Preparation method of titanium oxide-zirconium oxide composite ultrafiltration membrane
The titanium oxide-zirconia composite nano solution was prepared by sol-gel method and microwave hydrothermal method, and plasticizer and binder were added, which solved the problems of high moisture content and low crystallization of nanoparticles in ceramic ultrafiltration membranes, and achieved the The preparation of high-quality ceramic ultrafiltration membranes avoids the need for multiple coatings and improves the integrity and performance of the membrane layer.
Patent Information
- Application Number
- CN202410964172.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing ceramic ultrafiltration membrane preparation methods, the nanoparticles prepared by the sol-gel method have high moisture content and low crystallization degree, which leads to the membrane layer being prone to cracking, and the coating film needs to be repeated multiple times to ensure integrity.
Titanium oxide-zirconia composite sol is prepared by sol-gel method, and a uniform nano solution is obtained by microwave hydrothermal treatment. Plasticizer and binder are added, and a complete ceramic can be prepared after a coating film and low-temperature calcination. Ultrafiltration membrane.
The preparation of ceramic ultrafiltration membranes with fine grains, uniform grain size and complete crystal shape is achieved, avoiding the defects of multiple coatings and improving the integrity and performance of the membrane layer.
Smart Images

Figure CN118904104A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultrafiltration membrane preparation, and specifically relates to a method for preparing a titanium oxide-zirconium oxide composite ultrafiltration membrane. Background Art
[0002] Ceramic ultrafiltration membranes have become a research hotspot in the field of ultrafiltration membranes in recent years due to their advantages in high temperature resistance, solvent resistance, corrosion resistance, and high mechanical strength in the actual separation process. Ceramic membrane materials mainly include aluminum oxide, titanium oxide, zirconium oxide, and silicon oxide. In particular, zirconium oxide (ZrO2) materials stand out for their higher mechanical strength, better thermal stability, and chemical stability. Therefore, the development of zirconium oxide ultrafiltration membranes has important market development and application value.
[0003] Sol-gel method is the main method for preparing ceramic ultrafiltration membranes. However, the nanoparticles prepared by this method have a high water content and a low degree of crystallization, which makes the membrane layer easy to crack. In order to ensure the integrity of the membrane layer, it is usually necessary to repeat the coating several times. Summary of the invention
[0004] The present invention aims to overcome the defects of the prior art and provide a method for preparing a titanium oxide-zirconium oxide composite ultrafiltration membrane.
[0005] The technical solution of the present invention is as follows:
[0006] A method for preparing a titanium oxide-zirconia composite ultrafiltration membrane comprises the following steps:
[0007] (1) adding a first dispersant to a mixed solution of an inorganic zirconium salt and an organic titanium alkoxide, adding ammonia water or sodium hydroxide dropwise thereto at 50-65° C. while stirring to adjust the pH to 9-11, then keeping the mixture warm for 2-3 hours, and then performing solid-liquid separation to obtain a solid, drying the solid and redispersing it in water, adding a nitric acid solution for peptization and making the pH of the peptized material 1-2, to obtain a Ti-Zr composite sol; the first dispersant is polyethylene glycol with a weight average molecular weight of 550-650; in the mixed solution, the molar ratio of the inorganic zirconium salt to the organic titanium alkoxide is 5-10:1, and in the mixed solution, the concentration of the inorganic zirconium salt is 0.5-2 mol / L, and the concentration of the organic titanium alkoxide is 0.5-2 mol / L;
[0008] (2) adding a second dispersant to the Ti-Zr composite sol obtained in step (1), stirring evenly, placing in a microwave hydrothermal reaction system with a filling degree of 50-80%, keeping warm for 1-3 hours at a pressure of 0.5-2 MPa, and obtaining a Ti-Zr composite nano-solution after cooling; the second dispersant is glycerol or PEG400;
[0009] (3) adding a plasticizer and a binder to the Ti-Zr composite nano-solution obtained in step (2), mixing them evenly, and then adding an organosilicon defoamer to obtain a coating solution; the plasticizer is polyethylene glycol with a weight average molecular weight of 350-450, and the binder is a cellulose compound with a molecular weight of 6000-10000;
[0010] (4) Apply the above coating liquid on the porous alumina ceramic membrane support, heat it to 100-120°C and dry it for 2-5 hours, then heat it to 600-700°C and calcine it for 2-3 hours, and then cool it to obtain the titanium oxide-zirconia composite ultrafiltration membrane.
