introduced at a certain angle to the mineralized raw materials, such as 90°. In some specific implementations, the flow rate of the gas is 0.20m / s~4.00m / s, preferably 0.50m / s~3.50m / s.

[0017] The present application updates the surface of the mineralized raw material according to a predetermined update frequency during the mineralization process, so that CO2 in the gas can fully contact the mineralized raw material and react quickly. Specifically, the surface update refers to updating the surface of the mineralized raw material in contact with the gas. In some specific implementations, the surface update method includes but is not limited to at least one of tumbling, stirring, flat scraping, vibration, sweeping, swinging, sliding and fluidization, as long as the surface of the mineralized raw material in contact with the gas can be changed.

[0018] In some specific implementations, the present application updates the surface of the mineralized raw material according to a predetermined update frequency. As described above, the update frequency is determined according to the functional relationship between the physical property parameters of the mineralized raw material and the physical property parameters of the gas; the physical property parameters of the mineralized raw material include the water content of the mineralized raw material. , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials and at least one of the particle size d of the mineralized raw material; the physical property parameters of the gas include the partial pressure of CO2 in the gas and the absolute humidity of the gas At least one of the following. The present application provides for the moisture content of the mineralized raw material , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials , particle size d of mineralized raw materials, partial pressure of CO2 in gas and the absolute humidity of the gas There is no particular limitation on the determination method, and any method known to those skilled in the art may be used. For example, the moisture content of the mineralized raw material It can be determined as follows:

[0019] Drying method: The mineralized raw materials are heated at a certain temperature to evaporate the water, and the moisture content is calculated by weighing the change in the sample mass. The commonly used drying temperature is 105°C, and the mineralized raw materials are dried until the mass is basically constant.

[0020] The content of the fixed CO2 component in the mineralized raw material It can be determined by the following method:

[0021] Sucrose method: The basic principle of this method is to use the reactivity of sucrose and calcium hydroxide in water, determine the content of calcium generated by the reaction by titration, and thus deduce the content of the fixable CO2 component (calculated as calcium hydroxide).

[0022] The bulk density of the mineralized material It can be determined by the following method:

[0023] Vibration compaction method: The vibration compaction method is a commonly used bulk density detection method. It uses a vibration compactor to compact the material under certain conditions to obtain the bulk density of the mineralized raw material.

[0024] The particle size d of the mineralized raw material can be measured according to the following method:

[0025] Sieving method: Sieving method is one of the most commonly used traditional particle size testing methods. It determines the distribution of particles in different size ranges by sieving the granular material through a series of sieves with different aperture sizes.

[0026] The partial pressure of CO2 in the gas It can be determined by the following method:

[0027] Dalton's law of partial pressure: = × P total Calculate the partial pressure of CO2 in a gas ,in is the mole fraction of CO2, P total is the total pressure of the gas.

[0028] Absolute humidity of the gas It can be determined by the following method:

[0029] Wet-and-dry bulb method: Wet-and-dry bulb method is a common method for measuring absolute humidity. It uses the relationship between the heat required for evaporation of water in the gas and the relative humidity in the gas to calculate the absolute humidity value.

[0030] In some specific implementations, when gas is introduced into the mineralized raw material under the condition of moving, the mineralized raw material has a moving speed and the gas has a flow speed. The moving speed of the mineralized raw material and the flow speed of the gas will also affect the absorption rate of CO2 by the mineralized raw material. Based on this, the physical property parameters of the mineralized raw material selected in this application include the water content of the mineralized raw material. , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials , the particle size d of the mineralized material, and also the movement speed of the mineralized material The physical properties of the gas selected in this application are as follows: , absolute humidity of gas , also includes the gas flow rate, that is, the gas flow rate The present application provides for the movement speed of the mineralized raw material. and gas flow rate There is no particular limitation on the method for determining the speed of the mineralized material, and any method known to those skilled in the art may be used. It can be determined by the following method:

[0031] Speed ​​method: An important physical quantity that describes the state of motion of an object, which indicates the distance moved by the object in a unit of time, in m / s (meters per second). Specifically, a marker or internal standard can be selected based on the distance moved in a unit of time, and the moving distance of the marker at time t0 and t can be recorded to calculate the moving speed;

[0032] Gas flow rate can be determined by the following method:

[0033] The wind speed is determined by an anemometer, which measures the rotation speed of the cup or propeller. The cup or propeller rotates around its axis under the influence of wind force, and its rotation speed is proportional to the wind speed.

