Modified silica gel as well as preparation method and application thereof
Through the preparation method of modified silica gel, the porosity and coating of silica gel are improved by using surfactants, fluorides, TRIS and sodium alginate, which solves the problem of insufficient adsorption performance of silica gel and achieves carbon dioxide and VOC Excellent adsorption effect and purification and treatment of wastewater.
Patent Information
- Application Number
- CN202410968184.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The application of existing silicone in the adsorption field is limited by its poor selectivity and adsorption capacity, especially the reduction in adsorption performance after use, which limits the recycling of waste silicone. The modified silicone adsorbent is mainly used for aldehydes and ketones. Not suitable for widespread applications.
By soaking the waste silica gel in a solution containing surfactant, then reacting with the desulfurization wastewater containing fluoride, then adding sodium alginate to the TRIS solution, and soaking in the desulfurization wastewater containing calcium chloride and magnesium chloride, the modification is formed Silicone, which uses fluorine, TRIS and sodium alginate to improve the porosity and coating of silica gel, and enhances its adsorption performance and stability.
The modified silica gel produced has excellent adsorption effect on carbon dioxide and VOC, and is purified in wastewater treatment, improving the stability and mechanical strength of silica gel, and is suitable for a wide range of gas adsorption applications.
Smart Images

Figure BDA0004952330070000091 
Figure BDA0004952330070000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of power plant desulfurization wastewater treatment and silica gel modification, in particular to a modified silica gel and a preparation method and application thereof. Background Art
[0002] Silica gel is an amorphous substance with rich pore structure, which can be used as an adsorption material. After being discarded, silica gel can be recycled through mechanical recycling and chemical recycling. Among them, the mechanical recycling method is to crush the discarded silica gel into fragments or powder, filter through a sieve, wash, and dry it for recycling; the chemical recycling method is to decompose silica gel into basic materials through chemical methods such as acid-base catalytic cracking, ultrasonic cracking, and thermal cracking, and then recycle it.
[0003] The adsorption characteristics of silica gel mainly come from the abundant silanol groups on its surface. Due to the poor adsorption selectivity and adsorption capacity, the application of silica gel in the adsorption field is greatly limited; in particular, the adsorption performance of silica gel after use is significantly reduced, which is not conducive to the recycling of waste silica gel. CN 111468068A discloses a modified silica gel adsorbent, which is grafted with terminal amino hyperbranched polyamide amine on silica gel to make the silica gel surface contain sufficient terminal amino groups, and then produce condensation reaction with aldehydes and ketones to capture and fix a large number of volatile substances of aldehydes and ketones; however, the above-mentioned modified silica gel adsorbent is mainly used for adsorbing aldehydes and ketones, which is not conducive to the wide application of the adsorbent.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a modified silica gel and a preparation method and application thereof, which can achieve purification of desulfurization wastewater while modifying waste silica gel, and the prepared modified silica gel has excellent adsorption effect on carbon dioxide and VOC.
[0006] The present invention provides a method for preparing modified silica gel, comprising the following steps:
[0007] S1: soaking the waste silica gel in a solution containing a surfactant, and washing it after soaking to obtain a silica gel raw material;
[0008] S2: reacting the silica gel raw material with the desulfurization wastewater containing fluoride, and taking it out after the reaction to obtain pretreated silica gel;
[0009] S3: soaking the pretreated silica gel in a TRIS solution, adding sodium alginate to the TRIS solution and continuing to soak, taking it out after soaking, and obtaining a coated silica gel;
[0010] S4: Soaking the coated silica gel in desulfurization wastewater containing calcium chloride and magnesium chloride, and drying after soaking to obtain modified silica gel.
[0011] In step S1, the solution containing a surfactant includes laundry detergent and water, and the mass ratio of the laundry detergent to water in the solution is 1: (80-120); soaking is performed under oscillation or stirring conditions, and the soaking time is 2-4 days; during soaking, the mass ratio of the waste silica gel to the solution containing a surfactant can be 1: (50-150); in addition, cleaning after soaking includes brushing and soaking with tap water or oscillating cleaning. Studies have shown that soaking the waste silica gel with a solution containing laundry detergent can clean and open the blocked internal pores of the waste silica gel, which is beneficial to improving the subsequent modification effect of the silica gel raw material.