[0011] In a preferred embodiment of the present invention, the inorganic zirconium salt is zirconium oxychloride or zirconium sulfate.
[0012] More preferably, the inorganic zirconium salt is zirconium oxychloride.
[0013] In a preferred embodiment of the present invention, the organic titanium alkoxide is titanium isopropoxide or titanium tert-butoxide.
[0014] More preferably, the organic titanium alkoxide is titanium isopropoxide.
[0015] In a preferred embodiment of the present invention, the cellulose compound is hydroxymethyl cellulose, hydroxyethyl cellulose or hydroxypropyl cellulose.
[0016] More preferably, the cellulose compound is hydroxymethyl cellulose.
[0017] In a preferred embodiment of the present invention, the inorganic zirconium salt is zirconium oxychloride, the organic titanium alkoxide is titanium isopropoxide, and the cellulose compound is hydroxymethyl cellulose.
[0018] In a preferred embodiment of the present invention, in the step (1), the first dispersant is added to a final concentration of 1-3wt%; in the step (2), the second dispersant is added to a final concentration of 1-3wt%; in the step (3), the plasticizer and the binder are added to a final concentration of 2-5wt% and 0.1-0.5wt%, respectively, and the silicone defoamer is added to a final concentration of 0.01-0.1wt%.
[0019] Further preferably, the step (4) is: apply the above-mentioned coating liquid on the porous alumina ceramic membrane support, heat it to 100-120°C at a rate of 1-3°C / min, and then keep it warm and dry for 2-5h, then heat it to 600-700°C at a rate of 1-3°C / min, and then keep it warm and calcine for 2-3h, and then cool it to obtain the titanium oxide-zirconia composite ultrafiltration membrane.
[0020] The beneficial effects of the present invention are as follows: the present invention adopts a sol-gel method to prepare a Ti-Zr composite sol as a precursor; subsequently, a Ti-Zr composite nano-solution with uniform particle size is obtained by microwave hydrothermal treatment; a proper amount of additives is added to the Ti-Zr composite nano-solution to directly prepare a coating liquid; after a coating, a drying and calcination process is performed, a Ti-Zr composite ultrafiltration membrane can be prepared; compared with the method of preparing nanoparticles by a traditional hydrothermal method, the powder prepared by the present invention using the sol-microwave hydrothermal method exhibits the advantages of fine grains, uniform particle size, complete crystal development and no agglomeration, and in addition, by adding a plasticizer and a binder and undergoing low-temperature calcination, the present invention successfully prepares a ceramic ultrafiltration membrane, and realizes the preparation of a defect-free Ti-Zr composite ceramic ultrafiltration membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope photograph of the membrane layer of the titanium oxide-zirconium oxide composite ultrafiltration membrane prepared in Example 1 of the present invention.
[0022] Figure 2 This is a scanning electron microscope photograph of the membrane layer of the comparative composite ceramic ultrafiltration membrane prepared in Comparative Example 1 of the present invention.
[0023] Figure 3 This is a scanning electron microscope photograph of the membrane layer of the zirconia ceramic ultrafiltration membrane prepared in Comparative Example 2 of the present invention.
[0024] Figure 4 This is a scanning electron microscope photograph of the membrane layer of the comparative composite ceramic ultrafiltration membrane prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.
