Copper-zirconium bi-component catalyst prepared by flame jet cracking method as well as catalyst and application thereof

The copper-zirconium catalyst is prepared in one step by single flame and double flame jetting, which solves the problem of difficult regulation of the interaction between copper-zirconium components in the prior art, and realizes the preparation of a high-active catalyst, simplifies the process and reduces costs.

CN118904338APending Publication Date: 2024-11-08DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310505475.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing copper-zirconium catalyst preparation methods are difficult to flexibly regulate the interaction of copper-zirconium components, resulting in unstable catalytic activity, and the preparation process is complex and costly, which easily leads to the agglomeration of metal particles and unnecessary steps of high-temperature heat treatment procedures.

Method used

The copper-zirconium two-component catalyst is prepared in one step by single flame and double flame jet cracking. By regulating the combustion parameters of the nozzle, the valence state and particle size of the copper components are accurately controlled, and the sintering and aggregation are avoided, forming a highly active copper-zirconium interface, simplifying Preparation process.

Benefits of technology

The high activity and excellent performance of the copper-zirconium catalyst are achieved, the preparation process is simplified, the cost and operation complexity is reduced, multiple steps of high-temperature heat treatment is avoided, and the stability and performance of the catalyst are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004215496610000111
    Figure BDA0004215496610000111
  • Figure BDA0004215496610000121
    Figure BDA0004215496610000121
  • Figure BDA0004215496610000122
    Figure BDA0004215496610000122
Patent Text Reader

Abstract

The invention provides the copper-zirconium bi-component catalyst prepared in one step by single-flame and double-flame jet cracking methods, the copper component presents different valence states and particle sizes, and the copper-zirconium bi-component catalyst has the advantages that (1) one-step combustion, rapid forming and continuous preparation are realized, and subsequent treatment is not needed; (2) the size and valence state of copper particles in the copper-zirconium bi-component catalyst after hydrogen reduction can be regulated and controlled by adjusting flame parameters of the single nozzle and the double nozzles; (3) simultaneously adjusting the particle sizes of copper and zirconium components through a single nozzle; (4) copper and zirconium components are respectively controlled by double nozzles, so that the valence state and the particle size of the copper component can be accurately regulated and controlled without influencing the zirconium component; (5) the copper zirconium oxide has the characteristics of active lattice oxygen, high dispersion and large specific surface area through ultrahigh-temperature combustion and instantaneous quenching of a flame jet method; and (6) two-step preparation is simplified into one step, the preparation process is simple and rapid, subsequent high-temperature roasting treatment is not needed, and energy conservation and emission reduction are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a copper-zirconium dual-component catalyst in one step by a flame jet cracking method. The instant high-temperature quenching process of the method avoids the sintering and aggregation of copper, promotes the strong interaction between copper and zirconium oxide, and generates new high-valent copper active species. By adjusting the working parameters of a single nozzle and a double nozzle device, the single nozzle can simultaneously adjust the copper-zirconium dual components, and the double nozzle adjusts the copper component without affecting the zirconium component. After hydrogen reduction, the valence state and particle size of copper particles are adjusted to form a high-activity copper-zirconium interface, and more excellent performance is shown in the carbon dioxide hydrogenation to methanol reaction. Background Art

[0002] Since the Industrial Revolution, excessive burning of fossil fuels has led to massive emissions of greenhouse gas CO2, causing irreversible damage to the global climate. Therefore, the recycling of carbon resources has attracted increasing attention. Using solar energy to electrolyze water to produce hydrogen, the "green hydrogen" obtained converts CO2 into methanol, which can effectively use renewable energy to fix carbon, forming the concept of "liquid sunshine" and gradually gaining popularity. In recent years, CO2 hydrogenation to methanol technology has been vigorously developed, which not only reduces dependence on fossil fuels, but also produces methanol, which is also one of the important industrial raw materials. The annual world demand is 50 million tons, making the carbon dioxide hydrogenation to methanol route of great research significance.

[0003] Studies have shown that among the many catalysts for hydrogenating carbon dioxide to methanol, copper-based catalysts have mild reaction conditions, are economical and efficient, and have attracted much attention. It is currently believed that the particle size of copper directly affects the catalytic activity (Chinese Patent 201410141351.4; Chinese Patent 201510695863.X), and zirconium oxide as a functional carrier can activate carbon dioxide, especially tetragonal zirconium oxide can stabilize monovalent active copper species (Chinese Patent 202110010231.0), and the highly active copper-zirconium reaction active interface promotes the synthesis of methanol. However, copper has a high structural sensitivity. Traditional methods such as impregnation, precipitation, hydrothermal synthesis, sol-gel and citric acid complexation are difficult to regulate the structure of the copper component due to the limitations of the preparation method itself, which easily causes changes in other components of the catalyst (Chinese Patent 202011043607.X), and cannot guarantee flexible regulation of the interaction between the copper-zirconium components; and the operation is complicated, the preparation cycle is long, the equipment investment and production operation costs are high, and the multi-step high-temperature heat treatment procedure is also prone to cause particle agglomeration.

[0004] The flame spray pyrolysis method is a new type of multifunctional nanomaterial preparation method developed in recent years. The whole process is simple and fast, with only two steps: precursor mixing and flame combustion. The preparation cycle is short, easy to scale up, and there is no subsequent heat treatment process and washing and separation process, saving investment and operating costs (Chinese Patent 201611098884.4; Chinese Patent 201711249629.X; Chinese Patent 202011537955.2). Moreover, the zirconium oxide prepared by the flame spray method has a high-purity, highly active, metastable tetragonal phase structure (Chinese Patent 202110010231.0), which is conducive to the synthesis of methanol on a copper zirconium catalyst. In addition, the single-nozzle flame spraying method can simultaneously regulate the structure of the copper-zirconium dual components; the improved dual-nozzle flame spraying device can directionally regulate the structure and valence of the copper component while keeping the zirconium component structure unchanged, without introducing unnecessary operating steps, thereby strengthening the targeted regulation of the target component and avoiding the influence of factors such as metal particle size and specific surface area on the multi-step preparation method to reduce activity, thereby further optimizing the catalyst performance. Summary of the invention

[0005] The present invention provides a copper-zirconium dual-component catalyst prepared in one step by a single flame and a double flame spray cracking method, wherein the copper component presents different valence states and particle sizes, and the valence state and particle size of the copper component in the catalyst can be changed by regulating the combustion parameters of the single flame and the double flame. The single nozzle changes the copper-zirconium dual components at the same time to complete the regulation of the copper component; the double nozzle controls the copper-zirconium components separately, and the valence state and particle size of the copper component can be accurately regulated without affecting the zirconium component.