[0034] In some specific implementations, the functional relationship between the physical property parameters of the mineralized raw material and the physical property parameters of air satisfies formula (1):

[0035] Formula (1);

[0036] In formula (1), F is the surface renewal frequency of the mineral raw material, the unit is 1 / h; is the partial pressure of CO2 in the gas, in kp a ; is the absolute humidity of the gas, in g / Kg dry gas; is the gas flow rate, in m / s; is the moisture content of the mineralized raw material, in %; It is the content of fixed CO2 component in the mineralized raw material, in %; is the bulk density of the mineralized raw material, in kg / m 3 ; is the moving speed of the mineralized raw material, in m / s; d is the particle size of the mineralized raw material, in m;

[0037] is the highest power coefficient of the power function of the effect of the partial pressure of CO2 in the gas on the CO2 absorption rate; is the highest power coefficient of the power function of the effect of gas flow rate on CO2 absorption rate; The highest power coefficient of the power function of the influence of the movement speed of the mineralized material on the CO2 absorption rate; It is the highest power coefficient of the power function of the effect of the particle size of the mineralized raw material on the CO2 absorption rate.

[0038] In some specific implementations, , , and Satisfies formula (2):

[0039] Formula (2).

[0040] In some specific implementations, Obtained as follows:

[0041] After spreading the mineral raw materials, gas is introduced under closed conditions for mineralization to establish the partial pressure of CO2 in the gas. The functional relationship between the absorption rate η of CO2 and value;

[0042] The CO2 absorption rate η is calculated according to formula (3):

[0043] Formula (3);

[0044] In formula (3), η is the absorption rate of CO2, in g / h; P is the absolute pressure of the gas, in Kpa; V in is the inlet gas flow rate, in m 3 / h; C in is the carbon dioxide concentration in the inlet gas, in vol%; V out is the outlet gas flow rate, in m 3 / h; C out is the outlet gas carbon dioxide concentration, in vol%; Z is the compression factor, dimensionless; R is the gas constant, which is 8.314 J / (mol·K); T is the gas temperature, in K; 44 is the molar mass of carbon dioxide, in g / mol.

[0045] Specifically, the present application selects the absolute pressure of the gas during a series of mineralization processes to obtain a series of partial pressures of CO2 in the gas: , experimentally obtain a series of CO2 absorption rates η, and then establish the partial pressure of CO2 in the gas The functional relationship between the absorption rate η of CO2 and the highest power coefficient is value.

[0046] In some specific implementations, Obtained as follows:

[0047] After spreading the mineral raw materials, gas is introduced under closed conditions to establish the gas flow rate on the surface of the mineral raw materials. The functional relationship between the absorption rate η of CO2 and Value, where the CO2 absorption rate η is calculated according to formula (3).

[0048] Specifically, this application selects the air flow rate during the series mineralization process , thereby calculating the absorption rate η of the series CO2, and then establishing the air flow rate The functional relationship between the absorption rate η of CO2 and the highest power coefficient is value.

[0049] In some specific implementations, Obtained as follows:

[0050] After spreading the mineral raw materials, gas is introduced while moving the mineral raw materials under closed conditions to establish the moving speed of the mineral raw materials. The functional relationship between the absorption rate η of CO2 and Value, where the CO2 absorption rate η is calculated according to formula (3).

[0051] Specifically, the application selects the movement speed of the mineral raw materials during the series mineralization process , thereby calculating the absorption rate η of the series CO2, and then establishing the movement speed of the mineral raw materials The functional relationship between the absorption rate η of CO2 and the highest power coefficient is value.

[0052] In some specific implementations, Obtained as follows:

[0053] After spreading the mineral raw materials, gas is introduced under closed conditions to establish a functional relationship between the particle size d of the mineral raw materials and the absorption rate η of CO2, and obtain Value, where the CO2 absorption rate η is calculated according to formula (3).

[0054] Specifically, the present application selects the particle size d of the mineral raw material in the series of mineralization processes to calculate the absorption rate η of the series of CO2, and then establishes the functional relationship between the particle size d of the mineral raw material and the absorption rate η of CO2, and selects its highest power coefficient, which is value.