[0026] Example 1
[0027] (1) adding a dispersant polyethylene glycol PEG600 to a mixed solution containing 0.5 mol / L zirconium oxychloride and 0.1 mol / L titanium isopropoxide to a final concentration of 2 wt %, and adding 0.1 mol / L ammonia water dropwise thereto at 60° C. while stirring to adjust the pH value to 9; reacting for 2.5 hours, filtering to separate the solid and liquid, taking the solid part and drying it at 60° C., redispersing it in water, adding a 0.1 mol / L nitric acid solution to peptize it and adjusting the pH value of the peptized solution to 1, to obtain a Ti-Zr composite sol;
[0028] (2) adding 1 wt % glycerol to the Ti-Zr composite sol prepared in step (1), stirring evenly, placing in a microwave hydrothermal reactor with a filling degree of 60%, keeping the reaction temperature at 0.5 MPa for 2 h, cooling, and obtaining a Ti-Zr composite nano-solution;
[0029] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Ti-Zr composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 3wt% and 0.3wt% respectively, stirring evenly, and then adding silicone defoaming agent Dow Corning DC65 to a final concentration of 0.05wt%, mixing evenly, and preparing a coating solution;
[0030] (4) Apply the coating liquid obtained in step (3) on a porous alumina ceramic membrane support with an average pore size of 0.1 μm, heat it to 120°C at a heating rate of 2°C / min, dry it for 3 hours, then heat it to 650°C at a heating rate of 2°C / min, keep it warm and calcine it for 2 hours, and cool it to obtain a titanium oxide-zirconia composite ultrafiltration membrane with performance parameters as shown in Table 1. The titanium oxide-zirconia composite ultrafiltration membrane prepared in this embodiment has an average pore size of 8-10nm. Under the 0.3MPa pressure test condition, the titanium oxide-zirconia composite ultrafiltration membrane has a retention rate of more than 95% for 2g / L dextran (molecular weight 100,000), a flux of 123LHM, and after a bubble pressure test, the overall bubble pressure is greater than 0.5MPa. The membrane layer of the titanium oxide-zirconia composite ultrafiltration membrane is as shown in Table 1. Figure 1 shown.
[0031] Example 2
[0032] (1) adding a dispersant polyethylene glycol PEG600 to a mixed solution containing 0.5 mol / L zirconium oxychloride and 0.1 mol / L titanium isopropoxide to a final concentration of 2%, and adding 0.1 mol / L ammonia water dropwise thereto at 60° C. while stirring to adjust the pH value to 9; reacting for 2.5 hours, filtering to separate the solid and liquid, taking the solid part and drying it at 60° C., redispersing it in water, adding a nitric acid solution with a concentration of 0.1 mol / L to peptize it and adjusting the pH value of the solution after peptization to 1, to obtain a Ti-Zr composite sol;
[0033] (2) adding 1 wt % glycerol to the Ti-Zr composite sol prepared in step (1), stirring evenly, placing in a microwave hydrothermal reactor with a filling degree of 60%, keeping the reaction temperature at 1 MPa for 2 h, cooling, and obtaining a Ti-Zr composite nano-solution;
[0034] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Ti-Zr composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 3wt% and 0.3wt% respectively, stirring evenly, and then adding silicone defoaming agent Dow Corning DC65 to a final concentration of 0.05wt%, mixing evenly, and preparing a coating solution;
[0035] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 0.1 μm, and the temperature is raised to 120°C at a heating rate of 2°C / min, dried for 3 hours, and then raised to 650°C at a heating rate of 2°C / min, calcined for 2 hours, and cooled to obtain a titanium oxide-zirconia composite ultrafiltration membrane having performance parameters as shown in Table 1. The titanium oxide-zirconia composite ultrafiltration membrane prepared in this embodiment has an average pore size of 12-13 nm. Under the 0.3 MPa pressure test condition, the titanium oxide-zirconia composite ultrafiltration membrane has a retention rate of more than 92 wt% for 2 g / L dextran (molecular weight 100,000), a flux of 141 LHM, and an overall bubble pressure greater than 0.5 MPa after a bubble pressure test.