[0006] The operation steps and features are as follows:

[0007] The copper content in the catalyst is 5-60% by mass, preferably 10-30% by mass; the rest is zirconium oxide component;

[0008] (1) Preparation is carried out using a single flame nozzle or a double flame nozzle;

[0009] Single flame nozzle:

[0010] a. Mixing and dissolving the precursor compounds of copper and zirconium in an organic solvent according to the ratio required by the composition of the catalyst to form a copper-zirconium mixed solution;

[0011] b. Pumping the copper-zirconium mixed solution into a nozzle, the solution is sprayed out from the nozzle, dispersed into droplets by the dispersion gas, and introduced into the flame formed by the combustion gas flowing out of the air holes arranged around the outside of the nozzle to burn; oxides containing copper components and zirconium components are generated in the single flame nozzle, and the copper and zirconium oxides in the single flame nozzle are mixed during the flame combustion process;

[0012] Or, dual flame nozzle:

[0013] a. dissolving a copper precursor compound in an organic solvent to form a copper solution; dissolving a zirconium precursor compound in an organic solvent to form a zirconium solution;

[0014] b. The copper solution and the zirconium solution are pumped into two different nozzles respectively. The solutions are sprayed out from the two nozzles in the ratio required by the composition of the catalyst respectively. The solutions are dispersed into droplets by the dispersion gas respectively. The droplets are introduced into the flame formed by the combustion gas flowing out of the air holes arranged around the outer sides of the two nozzles respectively. The flames formed by the combustion gas flowing out of the air holes arranged around the outer sides of the two nozzles intersect at one end (flame tip area) away from the air holes to form a double flame intersection area. In the double flame nozzle, one flame nozzle produces an oxide containing a copper component, and the other flame nozzle produces an oxide containing a zirconium component. The oxides produced by the two flame nozzles of the double flame are collected in the double flame intersection area.

[0015] (2) Collect the catalyst particles formed after combustion.

[0016] (3) The single flame nozzle used: comprises a hollow tubular nozzle and a gas distribution plate, wherein the nozzle passes through the gas distribution plate from bottom to top and extends from the middle of the gas distribution plate, wherein the gas distribution plate around the nozzle outlet is provided with combustion gas outlet holes and dispersion gas outlet holes; the number of the combustion gas outlet holes is more than 2, and the combustion gas outlet holes are evenly distributed along the circumferential direction, the geometric center of the circumferential distribution of the combustion gas outlet holes is the geometric center of the nozzle outlet as the circle center and the radius is R1; the number of the dispersion gas outlet holes is more than 2, and the dispersion gas outlet holes are evenly distributed along the circumferential direction, the geometric center of the circumferential distribution of the dispersion gas outlet holes is the geometric center of the nozzle outlet as the circle center and the radius is R2, and R2 is greater than R1, the gas distribution plate around the nozzle inlet is provided with a combustion gas inlet and a dispersion gas inlet, and the combustion gas inlet is connected to the combustion gas outlet hole, and the dispersion gas inlet is connected to the dispersion gas outlet hole, and a cylindrical container B is provided on the air inlet side of the gas distribution plate, The cylindrical container B is sealed at one end and open at the other end, and the edges of the gas distribution plate are sealed and connected to the open end of the cylindrical container B. The cylindrical container B is provided with an air connection inlet connected to an air pump or an air compressor or an oxygen connection inlet connected to an oxygen source. A cylindrical container A is sealed at one end and open at the other end in the cylindrical container B, and the open end of the cylindrical container A is sealed and connected to the plate surface between the combustion gas outlet hole and the dispersion gas outlet hole on the gas distribution plate. The cylindrical container A is provided with a combustion gas connection inlet connected to the combustion gas source. The gas in the cylindrical container A enters each combustion gas inlet, and the gas in the cylindrical container B enters each dispersion gas inlet. At the same time, the cylindrical container A blocks the gas in the cylindrical container B from entering the combustion gas inlet. In addition, a pipeline is provided at the nozzle inlet, which passes through the cylindrical container A and the cylindrical container B and then pumps the organic precursor to be burned at a uniform speed with a liquid injection pump.

[0017] Alternatively, the double flame nozzle used includes the two single flame nozzles mentioned above, wherein the double nozzle spacing between the geometric centers of the two nozzles on the upper surface of the gas distribution plate of the two single flame nozzles is 1-30 cm, preferably 5-15 cm; the flame combustion angle formed by the axes of the two nozzle outlets is 10-120 degrees, preferably 45-90 degrees.

[0018] The combustion gas required for flame combustion is a mixture of methane and oxygen. The inner diameter of the combustion gas outlet is 1-10 mm. The sum of the radial cross-sectional areas of all through holes A on the gas distribution plate is 1-20 square centimeters. The flow rates of methane and oxygen are 0.1-5 L / min respectively.

[0019] The dispersed gas is air, the inner diameter of the dispersed gas outlet hole is 1-10 mm, the sum of the radial cross-sectional areas of all through holes B on the gas distribution plate is 1-20 square centimeters, and the dispersed gas flow rate is 2-20 L / min;

[0020] The inner diameter of the nozzle is 0.5-2.5 mm, and the speed of the solution pumping out is 0.1-20 ml / min.

