Method for preparing coal gas desulfurizer by activating formed semi-coke powder and application of coal gas desulfurizer
By forming the orchid powder into a pellet and heating and steam activation, an efficient gas desulfurization agent is formed, which solves the problem of hydrogen sulfide removal in blast furnace gas and replacing coke powder in sintering, and reduces volatile components and costs. save.
Patent Information
- Application Number
- CN202410967750.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the removal of hydrogen sulfide in blast furnace gas mainly depends on activated carbon adsorption method, which has problems such as high raw material cost and high operating cost. In addition, the sintering process of orchid carbon powder has high volatility, fast combustion speed, and easy to block the dust collector. Limits the proportion of its replacement coke powder.
After the orchid powder is formed into a pellet, the orchid is processed by heating and carbonization, and water vapor is introduced to activate it, reducing volatile components, forming an efficient gas desulfurization agent, replacing activated carbon to achieve the removal of hydrogen sulfide, and replacing metallurgical coke powder during the sintering process.
The volatile content of orchid charcoal powder is effectively reduced to about 2%, achieving efficient removal of hydrogen sulfide, reducing production costs, and allowing a larger proportion of orchid charcoal powder to be used in sintering, improving fuel performance and economicality.
Smart Images

Figure CN118904284A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of fine desulfurization of blast furnace gas in the steel industry, and in particular relates to a method for preparing a gas desulfurizer by activating semi-coke powder after molding and application thereof. Background Art
[0002] Using coal fractionation technology to convert low-rank coal into three different forms of energy, namely coal gas, tar and lignite, is a very effective means of utilizing low-rank coal. Among them, the main product lignite, as a new type of carbon material, has the advantages of high fixed carbon, high chemical activity, high specific resistivity, low ash content, low sulfur and low phosphorus, and has been widely used in the calcium carbide and ferrosilicon industries. In recent years, with the large-scale promotion of coal fractionation technology, especially crushed coal and pulverized coal pyrolysis technology, it is urgent to develop new application markets to consume the large amount of powdered lignite produced.
[0003] On the one hand, with the rapid development of the steel industry, the demand for high-quality anthracite and metallurgical coke powder for iron ore sintering has continued to increase, making the scarcity of anthracite and coking coal increasingly prominent, and it is urgent to seek high-quality alternative raw materials. Compared with anthracite and coke powder, lignite has the advantages of high calorific value, low ash content, and low S / P of harmful elements. Replacing coke powder for sintering can improve the quality of sintered ore and reduce the concentration of pollutants in sintering flue gas. However, lignite powder has the disadvantage of high volatile matter. When it is used as a substitute for metallurgical coke powder for sintering, there are problems such as fast combustion speed and easy clogging of dust collector filter bags. The proportion of lignite powder used during sintering has been limited to about 20%, and the substitution ratio is difficult to further increase, which limits the amount of lignite powder used.
[0004] On the other hand, organic sulfur in blast furnace gas is mainly COS (carbonyl sulfide), which is neutral or weakly acidic and has relatively stable chemical properties, so it is not suitable for conventional desulfurization methods. Experimental verification shows that the hydrolysis catalytic method can effectively achieve the conversion of carbonyl sulfide in blast furnace gas. Its principle is to convert organic sulfur into easily removed hydrogen sulfide through hydrolysis reaction. After carbonyl sulfide is converted into hydrogen sulfide, the total H2S concentration in blast furnace gas is generally 50-200 mg / Nm 3 At present, the removal of hydrogen sulfide is mainly achieved by activated carbon adsorption. Although this method is simple to operate and has stable effects, it requires regular replacement and regeneration of activated carbon, and has the problems of high raw material costs and high operating costs. Summary of the invention
[0005] In order to solve the problems of high raw material cost and high operating cost when the removal of hydrogen sulfide in the prior art is mainly carried out by activated carbon adsorption, the present invention provides a method and application of blue charcoal powder after being formed and activated to prepare a coal gas desulfurizer. The method reduces the volatile matter of blue charcoal to about 2%, and can achieve two uses of one pellet, thereby reducing the production cost as much as possible, achieving the removal of hydrogen sulfide, and providing a new idea for the large-scale utilization of blue charcoal powder.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a coal gas desulfurizer by activating blue carbon powder after molding, comprising the following steps:
[0008] The uniformly mixed semi-coke powder, carbon raw material, binder and additive are pressed and formed to obtain semi-coke pellets with regular shapes;
[0009] The semi-coke pellets are heated to 800-1000°C, and activated by water vapor for 1-6 hours to obtain a coal gas desulfurizer.