[0036] Example 3
[0037] (1) adding a dispersant polyethylene glycol PEG600 to a mixed solution containing 0.5 mol / L zirconium oxychloride and 0.1 mol / L titanium isopropoxide to a final concentration of 2 wt %, and adding 0.1 mol / L ammonia water dropwise thereto at 60° C. while stirring to adjust the pH value to 9; reacting for 2.5 hours, filtering to separate the solid and liquid, taking the solid part and drying it at 60° C., redispersing it in water, adding a 0.1 mol / L nitric acid solution to peptize it and adjusting the pH value of the peptized solution to 1, to obtain a Ti-Zr composite sol;
[0038] (2) adding 1 wt % glycerol to the Ti-Zr composite sol prepared in step (1), stirring evenly, placing in a microwave hydrothermal reactor with a filling degree of 60%, keeping the reaction temperature at 0.5 MPa for 2 h, cooling, and obtaining a Ti-Zr composite nano-solution;
[0039] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Ti-Zr composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 3wt% and 0.3wt% respectively, stirring evenly, and then adding silicone defoaming agent Dow Corning DC65 to a final concentration of 0.05wt%, mixing evenly, and preparing a coating solution;
[0040] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 0.1 μm, and the temperature is raised to 120°C at a heating rate of 2°C / min, dried for 3 hours, and then raised to 650°C at a heating rate of 2°C / min, calcined for 2 hours, and cooled to obtain a titanium oxide-zirconia composite ultrafiltration membrane having performance parameters as shown in Table 1. The titanium oxide-zirconia composite ultrafiltration membrane prepared in this embodiment has an average pore size of 14-15 nm. Under the 0.3 MPa pressure test condition, the titanium oxide-zirconia composite ultrafiltration membrane has a retention rate of more than 90 wt% for 2 g / L dextran (molecular weight 100,000), a flux of 150 LHM, and an overall bubble pressure greater than 0.5 MPa after a bubble pressure test.
[0041] Comparative Example 1
[0042] (1) adding a dispersant polyethylene glycol PEG600 to a mixed solution containing 0.5 mol / L zirconium oxychloride and 0.1 mol / L titanium isopropoxide to a final concentration of 2 wt %, and adding 0.1 mol / L ammonia water dropwise thereto at 60° C. while stirring to adjust the pH value to 9; reacting for 2.5 hours, filtering to separate the solid and liquid, taking the solid part and drying it at 60° C., redispersing it in water, adding a 0.1 mol / L nitric acid solution to peptize it and adjusting the pH value of the peptized solution to 1, to obtain a Ti-Zr composite sol;
[0043] (2) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Ti-Zr composite sol prepared in step (1), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 3wt% and 0.3wt% respectively, stirring evenly, and then adding an organosilicon defoamer Dow Corning DC65 to a final concentration of 0.05wt%, mixing evenly, and preparing a coating solution;
[0044] (3) The coating liquid prepared in step (2) is applied to a porous alumina ceramic membrane support with an average pore size of 0.1 μm, and the temperature is raised to 120°C at a heating rate of 2°C / min, dried for 3 hours, and then raised to 650°C at a heating rate of 2°C / min, calcined for 2 hours, and cooled to obtain a comparative composite ceramic ultrafiltration membrane with performance parameters as shown in Table 1. Under the 0.3 MPa pressure test condition, the comparative composite ceramic ultrafiltration membrane has a retention rate of more than 5 wt% for 2 g / L dextran (molecular weight 100,000), a flux of 350 LHM, and a bubble pressure test shows that the overall bubble pressure is greater than 0.25 MPa. The membrane layer of the comparative composite ceramic ultrafiltration membrane is as shown in Table 1. Figure 2 shown.