[0021] R1 = 0.5-3 cm, R2 = 1-10 cm;

[0022] The outlet of the nozzle and the outlets of the through holes A and B face the same direction (upward or sideways upward).

[0023] (5) Preparation of copper-zirconium precursor solution: dissolving a precursor compound containing copper and zirconium in a solvent; injecting the prepared solution into a single flame nozzle at a uniform speed; igniting a combustion gas to form a flame, wherein the combustion gas required for flame combustion is a mixture of methane and oxygen; the dispersion gas is air, which is blown to the entire flame area from a gas distribution plate surrounding the nozzle and having gas through holes uniformly distributed on the surface; the solution is pumped into the flame, and the air disperses the solution at the injection needle port in the center of the nozzle into small mist droplets, which are introduced into the flame for combustion. The precursor compounds of each component are decomposed under the high temperature of the flame to form oxide particles, and the formed oxide particles leave the flame area driven by the air; the single flame nozzle completes the mixing of copper and zirconium oxides during the combustion process; and the catalyst powder formed after the aggregation is collected;

[0024] Or, dissolving a copper-containing precursor compound in a solvent; dissolving a zirconium-containing precursor compound in a solvent;

[0025] Pump the prepared solution into two nozzles of the double flame nozzle respectively;

[0026] The combustion gas is ignited to form a flame. The combustion gas required for flame combustion is a mixture of methane and oxygen. The dispersion gas is air and / or oxygen. The air is blown to the entire flame area from a gas distribution plate surrounding the nozzle and having gas through holes evenly distributed on the surface. The solution is pumped into the flame, and the air disperses the solution at the injection needle in the center of the nozzle into small mist droplets, which are introduced into the flame for combustion. The precursor compounds of each component are decomposed under the high temperature of the flame to form oxide particles, and the formed oxide particles leave the flame area driven by the air. The oxides produced by the two nozzles of the double flame are gathered in the flame tip area, and the catalyst powder formed after the gathering is collected.

[0027] The copper precursor compound is a compound soluble in a solvent, preferably one or more of copper acetate, copper citrate, copper acetylacetonate, copper nitrate, and copper (II) diethylhexanoate; the molar concentration of copper in the copper solution is 0.1-2 mol / L, preferably 0.1-0.5 mol / L;

[0028] The zirconium precursor compound is a compound that can be dissolved in a solvent, preferably one or more of zirconium n-butoxide, zirconium acetate, zirconium acetylacetonate, zirconium citrate, and zirconium diethylhexanoate, and the molar concentration of zirconium in the zirconium solution is 0.1-2 mol / L, preferably 0.1-0.5 mol / L;

[0029] The solvent is a combustible organic solvent, preferably one or more of methanol, ethanol, xylene, liquid hydrocarbons, and organic acids;

[0030] The total molar concentration of copper-zirconium metal ions in the copper-zirconium mixed solution is 0.01-2 mol / L, preferably 0.1-0.5 mol / L.

[0031] (6) A copper-zirconium two-component catalyst is used for hydrogenation of carbon dioxide to produce methanol by regulating the valence state of Cu through hydrogen reduction: before use, the catalyst needs to be subjected to hydrogen reduction treatment, the reduction temperature is 250-400°C, preferably 250-350°C, and the time is 0.5-4h, preferably 1-2h; after the catalyst is subjected to hydrogen reduction, the zirconium oxide remains unchanged, and the copper oxide is reduced to monovalent copper and zero-valent copper, and the proportion of monovalent copper in all copper contents reaches 10-30%, preferably 20-30%; the particle size of the copper particles is 1.5-7nm, preferably 1.5-5nm.

[0032] (7) The catalyst is used for the thermal catalytic synthesis of methanol from carbon dioxide and hydrogen, characterized in that: the hydrogenation reaction conditions are: the molar ratio of H2 to CO2 in the raw gas is 1-10, preferably 3-5, the reaction temperature is 150-300°C, preferably 180-250°C, the reaction pressure is 1.0-10.0 MPa, preferably 2.0-4.0 MPa, and the raw gas gas space velocity is 2040-24000 ml / (h·g cat ).

[0033] The advantages of the present invention are: (1) one-step combustion, rapid molding, continuous preparation, and no need for subsequent treatment; (2) by adjusting the flame parameters of the single nozzle and the double nozzle, the size and valence of the copper particles in the copper-zirconium two-component catalyst after hydrogen reduction can be controlled; (3) the single nozzle simultaneously adjusts the particle size of the copper-zirconium component; (4) the double nozzles control the copper-zirconium component separately, and the valence and particle size of the copper component can be accurately controlled without affecting the zirconium component; (5) after ultra-high temperature combustion and instantaneous quenching by the flame spray method, the copper-zirconium oxide has the characteristics of active lattice oxygen, high dispersion, and large specific surface area; (6) the two-step preparation is simplified to one step, the preparation process is simple and fast, no subsequent high-temperature roasting treatment is required, and energy saving and emission reduction are achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The X-ray diffraction patterns of the catalysts in Examples 1 and 2 and Comparative Example 1 are shown.

[0035] Figure 2 The X-ray diffraction patterns of the catalysts of Examples 3 and 4 are shown in FIG.

[0036] Figure 3 This is a graph showing the variation of the content of various copper species with reduction temperature during the reduction process of the sample in Example 1, which is fitted based on the X-ray absorption near-edge spectrum.

[0037] Figure 4 This is a schematic diagram of the single flame nozzle structure.

[0038] Figure 5 This is a schematic diagram of the double flame nozzle structure.