[0012] In step S2, the mass content of fluoride in the desulfurization wastewater is 10-30 mg / L; the reaction is carried out under stirring conditions, the reaction temperature is room temperature, and the reaction time is 2-4 days; during the reaction, the mass ratio of the silica gel raw material to the desulfurization wastewater containing fluoride can be 1: (200-400). Studies have shown that reacting the silica gel raw material with the desulfurization wastewater containing fluoride can use the fluorine element and its composition to drill holes inside the silica gel raw material, which is beneficial to improving the subsequent modification effect of the silica gel raw material and can effectively remove the fluoride in the desulfurization wastewater.
[0013] In step S3, the mass content of TRIS (trishydroxymethylaminomethane) in the TRIS solution is 5-12%; the immersion is carried out under stirring conditions for 0.5-1.5 hours; during the immersion, the mass ratio of the pretreated silica gel to the TRIS solution can be 1: (200-300). In addition, sodium alginate is added to make the mass content of sodium alginate in the TRIS solution 2-5%; the immersion is continued under stirring conditions for 2-4 hours. Soaking the pretreated silica gel in the TRIS solution is conducive to TRIS entering the internal pores of the pretreated silica gel, which is conducive to improving the adsorption performance of the modified silica gel; adding sodium alginate is conducive to forming a coating film on the surface of the pretreated silica gel, thereby improving the stability of the modified silica gel in structure and adsorption performance.
[0014] In step S4, the mass content of calcium chloride in the desulfurization wastewater is 10-20 mg / L, and the mass content of magnesium chloride is 5-15 mg / L; soaking is carried out under stirring conditions, and the soaking time is 8-12 hours; during soaking, the mass ratio of the coated silica gel to the desulfurization wastewater containing calcium chloride and magnesium chloride can be 1: (200-400); the desulfurization wastewater can use the supernatant of the desulfurization wastewater after the reaction in step S2. In addition, the drying temperature is 35-45°C, and the drying time is 6-12 hours. The coated silica gel is soaked in the desulfurization wastewater containing calcium chloride and magnesium chloride, and the water retention of chloride ions and TRIS are used to form a liquid-solid intermediate state, which significantly improves the modification effect; at the same time, the coating film formed by sodium alginate coating can adsorb calcium ions and heavy metal ions in the desulfurization wastewater, greatly improving the ionic strength of the coating film, and enhancing the mechanical strength of the coating film, further improving the stability of the modified silica gel.
[0015] The invention also provides a modified silica gel, which is prepared according to the preparation method.
[0016] The present invention also provides the application of modified silica gel in gas adsorption; there is no strict restriction on the adsorbed gas, including but not limited to carbon dioxide, VOC and the like.
[0017] The present invention soaks the waste silica gel in a solution containing a surfactant to open the blocked internal pores of the waste silica gel; the desulfurization wastewater containing fluoride reacts with the silica gel raw material, and the fluorine element and its composition are used to drill holes in the silica gel raw material, which is beneficial to improving the subsequent modification effect of the silica gel raw material; the pre-treated silica gel is soaked in a TRIS solution, which is beneficial for TRIS to enter the internal pores of the pre-treated silica gel and improve the adsorption performance of the modified silica gel; the addition of sodium alginate is beneficial for coating the surface of the pre-treated silica gel to form a coating film; the desulfurization wastewater containing calcium chloride and magnesium chloride is used to soak the coated silica gel, which can not only use the water retention of chloride ions to work with TRIS to form a liquid-solid intermediate state, but also enable the coating film to adsorb calcium ions and heavy metals in the desulfurization wastewater to improve the mechanical strength, greatly improve the stability of the modified silica gel, and realize the purification of the desulfurization wastewater while modifying the waste silica gel, and the prepared modified silica gel has an excellent adsorption effect on carbon dioxide and VOC. DETAILED DESCRIPTION
[0018] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0019] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0020] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] The preparation method of the modified silica gel of this embodiment comprises the following steps:
[0023] S1: Cleaning
[0024] Mix Blue Moon laundry detergent and water in a mass ratio of 1:100 to obtain a cleaning solution.