[0045] Comparative Example 2
[0046] (1) adding a dispersant polyethylene glycol PEG600 to a 0.5 mol / L zirconium oxychloride solution to a final concentration of 2 wt %, and adding 0.1 mol / L ammonia water dropwise thereto at 60° C. while stirring to adjust the pH value to 9; reacting for 2.5 hours, filtering to separate the solid and liquid, taking the solid part and drying it at 60° C., redispersing it in water, adding a 0.1 mol / L nitric acid solution to peptize it and making the pH value of the peptized solution 1.5, to obtain a zirconium oxide sol;
[0047] (2) placing the zirconium oxide sol obtained in step (1) into a hydrothermal reactor with a filling degree of 60%, reacting at 200° C. for 10 h, and cooling to obtain a zirconium oxide nano-solution;
[0048] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the zirconium oxide nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 3wt% and 0.3wt% respectively, stirring evenly, and then adding silicone defoaming agent Dow Corning DC65 to a final concentration of 0.05wt%, mixing evenly, and preparing a coating solution;
[0049] (4) Apply the coating liquid obtained in step (3) to a porous alumina ceramic membrane support with an average pore size of 50 nm, heat it to 120°C at a heating rate of 2°C / min, dry it for 3 hours, then heat it to 650°C at a heating rate of 2°C / min, calcine it at this temperature for 2 hours, and cool it to obtain a zirconia ceramic ultrafiltration membrane with performance parameters as shown in Table 1. Under the 0.3MPa pressure test condition, the zirconia ceramic ultrafiltration membrane has a retention rate of more than 35wt% for 2g / L dextran (molecular weight 100,000), a flux of 300LHM, and a bubble pressure test shows that the overall bubble pressure is greater than 0.5MPa. The membrane layer of the zirconia ceramic ultrafiltration membrane is as shown in Table 1. Figure 3 shown.
[0050] Comparative Example 3
[0051] (1) adding a dispersant polyethylene glycol PEG600 to a mixed solution containing 0.5 mol / L zirconium oxychloride and 0.1 mol / L titanium isopropoxide to a final concentration of 2 wt %, and adding 0.1 mol / L ammonia water dropwise thereto at 60° C. while stirring to adjust the pH value to 9; reacting for 2.5 hours, filtering to separate the solid and liquid, taking the solid part and drying it at 60° C., redispersing it in water, adding a 0.1 mol / L nitric acid solution to peptize it and adjusting the pH value of the peptized solution to 1, to obtain a Ti-Zr composite sol;
[0052] (2) placing the Ti-Zr composite sol obtained in step (1) into a hydrothermal reaction kettle with a filling degree of 60%, reacting at 200° C. for 10 h, and cooling to obtain a Ti-Zr composite nano-solution;
[0053] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Ti-Zr composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 3wt% and 0.3wt% respectively, stirring evenly, and then adding silicone defoaming agent Dow Corning DC65 to a final concentration of 0.05wt%, mixing evenly, and preparing a coating solution;
[0054] (4) Apply the coating liquid obtained in step (3) to a porous alumina ceramic membrane support with an average pore size of 0.1 μm, heat it to 120°C at a heating rate of 2°C / min, dry it for 3 hours, then heat it to 650°C at a heating rate of 2°C / min, calcine it at this temperature for 2 hours, and cool it to obtain a comparative composite ceramic ultrafiltration membrane with performance parameters as shown in Table 1. Under the 0.3 MPa pressure test condition, the comparative composite ceramic ultrafiltration membrane has a retention rate of more than 82 wt% for 2 g / L dextran (molecular weight 100,000), a flux of 195 LHM, and a bubble pressure test shows that the overall bubble pressure is greater than 0.5 MPa. The membrane layer of the comparative composite ceramic ultrafiltration membrane is as shown in Table 1. Figure 4 shown.