[0039] In the figure: 1 is the nozzle outlet, 2 is the combustion gas outlet, 3 is the dispersion gas outlet, 4 is the nozzle inlet, connected to the liquid injection pump, and the organic precursor to be burned is pumped in at a constant speed; 5 is the combustion gas inlet, 6 is the dispersion gas inlet, 7 is the distance between the two nozzles, and 8 is the flame combustion angle;

[0040] Table 1 shows the contents of each component on the catalyst of Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1, as well as the content of copper, particle size, and the proportion of monovalent copper after reduction.

[0041] Table 2 shows the contents of each component on the catalysts of Examples 3, 7, and 8, as well as the content of copper, particle size, and the proportion of monovalent copper after reduction.

[0042] Table 3 shows the ratio of monovalent copper after different reduction on the catalyst of Example 1 and Comparative Example 1.

[0043] Table 4 shows the effects of Examples 1, 3, 4, 6, and 8 on the catalyst of Comparative Example 1 to produce methanol by hydrogenation of carbon dioxide.

[0044] Table 5 shows the effect of space velocity on the catalyst of Example 1 on the performance of the carbon dioxide hydrogenation to methanol reaction DETAILED DESCRIPTION

[0045] The technical details of the present invention are described in detail by the following examples. It should be noted that the examples are only used to further illustrate the technical features of the present invention, rather than to limit the present invention.

[0046] like Figure 4 As shown, the single flame nozzle used includes a hollow tubular nozzle and a circular gas distribution plate, the nozzle outlet 1 passes through the gas distribution plate from bottom to top and extends from the middle of the gas distribution plate, and circular through holes A as combustion gas outlet holes 2 and circular through holes B as dispersion gas outlet holes 3 are opened on the gas distribution plate around the nozzle; the number of through holes A is 20, and the combustion gas outlet holes 2 are evenly distributed along the circumferential direction, that is, on the upper surface of the gas distribution plate, the geometric center of the 20 through holes A is evenly distributed on the circumference of a circle with the same radius R1 (R1 = 1.5 cm) with the geometric center of the nozzle as the center;

[0047] The number of through holes B is 40, and the dispersed gas outlet holes 3 are evenly distributed along the circumferential direction, that is, on the upper surface of the gas distribution plate, the geometric center of the 40 through holes B is evenly distributed along the circumference of the same radius R2 (R2 = 5 cm) with the geometric center of the nozzle as the center of the circle;

[0048] A cylindrical container B with one end sealed and the other end open is provided at the inlet end of the gas through hole of the gas distribution plate. The edges of the gas distribution plate are sealed and connected to the open end of the cylindrical container B. A gas inlet connected to an air compressor or an oxygen source is provided on the cylindrical container B.

[0049] A cylindrical container A is provided in the cylindrical container B, one end of which is sealed and the other end is open. The open end of the cylindrical container A is tightly connected to the lower surface of the plate between the through holes A and B of the gas distribution plate. A combustion gas inlet connected to a combustion gas source is provided on the cylindrical container A.

[0050] The inlet of the nozzle is connected to the outlet of the syringe;

[0051] The combustion gas required for flame combustion is a mixture of methane and oxygen, and the inner diameter of the combustion gas outlet is 4mm;

[0052] The dispersed gas is air or oxygen, and the inner diameter of the dispersed gas outlet hole is 6mm;

[0053] The outlet of the nozzle and the outlets of the through holes A and B face the same direction (upward or sideways upward).

[0054] like Figure 5As shown, the double flame nozzle used includes the above-mentioned two single flame nozzles, and the distance 7 between the geometric centers of the two nozzles on the upper surface of the gas distribution plate of the two single flame nozzles is 6, 10, and 15 cm; the angle 8 formed by the two nozzle outlet axes is 60 degrees.

[0055] Example 1

[0056] Preparation of copper-zirconium catalyst with single nozzle: ① 2.79 g copper acetate monohydrate Cu(CH3COO)2·H2O and 17.29 g zirconium n-butoxide (C 16 H 36 ② Place the solution on an ultrasonic stirrer and stir at room temperature until a clear solution is obtained. Use a syringe to pump the prepared solution into the nozzle at a speed of 5ml / min. The diameter of the liquid channel in the nozzle is 1mm. Use a gas distribution plate to blow out the combustion gas, ignite the combustion gas to form a flame, and the flame combustion gas is a mixture of methane (0.6L / min) and oxygen (1.9L / min). ③ Use a gas distribution plate to blow a large amount of air (6L / min) into the flame area, and driven by the high-speed air flow, the combustion products quickly leave the flame area. The prepared catalyst is recorded as SFSP-20Cu / ZrO2-1mm, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0057] Example 2

[0058] Preparation of copper-zirconium catalyst with single nozzle: ① 2.79 g copper acetate monohydrate Cu(CH3COO)2·H2O and 17.29 g zirconium n-butoxide (C 16 H 36 O4Zr content of 80wt%, the rest is n-butanol) is dissolved in a mixed solvent of 45ml of methanol and 45ml of 2-ethylhexanoic acid, the sum of the concentration of copper zirconium ions in the organic solution is 0.5mol / L, the solution is pumped into a nozzle, the diameter of the liquid channel in the nozzle is 1.5mm, and the remaining operation steps are the same as ②③ in Example 1. The prepared catalyst is recorded as SFSP-20Cu / ZrO2-1.5nm, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0059] Example 3

[0060] Preparation of copper-zirconium catalyst by double nozzles: ① Dissolve 2.64g of anhydrous copper acetate in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 1. Dissolve 17.29g of zirconium n-butoxide in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 2. The sum of the concentrations of copper-zirconium ions in the organic solution is 0.5mol / L. ② Place the two solutions in an ultrasonic stirrer and stir at room temperature until a clear solution is obtained. Use two syringes to pump the prepared solution 1 into the first nozzle at a speed of 5ml / min, and pump solution 2 into the second nozzle. The diameter of the liquid channel in the nozzle is 1mm. ③ Use a gas distribution plate to blow out the combustion gas, ignite the combustion gas to form a flame, and the flame combustion gas is a mixture of methane (0.6L / min) and oxygen (1.9L / min). Use a gas distribution plate to blow oxygen into the flame area, and the dispersed gas is oxygen (6L / min, pressure drop 3bar). ④ The center distance between the two nozzles was adjusted to 10 cm, and the angle between the two flames was 60 degrees. The nanoparticles produced by the two nozzles were collected above the flames, and the mixed catalyst particles were collected on the top of the collection bucket with the help of a vacuum pump using glass fiber filter paper. This process isolated the copper-zirconium components, and the prepared catalyst was recorded as DFSP-20Cu / ZrO2-1mm, and the theoretical mass fraction of oxidized Cu in the catalyst was 20%.