[0025] The waste silica gel was soaked in the above cleaning solution, the mass ratio of the waste silica gel to the cleaning solution was 1:100, and the soaking was carried out under stirring conditions for 3 days.
[0026] After soaking, the waste silica gel is first scrubbed with a brush, then soaked in tap water for shaking cleaning, and taken out after cleaning to obtain silica gel raw material.
[0027] S2: Preprocessing
[0028] Take desulfurization wastewater (i.e. desulfurization wastewater before treatment), and its main composition is shown in Table 1.
[0029] The silica gel raw material is reacted with the above-mentioned desulfurization wastewater, the mass ratio of the silica gel raw material to the desulfurization wastewater is 1:200, the reaction is carried out under stirring conditions, the reaction temperature is room temperature, and the reaction time is 3 days; after the reaction, the silica gel raw material is taken out to obtain pretreated silica gel; in addition, the desulfurization wastewater after the reaction is precipitated, and the supernatant is taken out for standby use after precipitation.
[0030] S3: Wrapping
[0031] TRIS was dissolved in water to prepare a TRIS solution with a mass content of 8%.
[0032] The pretreated silica gel was soaked in the above TRIS solution, the mass ratio of the pretreated silica gel to the TRIS solution was 1:200, and the soaking was carried out under stirring for 1 hour.
[0033] After soaking, sodium alginate was added to the TRIS solution to make the mass content of sodium alginate in the TRIS solution be 3%. The solution was soaked for 3 hours under stirring and then taken out to obtain coated silica gel.
[0034] S4: Modification
[0035] The coated silica gel is soaked in the supernatant of the desulfurization wastewater after the reaction in step S2, the mass ratio of the coated silica gel to the supernatant is 1:200, and the soaking is carried out under stirring for 10 hours. The main composition of the desulfurization wastewater after soaking (i.e., the treated desulfurization wastewater) is shown in Table 1.
[0036] After soaking, the mixture was dried at 40°C for 8 h to obtain modified silica gel.
[0037] Table 1 Main composition of desulfurization wastewater before and after treatment
[0038] Desulfurization wastewater Fluoride content Calcium chloride content Magnesium chloride content Desulfurization wastewater before treatment 14.4mg / L 19.1mg / L 12.2mg / L Treated desulfurization wastewater 9.2mg / L 9.5mg / L 7.4mg / L
[0039] Example 2
[0040] The preparation method of the modified silica gel of this embodiment comprises the following steps:
[0041] S1: Cleaning
[0042] Mix Blue Moon laundry detergent and water in a mass ratio of 1:80 to obtain a cleaning solution.
[0043] The waste silica gel was soaked in the above cleaning solution, the mass ratio of the waste silica gel to the cleaning solution was 1:100, and the soaking was carried out under stirring conditions for 2 days.
[0044] After soaking, the waste silica gel is first scrubbed with a brush, then soaked in tap water for shaking cleaning, and taken out after cleaning to obtain silica gel raw material.
[0045] S2: Preprocessing
[0046] The silica gel raw material is reacted with the desulfurization wastewater of Example 1, the mass ratio of the silica gel raw material to the desulfurization wastewater is 1:200, the reaction is carried out under stirring conditions, the reaction temperature is room temperature, and the reaction time is 2 days; after the reaction, the silica gel raw material is taken out to obtain pretreated silica gel; in addition, the desulfurization wastewater after the reaction is precipitated, and the supernatant is taken out for standby use after precipitation.
[0047] S3: Wrapping
[0048] TRIS was dissolved in water to prepare a TRIS solution with a mass content of 5%.
[0049] The pretreated silica gel was soaked in the above TRIS solution, the mass ratio of the pretreated silica gel to the TRIS solution was 1:200, and the soaking was carried out under stirring for 1.5 hours.
[0050] After soaking, sodium alginate was added to the TRIS solution to make the mass content of sodium alginate in the TRIS solution be 2%, and the solution was soaked for 4 hours under stirring. After soaking, the solution was taken out to obtain coated silica gel.