[0055] After obtaining the surface renewal frequency of the mineral raw materials, the surface of the mineralized raw materials is renewed according to the frequency, which can increase the absorption rate of the mineral raw materials for CO2 in the gas and increase the utilization rate of the fixable CO2 components in the mineralized raw materials.

[0056] This application establishes the partial pressure of CO2 in the gas and the absolute humidity of the gas Physical properties of gases and water content of mineralized raw materials , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials The functional relationship between the physical performance parameters of the mineralized raw materials, including the particle size d of the mineralized raw materials, etc., determines the frequency of surface renewal of the mineralized raw materials according to the above performance, and renews the surface of the mineralized raw materials according to the frequency, which can increase the absorption rate of CO2 in the gas by the mineral raw materials and increase the utilization rate of the fixed CO2 components in the mineralized raw materials. The experimental results show that when the method provided by the present application is used to mineralize CO2 in the air, the average absorption rate of CO2 in the air can reach 20g / m 2 / h or more, and the utilization rate of mineralizable components (calculated as calcium hydroxide) in the mineralized raw materials is more than 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 A schematic diagram of the process provided in this application. DETAILED DESCRIPTION

[0058] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0060] In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined. In addition, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0061] The present application provides a method for mineralizing CO2 in gas, comprising the following steps:

[0062] The CO2 in the gas is mineralized by using a mineralized raw material, and the surface of the mineralized raw material is updated according to a predetermined update frequency during the mineralization process;

[0063] The updating frequency is determined according to the functional relationship between the physical property parameters of the mineralized raw material and the physical property parameters of the gas;

[0064] The physical property parameters of the mineralized raw material include the moisture content of the mineralized raw material , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials and at least one of the particle size d of the mineralized raw material;

[0065] The physical properties of the gas include the partial pressure of CO2 in the gas and the absolute humidity of the gas At least one of .

[0066] See also Figure 1 , Figure 1 This is a flow chart of the method provided in the present application. In the present application, a CO2-containing gas, such as air, is introduced into a mineralized raw material for mineralization. After the surface of the mineralized raw material is renewed at a predetermined frequency, the CO2-containing gas is continued to be introduced for mineralization until all the mineralized raw material is carbonated. This method can increase the absorption rate of the mineral raw material for CO2 in the gas and increase the utilization rate of the fixable CO2 component in the mineralized raw material.

[0067] The method for mineralizing CO2 in gas provided by the present application is described in detail below with reference to the embodiments.

[0068] Example 1

[0069] In this embodiment, industrial solid waste carbide slag is used as the mineralization raw material. The moisture content of the carbide slag is 5%, the particle size is 100 mesh, and the bulk density is 400 kg / m 3 , where the mass fraction of calcium hydroxide, a component that can mineralize CO2, is 85%.

[0070] Determination of value:

[0071] Take 1 kg of the above carbide slag and spread it to a thickness of 0.002m, spreading area is 1.25m 2 , and then air was introduced into the chamber after sealing; the concentration of CO2 in the air at normal pressure was measured to be 380ppm, and the partial pressure of CO2 in the air was adjusted according to the data shown in Table 1 , while controlling the absolute humidity of the air The air velocity on the surface of carbide slag is 8 g / kg dry air. The air velocity is 3m / s, the concentration and ventilation volume of CO2 at the inlet and outlet are measured, and the absorption rate of CO2 η is calculated according to the following formula, in g / h:

[0072]

[0073] Where: P represents the absolute pressure of air, kPa; V in is the inlet air flow rate, m 3 / h;

[0074] C in is the carbon dioxide concentration of the inlet raw gas, vol%; V out is the outlet raw gas flow rate, m 3 / h;

[0075] C out is the outlet raw gas carbon dioxide concentration, vol%; Z is the compression factor, dimensionless; R is the gas constant, 8.314 J / (mol·K); T is the gas temperature, K; 44 is the molar mass of carbon dioxide, g / mol.

[0076] The results are shown in Table 1, which is Example 1. The experimental results of the determination of the value.

[0077] Table 1 Example 1 Experimental results of the determination of the value

[0078] The experimental results η and The fitting result is, η = 1123.12 - 3.61, R² = 0.99525, then The value is 1.

[0079] Determination of value:

[0080] The experimental operation and method are the same as The difference is that the air velocity on the surface of carbide slag is adjusted according to the parameters shown in Table 2. , the experimental results η and Fitting, , R² = 0.9891, then The value is 2.