[0010] A further improvement of the present invention is that the carbonaceous raw material is a mixture of one or more of anthracite, bituminous coal, metallurgical coke powder, waste activated coke and waste activated carbon.
[0011] A further improvement of the present invention is that the added amount of the carbonaceous raw material does not exceed 15% of the total weight of the blue charcoal powder, the carbonaceous raw material, the binder and the additives.
[0012] A further improvement of the present invention is that the binder is any two or more of starch, coal tar, adhesive coal powder, coal tar and humic acid.
[0013] A further improvement of the present invention is that the amount of binder added is 3-8% of the total weight of the blue charcoal powder and the carbonaceous raw material.
[0014] A further improvement of the present invention is that one or both of boric acid and slaked lime powder are used.
[0015] A further improvement of the present invention is that the amount of the additive added does not exceed 5% of the total weight of the blue charcoal powder and the carbonaceous raw material.
[0016] A further improvement of the present invention is that the shape of the semi-coke pellets is pillow-shaped, ellipsoidal or oval, and the three-dimensional size of the semi-coke pellets is between 15-50 mm.
[0017] The invention discloses an application of a coal gas desulfurizing agent produced by activating blue carbon powder after molding in removing hydrogen sulfide from blast furnace coal gas.
[0018] The invention discloses an application of a coal gas desulfurizing agent activated after blue carbon powder molding in the sintering of iron ore powder.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention proposes for the first time a method of using a combined process of molding + activation to use blue charcoal powder for the production of a blast furnace gas desulfurizer. After being heated and carbonized, the volatile matter of blue charcoal powder can be greatly reduced from the current 8-12% to about 2%, which is equivalent to the volatile matter data of metallurgical coke powder. The corresponding sintering section can use blue charcoal powder in a larger proportion or even entirely. In the present invention, blue charcoal powder is made into pellets and then heated and devolatilized. On the basis of the heating treatment, water vapor is introduced to activate and pore the blue charcoal pellets, and the blue charcoal pellets are converted into a desulfurizer for removing H2S from blast furnace gas. In this method, after blue charcoal powder is made into pellets and heated and activated, its adsorption capacity is first used to replace activated carbon to achieve H2S removal, and then the excellent fuel performance of the desulfurizer after H2S removal is used to replace conventional coke powder to achieve the sintering of iron ore powder. The present invention realizes the double utilization of the same material, and the economic advantage of the entire process is obvious. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the process of producing a coal gas desulfurizer by activating the semi-coke powder after molding according to the present invention;
[0022] Figure 2 It is a schematic diagram of the blue carbon pellet activation process in the present invention. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0024] The normal temperature in the present invention is 25°C.
[0025] In combination with the latest environmental protection needs of the steel industry, the present invention proposes a method for preparing a coal gas desulfurizer by activating blue charcoal powder after molding. First, powdered blue charcoal is pressed into pellets with a binder, and then the pellets are carbonized and activated in an air-isolated furnace for heating and activated with water vapor to prepare desulfurizer pellets. The desulfurizer pellets are then loaded into an adsorption tower to adsorb hydrogen sulfide in blast furnace gas, and discharged from the adsorption tower after saturation. Finally, they are crushed by a pulverizer and used as sintering raw materials for steel enterprises. This process route can reduce the volatile matter of blue charcoal powder to less than 2%. At the same time, the sulfur content of the desulfurizer after activation is close to that of activated carbon, which can replace high-value activated carbon to achieve the goal of removing hydrogen sulfide. The adsorption-saturated blue charcoal pellets are crushed and then used as sintering raw materials. After two uses, the production cost can be greatly diluted, ensuring that the new process has good economic efficiency, thereby realizing the large-scale use of blue charcoal powder in the sintering field.