[0051] S4: Modification
[0052] The coated silica gel is soaked in the supernatant of the desulfurization wastewater after the reaction in step S2, the mass ratio of the coated silica gel to the supernatant is 1:200, and the soaking is carried out under stirring for 8 hours.
[0053] After soaking, the mixture was dried at 45°C for 6 hours to obtain modified silica gel.
[0054] Example 3
[0055] The preparation method of the modified silica gel of this embodiment comprises the following steps:
[0056] S1: Cleaning
[0057] Mix Blue Moon laundry detergent and water in a mass ratio of 1:120 to obtain a cleaning solution.
[0058] The waste silica gel was soaked in the above cleaning solution, the mass ratio of the waste silica gel to the cleaning solution was 1:100, and the soaking was carried out under stirring conditions for 4 days.
[0059] After soaking, the waste silica gel is first scrubbed with a brush, then soaked in tap water for shaking cleaning, and taken out after cleaning to obtain silica gel raw material.
[0060] S2: Preprocessing
[0061] The silica gel raw material is reacted with the desulfurization wastewater of Example 1, the mass ratio of the silica gel raw material to the desulfurization wastewater is 1:200, the reaction is carried out under stirring conditions, the reaction temperature is room temperature, and the reaction time is 4 days; after the reaction, the silica gel raw material is taken out to obtain pretreated silica gel; in addition, the desulfurization wastewater after the reaction is precipitated, and the supernatant is taken out for standby use after precipitation.
[0062] S3: Wrapping
[0063] TRIS was dissolved in water to prepare a TRIS solution with a mass content of 12%.
[0064] The pretreated silica gel was soaked in the above TRIS solution, the mass ratio of the pretreated silica gel to the TRIS solution was 1:200, and the soaking was carried out under stirring for 0.5 h.
[0065] After soaking, sodium alginate was added to the TRIS solution to make the mass content of sodium alginate in the TRIS solution be 5%, and the solution was soaked for 2 hours under stirring. After soaking, the solution was taken out to obtain coated silica gel.
[0066] S4: Modification
[0067] The coated silica gel is soaked in the supernatant of the desulfurization wastewater after the reaction in step S2, the mass ratio of the coated silica gel to the supernatant is 1:200, and the soaking is carried out under stirring for 12 hours.
[0068] After soaking, the mixture was dried at 35°C for 12 h to obtain modified silica gel.
[0069] Comparative Example 1
[0070] Except for the cleaning solution in step S1, the rest is the same as that in embodiment 1.
[0071] The preparation method of the cleaning solution of this comparative example includes: uniformly mixing a quaternary ammonium salt surfactant and water at a mass ratio of 1:100 to obtain a cleaning solution.
[0072] Comparative Example 2
[0073] Except for the cleaning solution in step S1, the rest is the same as that in embodiment 1.
[0074] The preparation method of the cleaning solution of this comparative example includes: uniformly mixing the AES surfactant and water at a mass ratio of 1:100 to obtain a cleaning solution.
[0075] Comparative Example 3
[0076] The process is the same as that of Example 1 except that the pretreatment in step S2 is not performed and the silica gel raw material in step S1 is directly immersed in the TRIS solution in step S3.
[0077] Comparative Example 4
[0078] Except that step S3 does not use TRIS solution for soaking, the rest is the same as embodiment 1.
[0079] Step S3 of this comparative example is:
[0080] Sodium alginate was dissolved in water to prepare a sodium alginate solution with a mass content of 3%.
[0081] The pretreated silica gel was immersed in the sodium alginate solution, the mass ratio of the pretreated silica gel to the sodium alginate solution was 1:200, and the immersion was carried out under stirring for 3 hours; after immersion, the silica gel was taken out to obtain coated silica gel.
[0082] Comparative Example 5
[0083] Except that sodium alginate is not added in step S3, the rest is the same as Example 1.
[0084] Step S3 of this comparative example is:
[0085] TRIS was dissolved in water to prepare a TRIS solution with a mass content of 8%.
[0086] The pretreated silica gel was immersed in the above TRIS solution, the mass ratio of the pretreated silica gel to the TRIS solution was 1:200, and the immersion was carried out under stirring for 4 hours; after immersion, the silica gel was taken out to obtain coated silica gel.