[0081] Table 2 Example 1 Experimental results of the determination of the value

[0082] Determination of value:

[0083] The experimental method is the same as The difference is that the carbide slag rolls and moves at a certain rate. The moving speed of the carbide slag is adjusted according to the parameters in Table 3. , for the experimental results η and Fitting,

[0084] , R² = 0.9908, then The value is 3.

[0085] Table 3 Example 1 Experimental results of the determination of the value

[0086] Determination of value:

[0087] The experimental operation and method are the same as The difference is that the particle size d of the carbide slag is adjusted according to the parameters in Table 4, and the experimental results η and d are fitted to obtain: , R² = 0.9816, then The value is 1.

[0088] Table 4 Example 1 Experimental results of the determination of the value

[0089] , , and Satisfying formula 2

[0090] Formula 2.

[0091] Calculate the update frequency according to Formula 1:

[0092] Formula 1;

[0093] In this embodiment, the moisture content of carbide slag is 5%, the particle size of carbide slag is 100 mesh, that is, d is ; Measure the bulk density of carbide slag 400 kg / m 3 ; Mass fraction of calcium hydroxide, a component that can mineralize CO2 in carbide slag is 85%; under normal pressure, the concentration of CO2 in the air is 380ppm, the partial pressure is 0.0385kpa, and the absolute humidity of the air during the experiment 12g / kg dry air, air flow rate is 2.5m / s, and the relative movement speed of carbide slag is The surface renewal frequency of carbide slag is 0.12m / s, and it is calculated that the surface renewal frequency of carbide slag should be 34.4h, that is, the surface of carbide slag should be renewed every 34.4h.

[0094] Under the above conditions, 500 kg of calcium carbide slag is placed on a conveyor belt with an area of ​​12.5 m 2 The thickness of the carbide slag was 5 cm, and the conveyor belt was reciprocating. Air was blown above the conveyor belt. Every 34.4 hours, the surface with a thickness of 0.5 cm was cleaned by flat scraping until it was completely cleaned. After the reaction was completed, the change in the carbonate content in the carbide slag was measured, and the average air absorption rate was calculated to be 65.28 g / m 2 / h, the utilization rate of calcium hydroxide in carbide slag is 96.31%.

[0095] Example 2

[0096] The mineralization of CO2 in the air was carried out according to the same method and steps as in Example 1, except that the mineralization raw material was steel slag, the calcium oxide content in the steel slag was 35.26%, and the moisture content was 3%, the particle size is 200 mesh, that is, d is , the bulk density of steel slag 750 kg / m 3 , where the mass fraction of calcium oxide, a component that can mineralize CO2, is The absolute humidity of the air is 35.26%, using normal pressure air, the concentration of CO2 is 380ppm, the partial pressure is 0.0385kpa, and the absolute humidity of the air is 14g / kg dry air, air flow rate is 4.5m / s, and the relative movement speed of slag is is 0.5m / s, and the correlation coefficient of slag renewal frequency under the above conditions is measured =1, =3, =2, =3. According to the surface renewal frequency formula, the surface renewal frequency of steel slag should be 2.46h, that is, the surface of steel slag should be renewed every 2.46h.

[0097] Under the above conditions, take 500kg of steel slag and place it on a conveyor belt with an area of ​​12.5m 2 The thickness of the slag is 3 cm. The conveyor belt reciprocates at a speed of 0.5 m / s, and the above-mentioned conditioned air is blown above the conveyor belt at a flow rate of 4.5 m / s. The belt is vibrated every 2.46 hours to mix and replace the surface slag with the bottom slag. The change in the carbonate content in the slag after the reaction is completed is measured, and the average air absorption rate is calculated to be 25.06 g / m 2 / h, the utilization rate of calcium (calculated as calcium hydroxide) in steel slag is 90.17%.

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for mineralizing CO2 in gas, comprising the following steps: The CO2 in the gas is mineralized by using a mineralized raw material, and the surface of the mineralized raw material is updated according to a predetermined update frequency during the mineralization process; The updating frequency is determined according to the functional relationship between the physical property parameters of the mineralized raw material and the physical property parameters of the gas; The physical property parameters of the mineralized raw material include the moisture content of the mineralized raw material , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials and at least one of the particle size d of the mineralized raw material; The physical properties of the gas include the partial pressure of CO2 in the gas and the absolute humidity of the gas At least one of .