[0026] See also Figure 1 The method of preparing a coal gas desulfurizing agent by activating blue carbon powder after molding of the present invention comprises the following steps:
[0027] Step 1, the semi-coke powder, other carbon raw materials, binders and other additives are fully stirred and kneaded in a mixing device at room temperature according to the ratio requirements to obtain a molding mixture with uniform properties, and the mixture is pressurized and molded using a high-pressure ball press to obtain semi-coke pellets with regular shapes;
[0028] Among them, the other carbonaceous raw materials in step 1 are a mixture of one or more high-fixed carbon powder materials such as anthracite, bituminous coal, metallurgical coke powder, waste activated coke and waste activated carbon, and the addition amount of other carbonaceous raw materials does not exceed 15% of the total weight of the mixture.
[0029] In the present invention, by adding other carbonaceous raw materials, waste materials can be recycled.
[0030] The binder is any two or more of starch, coal tar, adhesive coal powder, coal tar and humic acid.
[0031] The amount of binder added is 3-8% of the total weight of the blue charcoal powder and other carbonaceous raw materials.
[0032] The other additives are one or both of boric acid and slaked lime powder, and the amount of additives added does not exceed 5% of the total weight of the blue charcoal powder and other carbonaceous raw materials.
[0033] The linear pressure of the high-pressure pellet press can reach 10-20 t / cm. The shape of the prepared pellets can be regular shapes such as pillow, ellipsoid or egg. The preferred three-dimensional dimensions of the pellets are between 10-50 mm.
[0034] Step 2: See Figure 2 , the semi-coke pellets prepared in step 1 are transported and added to a pellet carbonization activation furnace (often an externally heated vertical furnace), where the pellets are gradually heated from room temperature to 800-1000°C by a high-temperature circulating carrier gas. The residence time of the semi-coke pellets in the high-temperature zone of the carbonization activation furnace is controlled to be 1-6 hours. A water vapor nozzle is provided in the high-temperature zone, and the injected water vapor reacts with the high-temperature semi-coke pellets to complete the pore formation of the semi-coke. The activated semi-coke pellets are the coal gas desulfurizer. A partition-type water cooling device is provided at the bottom of the pellet carbonization activation furnace, and the activated pellets are finally discharged from the furnace bottom after partition-type cooling.
[0035] Preferably, the pellet carbonization activation furnace described in step 2 is preferably an externally heated vertical furnace using a circulating carrier gas, and the carrier gas is heated by a gas heating furnace (often a regenerative heating furnace), and the high-temperature circulating carrier gas generally uses a reducing gas containing more carbon monoxide and hydrogen. After the high-temperature circulating carrier gas contacts and exchanges heat with the blue charcoal pellets in the vertical furnace, the blue charcoal is heated to release pyrolysis gas, and the pyrolysis gas is mixed with the carrier gas and enters the purification system to remove coal tar and moisture, and then enters the regenerative heating furnace again after being pressurized by the gas blower for heating and heating and recycling. The maximum heating temperature, carbonization activation reaction time and water vapor addition amount can be selected according to the specific surface area and sulfur capacity requirements of the pellet desulfurizer. When the sulfur capacity requirement is high, it is necessary to appropriately increase the heating temperature, the residence time in the furnace and the amount of water vapor. The tar separated and captured by the purification system of the vertical furnace can be sold as a by-product, and the gas fuel part of the regenerative heating furnace uses the carrier gas removed from the tar by the purification system, and the insufficient part is supplemented by an external gas source.
[0036] The present invention adopts an external heating vertical furnace, which has the advantages of low cost, large output and small investment.