[0087] Comparative Example 6
[0088] Except that the improvement of step S4 is not performed, the rest is the same as that of embodiment 1.
[0089] Comparative Example 7
[0090] Except that sodium chloride solution is used to replace the supernatant of the desulfurization wastewater after the reaction in step S2 in step S4, the rest is the same as Example 1; the content of chloride ions in the sodium chloride solution is controlled to be the same as the content of chloride ions in the supernatant of the desulfurization wastewater after the reaction in step S2.
[0091] Comparative Example 8
[0092] Except that a mixed solution containing calcium nitrate and magnesium nitrate is used in step S4 to replace the supernatant of the desulfurization wastewater after the reaction in step S2, the rest is the same as Example 1; the content of calcium ions and the content of magnesium ions in the mixed solution are controlled to be the same as the content of calcium ions and the content of magnesium ions in the supernatant of the desulfurization wastewater after the reaction in step S2.
[0093] Test Example 1
[0094] The modified silica gel prepared in each embodiment and control example was used as an adsorbent to carry out a gas adsorption test; the gas adsorption test method is as follows:
[0095] The test was conducted in a 30 cubic sealed test chamber. The initial carbon dioxide content in the test chamber before adsorption was 500ppm and the initial VOC content was 1.0mg / m 3 ; at 300m 3 The contents of carbon dioxide and VOC after adsorption for 1 h at an air volume of / h are shown in Table 2.
[0096] Table 2 Adsorption effect test results of various modified silica gels
[0097]
[0098]
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing modified silica gel, characterized in that: The steps include: S1: soaking the waste silica gel in a solution containing a surfactant, and washing it after soaking to obtain a silica gel raw material; S2: reacting the silica gel raw material with the desulfurization wastewater containing fluoride, and taking it out after the reaction to obtain pretreated silica gel; S3: soaking the pretreated silica gel in a TRIS solution, adding sodium alginate to the TRIS solution and continuing to soak, taking it out after soaking, and obtaining a coated silica gel; S4: Soaking the coated silica gel in desulfurization wastewater containing calcium chloride and magnesium chloride, and drying after soaking to obtain modified silica gel.
2. The preparation method according to claim 1, characterized in that: In step S1, the solution containing a surfactant includes laundry detergent and water, and the mass ratio of the laundry detergent to water in the solution is 1:(80-120); soaking is performed under oscillation or stirring conditions, and the soaking time is 2-4 days.
3. The preparation method according to claim 1, characterized in that: In step S2, the mass content of fluoride in the desulfurization wastewater is 10-30 mg / L; the reaction is carried out under stirring conditions, the reaction temperature is room temperature, and the reaction time is 2-4 days.
4. The preparation method according to claim 1, characterized in that: In step S3, the mass content of TRIS in the TRIS solution is 5-12%; the immersion is performed under stirring for 0.5-1.5 hours.
5. The preparation method according to claim 1, characterized in that: In step S3, sodium alginate is added to make the mass content of sodium alginate in the TRIS solution be 2-5%; and the immersion is continued under stirring for 2-4 hours.
6. The preparation method according to claim 1, characterized in that: In step S4, the mass content of calcium chloride in the desulfurization wastewater is 10-20 mg / L, and the mass content of magnesium chloride is 5-15 mg / L; the soaking is carried out under stirring conditions for 8-12 hours.
7. The preparation method according to claim 1, characterized in that: In step S4, the drying temperature is 35-45° C. and the drying time is 6-12 hours.
8. A modified silica gel, characterized in that: Prepared according to the preparation method described in any one of claims 1 to 7.
9. Use of the modified silica gel according to claim 8 in gas adsorption.
10. The use according to claim 9, characterized in that: Gases include carbon dioxide and VOCs.
Citation Information
Patent Citations
Preparation method of spherical calcium-based CO2 adsorbent
CN106000301A
Production method of modified pressure swing adsorption silica gel
CN106276926A
Efficient active ore capable of adsorbing a variety of gases
CN107308916A
Modified silica gel CO2 adsorbent and preparation method and application thereof
CN111298763A