[0061] Example 4

[0062] Preparation of copper-zirconium catalyst by double nozzles: ① Dissolve 2.64g of anhydrous copper acetate in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 1. Dissolve 17.29g of zirconium n-butoxide in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 2. The sum of the concentrations of copper-zirconium ions in the organic solution is 0.5mol / L. ② Solution 1 is pumped into the first nozzle, and the diameter of the liquid channel in the first nozzle is 0.5mm. Solution 2 is pumped into the second nozzle, and the diameter of the liquid channel in the second nozzle is 1mm. The remaining operating steps are the same as ②③④ in Example 3. The copper-zirconium component is isolated in this process. The prepared catalyst is recorded as DFSP-20Cu / ZrO2-0.5mm, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0063] Example 5

[0064] Preparation of copper-zirconium catalyst by double nozzles: ① Dissolve 2.64g of anhydrous copper acetate in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 1. Dissolve 17.29g of zirconium n-butoxide in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 2. The sum of the concentrations of copper-zirconium ions in the organic solution is 0.5mol / L. ② Solution 1 is pumped into the first nozzle, and the liquid channel in the first nozzle is 1.5mm. Solution 2 is pumped into the second nozzle, and the liquid channel in the second nozzle is 1mm. The remaining operating steps are the same as ②③④ in Example 3. This process isolates the copper-zirconium component. The prepared catalyst is recorded as DFSP-20Cu / ZrO2-1.5mm, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0065] Example 6

[0066] Preparation of copper-zirconium catalyst by double nozzles: ① Dissolve 2.64g of anhydrous copper acetate in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 1. Dissolve 17.29g of zirconium n-butoxide in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 2. The sum of the concentrations of copper-zirconium ions in the organic solution is 0.5mol / L. ② Solution 1 is pumped into the first nozzle, and solution 2 is pumped into the second nozzle. The diameters of the two nozzles are both 1mm unchanged. The first nozzle uses oxygen (10L / min, pressure drop 3bar) as the dispersion gas, and the second nozzle uses oxygen (6L / min, pressure drop 3bar) as the dispersion gas. The remaining operating steps are the same as ②③④ in Example 3. The copper-zirconium component is isolated in this process. The prepared catalyst is recorded as DFSP-20Cu / ZrO2-10L / min, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0067] Example 7

[0068] Preparation of copper-zirconium catalyst by double nozzles: ① Dissolve 2.64g of anhydrous copper acetate in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 1. Dissolve 17.29g of zirconium n-butoxide in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 2. The sum of the concentrations of copper-zirconium ions in the organic solution is 0.5mol / L. ③ Adjust the center distance of the two nozzles to 15cm. The remaining operating steps are the same as ②③④ in Example 3. The copper-zirconium component is isolated in this process. The prepared catalyst is recorded as DFSP-20Cu / ZrO2-15cm, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0069] Example 8

[0070] Preparation of copper-zirconium catalyst by double nozzles: ① Dissolve 2.64g of anhydrous copper acetate in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 1. Dissolve 17.29g of zirconium n-butoxide in a mixed solvent of 20ml of methanol and 80ml of 2-ethylhexanoic acid to obtain 100ml of solution, which is recorded as solution 2. The sum of the concentrations of copper-zirconium ions in the organic solution is 0.5mol / L. ③ Adjust the center distance of the two nozzles to 6cm. The remaining operating steps are the same as ②③④ in Example 3. The copper-zirconium component is isolated in this process. The prepared catalyst is recorded as DFSP-20Cu / ZrO2-6cm, and the theoretical mass fraction of oxidized Cu in the catalyst is 20%.

[0071] Comparative Example 1

[0072] Preparation of Cu / ZrO2 catalyst by sedimentation precipitation method: First, prepare 200mL of zirconium oxide carrier with zirconium sec-butyl alcohol and 0.5mol / L of zirconium ion concentration in an organic solution, and the remaining steps are the same as those in Example 1 to obtain carrier zirconium oxide. Weigh 3.805g Cu(NO3)2·6H2O in 15mL of deionized water, weigh 13.25g Na2CO3 in 250mL of deionized water, weigh 4.0g ZrO2 carrier and pour into 200mL of deionized water, drip Cu(NO3)2 and Na2CO3 aqueous solutions into the aqueous solution at the same time, add to the above solution under constant stirring, keep pH=6.5, place the beaker in a 65℃ water bath for 1h; wash and centrifuge the precipitate with deionized water, transfer the obtained precipitate to a dryer, dry it in an oven at 120℃ overnight, and evaluate the reaction after direct reduction without high-temperature calcination.

[0073] The contents of the individual components were determined by inductively coupled plasma emission spectrometry (ICP). The results are shown in Tables 1 and 2. The results show that the catalysts prepared by single-nozzle and double-nozzle flame spraying methods have stable and flexibly adjustable component contents and are not affected by the preparation methods and conditions.