2. The method according to claim 1, characterized in that: During the mineralization process, gas is introduced under conditions that allow the mineralized material to move.

3. The method according to claim 2, characterized in that The physical property parameters of the mineralized raw material include the moisture content of the mineralized raw material , the content of fixed CO2 components in mineralized raw materials , Bulk density of mineralized raw materials , the particle size d of the mineralized raw material and the movement speed of the mineralized raw material ; The physical properties of the air include the partial pressure of CO2 in the gas , absolute humidity of gas and gas flow rate .

4. The method according to claim 3, characterized in that The functional relationship between the physical property parameters of the mineralized raw material and the physical property parameters of the gas satisfies formula (1): Formula (1): In formula (1), F is the surface renewal frequency of the mineral raw material, the unit is 1 / h; is the partial pressure of CO2 in the gas, in kp a ; is the absolute humidity of the gas, in g / Kg dry gas; is the gas flow rate, in m / s; is the moisture content of the mineralized raw material, in %; It is the content of fixed CO2 component in the mineralized raw material, in %; is the bulk density of the mineralized raw material, in kg / m 3 ; is the moving speed of the mineralized raw material, in m / s; d is the particle size of the mineralized raw material, in m; is the highest power coefficient of the power function of the effect of the partial pressure of CO2 in the gas on the CO2 absorption rate; is the highest power coefficient of the power function of the effect of gas flow rate on CO2 absorption rate; The highest power coefficient of the power function of the influence of the movement speed of the mineralized material on the CO2 absorption rate; It is the highest power coefficient of the power function of the effect of the particle size of the mineralized raw material on the CO2 absorption rate.

5. The method according to claim 4, characterized in that , , and Satisfies formula (2): Formula (2).

6. The method according to claim 5, characterized in that Obtained as follows: After spreading the mineral raw materials, gas is introduced under closed conditions to establish the partial pressure of CO2 in the gas. The functional relationship between the absorption rate η of CO2 and value; The CO2 absorption rate η is calculated according to formula (3): Formula (3); In formula (3), η is the absorption rate of CO2, in g / h; P is the absolute pressure of the gas, in Kpa; V in is the inlet gas flow rate, in m 3 / h; C in is the carbon dioxide concentration in the inlet gas, in vol%; V out is the outlet gas flow rate, in m 3 / h; C out is the outlet gas carbon dioxide concentration, in vol%; Z is the compression factor; R is the gas constant; T is the gas temperature, in K; Obtained as follows: After spreading the mineral raw materials, gas is introduced under closed conditions to establish the gas flow rate on the surface of the mineral raw materials. The functional relationship between the absorption rate η of CO2 and Value, where the CO2 absorption rate η is calculated according to formula (3); Obtained as follows: After spreading the mineral raw materials, gas is introduced while moving the mineral raw materials under closed conditions to establish the moving speed of the mineral raw materials. The functional relationship between the absorption rate η of CO2 and Value, where the CO2 absorption rate η is calculated according to formula (3); Obtained as follows: After spreading the mineral raw materials, gas is introduced under closed conditions to establish a functional relationship between the particle size d of the mineral raw materials and the absorption rate η of CO2, and obtain Value, where the CO2 absorption rate η is calculated according to formula (3).

7. The method according to any one of claims 1 to 6, characterized in that: The mineralized raw material is selected from carbide slag, steel slag, red mud, serpentine, forsterite, basalt, volcanic ash, concrete or wollastonite.

8. The method according to claim 7, characterized in that The dry weight of the mineralized raw material is 10 kg / m 2 ~50kg / m 2 ; The content of mineralizable CO2 components in the mineralized raw material is not less than 5%; the moisture content of the mineralized raw material is 2wt%~40wt%; the particle size of the mineralized raw material is 20 mesh~2000 mesh.

9. The method according to claim 7, characterized in that: The gas is air or waste gas containing CO2; The water content of the gas is 2 g / kg dry gas to 40 g / kg dry gas.

10. The method according to any one of claims 1 to 6, characterized in that: The surface renewal method is at least one of tumbling, stirring, scraping, vibrating, blowing, shaking, sliding and fluidizing.

Citation Information

Cited By

  • Method for mineralizing co 2 in gas

    WO2026045068A1