[0037] Step 3: The processed semi-coke pellets, i.e., the desulfurizer, are continuously added into the desulfurization adsorption tower (i.e., the blast furnace gas adsorption desulfurization device) to form an adsorption layer. The blast furnace gas flows through the adsorption layer in the adsorption tower to remove the H2S gas. After the fine desulfurization operation is completed, it enters the subsequent process section. The desulfurizer pellets saturated with adsorption are continuously discharged from the adsorption tower.
[0038] The desulfurization adsorption tower is a moving bed structure, which ensures that fresh semi-coke pellet desulfurizer can be continuously added from the top, and the adsorption saturated pellet desulfurizer is continuously and stably discharged from the bottom of the adsorption tower. The semi-coke adsorbent in the adsorption tower is continuously updated to ensure the adsorption effect.
[0039] Step 4: The adsorbed desulfurizer pellets are crushed and screened by crushing equipment, wherein the 3 mm screened particles are returned to the crushing equipment for re-crushing, and the fine particles below 3 mm are collected and used to replace anthracite and metallurgical coke powder for iron ore powder sintering.
[0040] The crushing equipment in step 4 is recommended to use fine crushing equipment such as double roll crusher, tooth roll crusher and cone crusher, and the particle size of the crushed product should be controlled below 3mm as much as possible.
[0041] In the present invention, the desulfurizing agent pellets after adsorption can be reused after desulfurization.
[0042] Example 1
[0043] See also Figure 1 Step 1: weigh and mix the semi-coke powder, anthracite powder, caking coal powder (fat coal powder) and slaked lime powder in a mass ratio of 80:10:8:2, and then knead them evenly in a kneader at room temperature to obtain a mixture.
[0044] Step 2, adding the mixture obtained in step 1 into the silo of the roller briquetting machine, and pressing it into pillow-shaped semi-coke pellets of 22×18×15 mm under a line pressure of 12 t / cm;
[0045] Step 3, the semi-coke pellet product obtained in step 2 is transferred to the top silo of the external heating vertical furnace, and evenly added to the carbonization furnace through the silo valve. The semi-coke pellets are gradually heated from room temperature to 900°C from top to bottom in the vertical furnace, and the constant temperature is maintained for 1 hour. A steam nozzle is provided in the high temperature constant temperature interval, and low-pressure steam is continuously sprayed into the furnace to activate the semi-coke pellets. After the activation is completed, it enters the cooling section at the bottom of the carbonization furnace and is cooled to 150°C. The cooled pellets are discharged from the bottom of the vertical furnace, and the discharge speed is controlled by the opening frequency and opening duration of the bottom gate valve, and finally transported to the product silo by the conveyor. Samples are taken at the bottom discharge port to detect the industrial analysis data of the pellets, and the discharge amount of the bottom pellets is adjusted according to the physical properties of the samples to regulate the activation reaction time of the pellets in the high temperature section.
[0046] Testing has determined that the average volatile matter of lignite pellets is 3.2%, the fixed carbon content exceeds 88%, the saturated sulfur capacity is 900 mg / g, and the grindability index of the crushed particles is 55%. Lignite pellets are not only a clean and high-quality carbonaceous material with performance exceeding that of coke powder and lignite powder currently used in sintering, but are also an excellent coal gas desulfurizer with performance close to that of activated carbon products used for desulfurization.
[0047] Step 4: The semi-coke pellets are further cooled in the storage bin, and the cooled semi-coke pellets are added to the moving bed adsorption tower as an adsorbent for blast furnace gas fine desulfurization. The blast furnace gas contacts the semi-coke pellet adsorbent moving downward in the adsorption tower from bottom to top in countercurrent, ensuring that the H2S concentration in the outlet gas is less than 20 mg / m 3 The H2S concentration is detected online. If the concentration exceeds the emission limit, the emission frequency of the blue carbon pellet adsorbent in the adsorption tower is accelerated. The adsorption saturated blue carbon pellets discharged from the adsorption tower are crushed and sieved using a double roll crusher. The 3mm oversize particles are returned to the crushing equipment for re-crushing, and the fine particles below 3mm are collected and used for iron ore powder sintering.