[0055] Table 1
[0056]
[0057]
[0058] As can be seen from Table 1, in the present invention, the method of doping TiO2 and ZrO2 with a crystal stabilizer can reduce the particle size and prepare a ceramic ultrafiltration membrane with a smaller pore size.
[0059] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A method for preparing a titanium oxide-zirconia composite ultrafiltration membrane, Features: The steps include: (1) adding a first dispersant to a mixed solution of an inorganic zirconium salt and an organic titanium alkoxide, adding ammonia water or sodium hydroxide dropwise thereto at 50-65° C. while stirring to adjust the pH to 9-11, then keeping the mixture warm for 2-3 hours, and then performing solid-liquid separation to obtain a solid, drying the solid and redispersing it in water, adding a nitric acid solution for peptization and making the pH of the peptized material 1-2, to obtain a Ti-Zr composite sol; the first dispersant is polyethylene glycol with a weight average molecular weight of 550-650; in the mixed solution, the molar ratio of the inorganic zirconium salt to the organic titanium alkoxide is 5-10:1, and in the mixed solution, the concentration of the inorganic zirconium salt is 0.5-2 mol / L, and the concentration of the organic titanium alkoxide is 0.5-2 mol / L; (2) adding a second dispersant to the Ti-Zr composite sol obtained in step (1), stirring evenly, placing in a microwave hydrothermal reaction system with a filling degree of 50-80%, keeping warm for 1-3 hours at a pressure of 0.5-2 MPa, and obtaining a Ti-Zr composite nano-solution after cooling; the second dispersant is glycerol or PEG400; (3) adding a plasticizer and a binder to the Ti-Zr composite nano-solution obtained in step (2), mixing them evenly, and then adding an organosilicon defoamer to obtain a coating solution; the plasticizer is polyethylene glycol with a weight average molecular weight of 350-450, and the binder is a cellulose compound with a molecular weight of 6000-10000; (4) Apply the above coating liquid on the porous alumina ceramic membrane support, heat it to 100-120°C and dry it for 2-5 hours, then heat it to 600-700°C and calcine it for 2-3 hours, and then cool it to obtain the titanium oxide-zirconia composite ultrafiltration membrane.
2. The preparation method according to claim 1, Features: The inorganic zirconium salt is zirconium oxychloride or zirconium sulfate.
3. The preparation method according to claim 2, Features: The inorganic zirconium salt is zirconium oxychloride.
4. The preparation method according to claim 1, Features: The organic titanium alkoxide is titanium isopropoxide or titanium tert-butoxide.
5. The preparation method according to claim 4, Features: The organic titanium alkoxide is titanium isopropoxide.
6. The preparation method according to claim 1, Features: The cellulose compound is hydroxymethyl cellulose, hydroxyethyl cellulose or hydroxypropyl cellulose.
7. The preparation method according to claim 6, Features: The cellulose compound is hydroxymethyl cellulose.
8. The preparation method according to claim 1, Features: The inorganic zirconium salt is zirconium oxychloride, the organic titanium alkoxide is titanium isopropoxide, and the cellulose compound is hydroxymethyl cellulose.
9. The preparation method according to any one of claims 1 to 8, Features: In the step (1), the first dispersant is added to a final concentration of 1-3wt%; in the step (2), the second dispersant is added to a final concentration of 1-3wt%; in the step (3), the plasticizer and the binder are added to a final concentration of 2-5wt% and 0.1-0.5wt%, respectively, and the organosilicon defoamer is added to a final concentration of 0.01-0.1wt%.
10. The preparation method as claimed in claim 1, Features: The step (4) is as follows: applying the coating liquid onto a porous alumina ceramic membrane support, heating the temperature to 100-120°C at a rate of 1-3°C / min, and then drying the mixture for 2-5 hours; then heating the temperature to 600-700°C at a rate of 1-3°C / min, and then calcining the mixture for 2-3 hours; and after cooling, the titanium oxide-zirconia composite ultrafiltration membrane is obtained.