[0074] The N2O oxidation method was used to determine the dispersion of Cu particles, and the X-ray photoelectron spectroscopy was used to characterize the proportion of monovalent Cu in the total Cu content of the catalyst after hydrogen reduction at 300°C for 1 hour. The results are shown in Tables 1 and 2. By comparing Examples 1 and 3 with Comparative Example 1, it can be found that when the catalyst preparation conditions are the same for the single-nozzle and double-nozzle flame spray methods, the copper particle sizes are similar and the dispersion is uniform. Compared with the traditional deposition precipitation method, the flame spray method is more conducive to high copper dispersion, stabilizes more monovalent copper, and promotes the formation of strong interactions between copper and zirconium. By comparing Examples 1 and 2, it was found that as the diameter of the single-nozzle liquid channel increases, the volume of droplets that the combustion gas and the dispersion gas contact per unit time increases, and the combustion effect becomes worse, resulting in an increase in the copper particle size, but it will not have a significant effect on the valence state of the copper after reduction. The crystalline structure of the catalysts in Examples 1, 2 and Comparative Example 1 was investigated using an X-ray diffractometer (XRD). Figure 1 By comparing Examples 1 and 2, it can be found that the diameter of the single nozzle liquid channel increases, the combustion effect becomes worse, causing changes in the copper and zirconium components, resulting in an increase in the copper particle size, and the proportion of the monoclinic phase in the zirconium oxide crystal phase tends to increase. The results show that the single nozzle flame spraying method can cause structural changes in the copper-zirconium two-component.

[0075] The dispersion of Cu particles was determined by N2O oxidation method, and the proportion of monovalent Cu in the total Cu content of the catalyst after 1 hour of hydrogen reduction at 300°C was characterized by X-ray photoelectron spectroscopy. The results are shown in Tables 1 and 2. By comparing Examples 3, 4, and 5, it can be found that the double nozzles control the copper-zirconium dual components respectively. The nozzle containing the zirconium component remains unchanged, the diameter of the liquid channel of the nozzle containing the copper component decreases, and the particle size of the copper particles decreases. The diameter of the liquid channel of the nozzle containing the copper component increases, and the particle size of the copper also increases accordingly. Changing the diameter of the nozzle liquid channel has almost no effect on the valence distribution of copper after reduction. The crystal phase structure of the catalysts of Examples 3 and 4 was investigated by X-ray diffractometer (XRD). Figure 2 The double nozzle can accurately control the structure of the copper-zirconium two-component material, and can regulate the size of the copper particles while maintaining the overall tetragonal phase structure and particle size of zirconium oxide unchanged.

[0076] The dispersion of Cu particles was determined by N2O oxidation method, and the proportion of monovalent Cu in the total Cu content of the catalyst after 1 hour of hydrogen reduction at 300°C was characterized by X-ray photoelectron spectroscopy. The results are shown in Tables 1 and 2. By comparing Examples 3 and 6, it can be found that increasing the dispersion gas flow rate of the copper-containing nozzle promotes high dispersion of droplets in the flame and accelerates the quenching of copper, which not only improves the dispersion of copper, reduces the size of copper particles, increases the proportion of monovalent copper, and enhances the interaction between copper and zirconium. While the double nozzle does not change the structure of the zirconium component, increasing the dispersion gas flow rate of the copper-containing component nozzle can enhance the interaction between copper and zirconium, while reducing the size of copper and increasing the proportion of reduced monovalent copper.

[0077] The dispersion of Cu particles was determined by N2O oxidation method, and the proportion of monovalent Cu in the total Cu content of the catalyst after 1 hour of hydrogen reduction at 300°C was characterized by X-ray photoelectron spectroscopy. The results are shown in Tables 1 and 2. By comparing Examples 3, 7, and 8, it can be found that increasing the distance between the two nozzles has little effect on the size of copper, the contact degree of the copper-zirconium components is weakened, the degree of interaction is weakened, and the monovalent copper is reduced after reduction; increasing the distance between the two nozzles, the contact of the copper-zirconium components is more sufficient, the degree of interaction is enhanced, and the monovalent copper is increased. The spacing between the two nozzles is more sensitive to regulating the valence of copper and the degree of interaction between copper and zirconium.

[0078] X-ray photoelectron spectroscopy was used to characterize the proportion of monovalent Cu in the total Cu content of the catalysts of Example 1 and Comparative Example 1 after hydrogen reduction at 250, 300, and 350°C for 1 hour, and the results are shown in Table 3. The results show that the flame spray method is more conducive to stabilizing monovalent copper, and a relatively high proportion of monovalent copper can be maintained after high-temperature reduction; the copper-zirconium catalyst prepared by the deposition precipitation method has a weak copper-zirconium interaction, a low and unstable monovalent copper content, and will be deeply reduced to zero-valent copper at high temperatures.

[0079] Comparison of catalyst evaluation results: The reaction was carried out in a fixed bed reactor, loaded with 0.2 g of catalyst, reduced with pure H2 (25 ml / min), at a temperature of 300 °C and a reduction time of 1 h. Reaction conditions: molar ratio H2 / CO2 = 3, temperature of 200-260 °C, space velocity of 6000 ml / (h·g cat ), the pressure is 3.0MPa. The effect of reaction temperature on catalyst performance was investigated, and Examples 1, 3, 4, 6, 8 and Comparative Example 1 were tested. The test results are shown in Table 1. Comparing Examples 1 and 3 with Comparative Example 1, the copper-zirconium catalysts prepared by single nozzle and double nozzle have similar copper size and monovalent copper ratio, similar number and activity of copper-zirconium interfaces, similar reaction results, and much higher methanol production than the copper-zirconium catalyst prepared by the deposition precipitation method. Comparing Examples 3, 4, 6, and 8, the results show that increasing the dispersion of copper and increasing the proportion of monovalent copper can increase the production of methanol, and in Example 6, both the copper size is reduced and the proportion of monovalent copper is increased, which is the most obvious for the increase in methanol production.