[0048] Example 2
[0049] Step 1, weighing and mixing blue carbon powder, corn starch, coal tar and waste activated carbon powder in a mass ratio of 88:2:4:6, and then kneading them evenly in a kneader at room temperature;
[0050] Step 2, adding the mixture obtained in step 1 into the silo of a roller pelletizer, and pressing into 50×16×12 mm oval pellets under a line pressure of 20 t / cm;
[0051] Step 3, the blue charcoal pellet product obtained in step 2 is transferred to the top silo of the internal heating carbonization furnace, and evenly added to the heating vertical furnace through the silo valve. The blue charcoal pellets are gradually heated from room temperature to 700°C from top to bottom in the vertical furnace, and the temperature is kept constant for about 2 hours in the high temperature section. Water vapor is sprayed into the constant temperature section of the vertical furnace to react with the blue charcoal pellets at high temperature. Part of the carbon in the blue charcoal pellets reacts with water vapor, and the pellets obtain a large specific surface area. After activation, the pellets enter the cooling section of the vertical furnace and are cooled to 150°C. The cooled pellets are discharged from the bottom of the vertical furnace. The discharge speed is controlled by the opening frequency and opening duration of the bottom gate valve, and finally transported to the storage bin for storage. The industrial analysis data of the pellets is sampled and tested at the bottom discharge port of the furnace, and the discharge amount of the bottom pellets is adjusted according to the volatile matter data of the sample. The test data of semi-coke pellets show that the grindability index of the sample reaches 60%, the average volatile matter is 4.0%, the fixed carbon content exceeds 86%, and the saturated sulfur capacity is 750 mg / g, which can meet the technical requirements of blast furnace gas desulfurization and iron ore powder sintering.
[0052] Step 4: The semi-coke pellets are further cooled in the silo, and the cooled semi-coke pellets are added to the moving bed adsorption tower as a desulfurizer for blast furnace gas to adsorb H2S. The semi-coke pellets saturated with adsorption in the adsorption tower are discharged and enter the multi-stage toothed roller crusher for crushing and screening, of which the 3mm oversize particles are returned to the crushing equipment for re-crushing, and the fine particles below 3mm are collected and used for iron ore powder sintering.
[0053] Example 3
[0054] Step 1, weighing and mixing blue carbon powder, metallurgical coke powder, corn starch and humic acid in a mass ratio of 78:15:2:5, and then kneading them in a kneader at room temperature to ensure that the two binders are evenly distributed in the blue carbon powder, and the mixed materials are further compacted in a wheel mill to facilitate subsequent molding and ball pressing;
[0055] Step 2, adding the mixture obtained in step 1 into the silo of a roller pelletizer, and pressing into conical pellets of 25×25×18 mm under a line pressure of 8 t / cm;
[0056] Step 3, the semi-coke pellet product obtained in step 2 is transferred to the top silo of the external heating vertical furnace, and evenly added into the vertical furnace through the silo valve. The semi-coke pellets are gradually heated from room temperature to 1000°C from top to bottom in the vertical furnace, and the high-temperature constant temperature heating time is controlled to about 5h. The steam nozzle set in the high-temperature furnace section continuously sprays low-pressure steam to the pellets, so that the semi-coke pellets undergo activation reaction, achieving the purpose of pore formation and increasing specific surface area. After activation, the pellets enter the cooling section at the bottom of the carbonization furnace and are cooled to 150°C, and then discharged from the bottom of the carbonization furnace and transported to the storage silo by the high-temperature conveyor. The discharge speed is controlled by the opening frequency and duration of the bottom gate valve. The industrial analysis data of the pellets is sampled and tested at the furnace bottom discharge port, and the discharge amount of the furnace bottom pellets is adjusted according to the volatile matter data of the sample. The test determined that the average volatile matter of the lignite pellets was 1.5%, the fixed carbon content exceeded 90%, the grindability index was 49%, and the saturated sulfur capacity was 1100 mg / g. The pellets had excellent adsorption properties, but the grindability index was low.