[0080] Effect of reaction space velocity on catalyst performance: Reduction was performed with pure H2 (25 ml / min), reduction temperature was 300°C, and reduction time was 1 h. Reaction conditions: molar ratio H2 / CO2 = 3, temperature was 260°C, space velocity was 6000-18000 ml / (h·g cat ), the pressure is 3.0MPa, and the effect of different space velocities on the reaction performance at the same temperature in Example 5 is investigated. The test results are shown in Table 4. As the space velocity increases, the conversion rate decreases, but the selectivity increases. A high space velocity will bring a higher yield.

[0081] The sample prepared in Example 1 was subjected to X-ray near-edge absorption analysis during the in-situ temperature-programmed reduction process, and the species of each copper valence state were fitted. The changes in the mass proportion of each copper species in all copper were recorded during the process of heating at 5°C / min in a hydrogen atmosphere. Figure 3 . It can be seen that during the reduction and heating process of hydrogen atmosphere, divalent copper is reduced to zero-valent copper and monovalent copper in large quantities at the stage of 100-150°C, and the content of divalent copper suddenly decreases, and the ratio of zero-valent copper to monovalent copper increases accordingly. Generally speaking, monovalent copper is highly active but unstable and can be easily reduced to zero-valent copper. However, the monovalent copper of the sample of Example 1 can still exist stably during high-temperature reduction, and will not continue to be deeply reduced to zero-valent copper as the reduction temperature increases. Monovalent copper can stably account for 20% of the total copper content. In the reaction of carbon dioxide hydrogenation to methanol, monovalent copper is conducive to stabilizing intermediate species, inhibiting the desorption of intermediate species to produce CO, and then promoting the further hydrogenation of intermediate species to produce methanol, thereby improving the selectivity of methanol. The high-temperature quenching process in the flame spray preparation promotes the dispersion of copper and the strong interaction between copper and zirconium oxide, thereby stabilizing more highly active monovalent copper and showing better performance in the hydrogenation of carbon dioxide to methanol.

[0082] Table 1 Content of each component and copper content, particle size, and ratio of monovalent copper after reduction on the catalyst of Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1

[0083]

[0084]

[0085] Table 2 Content of each component on the catalyst of Examples 3, 7, and 8, content of copper, particle size, and proportion of monovalent copper after reduction

[0086]

[0087] Table 3 shows the ratio of monovalent copper after different reduction on the catalyst of Example 1 and Comparative Example 1

[0088]

[0089] Table 4 Effect of Examples 1, 3, 4, 6, 8 on the catalyst of Comparative Example 1 on the hydrogenation of carbon dioxide to methanol

[0090]

[0091]

[0092] Table 5 Effect of space velocity on catalyst of Example 1 on the performance of carbon dioxide hydrogenation to methanol reaction

[0093]

Claims

1. A method for preparing a copper-zirconium dual-component catalyst by flame spray pyrolysis, characterized in that: The copper content in the catalyst is 5-60% by mass, preferably 10-30% by mass; the rest is zirconium oxide component; (1) Preparation is carried out using a single flame nozzle or a double flame nozzle; Single flame nozzle: a. Mixing and dissolving the precursor compounds of copper and zirconium in an organic solvent according to the ratio required by the composition of the catalyst to form a copper-zirconium mixed solution; b. Pumping the copper-zirconium mixed solution into a nozzle, the solution is sprayed out from the nozzle, dispersed into droplets by the dispersion gas, and introduced into the flame formed by the combustion gas flowing out of the air holes arranged around the outside of the nozzle to burn; oxides containing copper components and zirconium components are generated in the single flame nozzle, and the copper and zirconium oxides in the single flame nozzle are mixed during the flame combustion process; Or, dual flame nozzle: a. dissolving a copper precursor compound in an organic solvent to form a copper solution; dissolving a zirconium precursor compound in an organic solvent to form a zirconium solution; b. The copper solution and the zirconium solution are pumped into two different nozzles respectively. The solutions are sprayed out from the two nozzles in the ratio required by the composition of the catalyst respectively. The solutions are dispersed into droplets by the dispersion gas respectively. The droplets are introduced into the flame formed by the combustion gas flowing out of the air holes arranged around the outer sides of the two nozzles respectively. The flames formed by the combustion gas flowing out of the air holes arranged around the outer sides of the two nozzles intersect at one end (flame tip area) away from the air holes to form a double flame intersection area. In the double flame nozzle, one flame nozzle produces an oxide containing a copper component, and the other flame nozzle produces an oxide containing a zirconium component. The oxides produced by the two flame nozzles of the double flame are collected in the double flame intersection area. (2) Collect the catalyst particles formed after combustion.

2. The method according to claim 1, characterized in that: The single flame nozzle used comprises a hollow tubular nozzle and a gas distribution plate, wherein the nozzle passes through the gas distribution plate from bottom to top and extends from the middle of the gas distribution plate, wherein the gas distribution plate around the nozzle outlet (1) is provided with combustion gas outlet holes (2) and dispersion gas outlet holes (3); the number of the combustion gas outlet holes (2) is more than 2, and the combustion gas outlet holes (2) are evenly distributed along the circumferential direction, and the geometric center of the circumferential distribution of the combustion gas outlet holes (2) is the geometric center of the nozzle outlet (1) as the center of the circle and the radius is R 1; the number of the dispersed gas outlet holes (3) is more than 2, and the dispersed gas outlet holes 3 are evenly distributed along the circumferential direction, the geometric center of the circumferential distribution of the dispersed gas outlet holes (3) is the geometric center of the nozzle outlet 1 as the center of the circle and the radius is R2, and R2 is greater than R1, and a combustion gas inlet (5) and a dispersed gas inlet (6) are provided on the gas distribution plate around the nozzle inlet (4), and the combustion gas inlet (5) is connected to the combustion gas outlet hole (2), and the dispersed gas inlet (6) is connected to the dispersed gas outlet hole (3), and the gas distribution A cylindrical container B is provided on the air inlet side of the plate, and one end of the cylindrical container B is sealed and the other end is open. The edges of the gas distribution plate are sealed and connected to the open end of the cylindrical container B. The cylindrical container B is provided with an air connection inlet connected to an air pump or an air compressor or an oxygen connection inlet connected to an oxygen source. A cylindrical container A is provided in the cylindrical container B with one end sealed and the other end open, and the open end of the cylindrical container A is sealed and connected to the plate surface between the combustion gas outlet hole (2) and the dispersion gas outlet hole (3) on the gas distribution plate. A combustion gas connection inlet connected to the combustion gas source is provided on the cylindrical container A. The gas in the cylindrical container A enters each combustion gas inlet (5), and the gas in the cylindrical container B enters each dispersion gas inlet (6). At the same time, the cylindrical container A blocks the gas in the cylindrical container B from entering the combustion gas inlet (5). In addition, a pipeline is provided at the nozzle inlet (4), which passes through the cylindrical container A and the cylindrical container B and then pumps the organic precursor to be burned at a uniform speed with a liquid injection pump. Alternatively, the double flame nozzle used includes the two single flame nozzles mentioned above, wherein the double nozzle spacing (7) between the geometric centers of the two nozzles on the upper surface of the gas distribution plate of the two single flame nozzles is 1-30 cm, preferably 5-15 cm; and the flame combustion angle (8) formed by the two nozzle outlet axes is 10-120 degrees, preferably 45-90 degrees.