[0057] Step 4: The cooled semi-coke pellets are added to the moving bed adsorption tower as an adsorbent for blast furnace gas fine desulfurization. The blast furnace gas contacts the semi-coke pellet adsorbent moving downward in the adsorption tower from bottom to top in countercurrent, ensuring that the H2S concentration in the outlet gas is less than 20 mg / m 3 The H2S concentration is detected online. If the concentration exceeds the emission limit, the emission frequency of the blue carbon pellet adsorbent in the adsorption tower is accelerated. After adsorption saturation, the blue carbon pellets are crushed, and fine particles below 3mm are collected and screened and mixed with iron ore powder, lime powder, etc., and then sintered in the sintering machine. The hydrogen sulfide adsorbed by the blue carbon powder is converted into sulfur dioxide during sintering, and is finally captured and treated by the tail gas treatment system of the sintering machine.
[0058] Example 4
[0059] The same as Example 3, except that, in step 1, the semi-coke powder, metallurgical coke powder, corn starch and humic acid are weighed and prepared in a mass ratio of 82:15:2:1, and then kneaded in a kneader at room temperature to ensure that the two binders are evenly distributed in the semi-coke powder, and the mixed material is further compacted in a wheel mill to facilitate subsequent molding and ball pressing.
[0060] Example 5
[0061] The same as Example 3, except that, in step 1, the semi-coke powder, metallurgical coke powder, corn starch and humic acid are weighed and prepared in a mass ratio of 87:5:2:6, and then kneaded in a kneader at room temperature to ensure that the two binders are evenly distributed in the semi-coke powder. The mixed material is further compacted in a wheel mill to facilitate subsequent molding and ball pressing.
[0062] Example 6
[0063] The same as Example 1, except that, in step 1, the blue carbon powder, anthracite powder, caking coal powder (fat coal powder) and slaked lime powder are weighed and mixed in a mass ratio of 70:10:3.6:6.4, and then kneaded evenly in a kneader at room temperature to obtain a mixture.
[0064] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
Claims
1. A method for preparing a coal gas desulfurizer by activating blue carbon powder after molding, characterized in that: The following steps are involved: The uniformly mixed semi-coke powder, carbon raw material, binder and additive are pressed and formed to obtain semi-coke pellets with regular shapes; The semi-coke pellets are heated to 800-1000°C, and activated by water vapor for 1-6 hours to obtain a coal gas desulfurizer.
2. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: The carbonaceous raw material is a mixture of one or more of anthracite, bituminous coal, metallurgical coke powder, waste activated coke and waste activated carbon.
3. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: The added amount of the carbonaceous raw material shall not exceed 15% of the total weight of the blue carbon powder, the carbonaceous raw material, the binder and the additive.
4. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: The binder is any two or more of starch, coal tar, adhesive coal powder, coal tar and humic acid.
5. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: The amount of binder added is 3-8% of the total weight of the blue charcoal powder and the carbonaceous raw material.
6. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: One or both of boric acid and slaked lime powder.
7. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: The amount of additive added shall not exceed 5% of the total weight of the blue carbon powder and the carbonaceous raw materials.
8. The method for preparing a coal gas desulfurizing agent by activating blue carbon powder after molding according to claim 1, characterized in that: The shape of the semi-coke pellets is pillow-shaped, ellipsoidal or oval, and the three-dimensional size of the semi-coke pellets is between 15-50mm.
9. Use of the semi-coke powder prepared by the method according to any one of claims 1 to 8, which is then activated to prepare a coal gas desulfurizing agent in removing hydrogen sulfide from blast furnace gas.
10. Use of semi-coke powder prepared by the method according to any one of claims 1 to 8 as a coal gas desulfurizer after being formed and activated in iron ore powder sintering.
Citation Information
Patent Citations
Method of preparing active coke for desulfurization and denitrification of sintering flue gas by using semi-coke
CN106698423A
Preparation method of semi-coke powder-based columnar activated carbon
CN108751193A
Preparation method of carbonized sludge particles for iron ore powder sintering additives
CN111074067A
Preparation method of active coke
CN112456489A