3. The method according to claim 1, characterized in that: The combustion gas required for flame combustion is a mixture of methane and oxygen. The inner diameter of the combustion gas outlet is 1-10 mm. The sum of the radial cross-sectional areas of all through holes A on the gas distribution plate is 1-20 square centimeters. The flow rates of methane and oxygen are 0.1-5 L / min respectively. The dispersed gas is air, the inner diameter of the dispersed gas outlet hole is 1-10 mm, the sum of the radial cross-sectional areas of all through holes B on the gas distribution plate is 1-20 square centimeters, and the dispersed gas flow rate is 2-20 L / min; The inner diameter of the nozzle is 0.5-2.5 mm, and the speed of the solution pumping out is 0.1-20 ml / min.

4. The method according to claim 2, characterized in that: R1 = 0.5-3 cm, R2 = 1-10 cm; The outlet of the nozzle and the outlets of the through holes A and B face the same direction (upward or sideways upward).

5. The method according to any one of claims 1 to 4, comprising the following steps: Dissolving a precursor compound containing copper and zirconium in a solvent; injecting the prepared solution into a single flame nozzle at a uniform speed; igniting a combustion gas to form a flame, wherein the combustion gas required for flame combustion is a mixture of methane and oxygen; The dispersion gas is air, which is blown to the entire flame area by a gas distribution plate surrounding the nozzle and having gas through holes uniformly distributed on the surface; the solution is pumped into the flame, and the air disperses the solution at the injection needle in the center of the nozzle into mist droplets, which are introduced into the flame for combustion. The precursor compounds of each component are decomposed under the high temperature of the flame to form oxide particles, and the formed oxide particles leave the flame area driven by the air; the single flame nozzle completes the mixing of copper and zirconium oxides during the combustion process; the catalyst powder formed after the collection is collected; Or, dissolving a copper-containing precursor compound in a solvent; dissolving a zirconium-containing precursor compound in a solvent; Pump the prepared solution into two nozzles of the double flame nozzle respectively; Ignite the combustion gas to form a flame, the combustion gas required for flame combustion is a mixture of methane and oxygen; The dispersion gas is air and / or oxygen, and the air is blown to the entire flame area from a gas distribution plate with gas holes uniformly distributed on the surface and surrounding the nozzle; the solution is pumped into the flame, and the air disperses the solution at the injection needle in the center of the nozzle into small mist droplets, which are introduced into the flame for combustion. The precursor compounds of each component are decomposed under the high temperature of the flame to form oxide particles, and the formed oxide particles leave the flame area driven by the air; The oxides produced by the two nozzles of the double flame converge in the flame tip area, and the catalyst powder formed after the convergence is collected.

6. The preparation method according to claim 1 or 5, characterized in that: The copper precursor compound is a compound soluble in a solvent, preferably one or more of copper acetate, copper citrate, copper acetylacetonate, copper nitrate, and copper (II) diethylhexanoate; the molar concentration of copper in the copper solution is 0.1-2 mol / L, preferably 0.1-0.5 mol / L; The zirconium precursor compound is a compound that can be dissolved in a solvent, preferably one or more of zirconium n-butoxide, zirconium acetate, zirconium acetylacetonate, zirconium citrate, and zirconium diethylhexanoate, and the molar concentration of zirconium in the zirconium solution is 0.1-2 mol / L, preferably 0.1-0.5 mol / L; The solvent is a combustible organic solvent, preferably one or more of methanol, ethanol, xylene, liquid hydrocarbons, and organic acids; The total molar concentration of copper-zirconium metal ions in the copper-zirconium mixed solution is 0.01-2 mol / L, preferably 0.1-0.5 mol / L.

7. A copper-zirconium two-component catalyst prepared by the method according to any one of claims 1 to 6.

8. Use of the copper-zirconium two-component catalyst according to claim 7 in catalyzing the hydrogenation reaction of carbon dioxide.

9. The use according to claim 8, characterized in that: Before the catalyst is used, it needs to be subjected to hydrogen reduction treatment, the reduction temperature is 250-400°C, preferably 250-350°C, the time is 0.5-4h, preferably 1-2h; after the catalyst is subjected to hydrogen reduction, the zirconium oxide remains unchanged, the copper oxide is reduced to monovalent copper and zero-valent copper, and the proportion of monovalent copper in all copper contents reaches 10-30%, preferably 20-30%; the particle size of the copper particles is 1.5-7nm, preferably 1.5-5nm. (6) The catalyst is used for the thermal catalytic synthesis of methanol from carbon dioxide and hydrogen.

10. The use according to claim 8 or 9, characterized in that: The hydrogenation reaction conditions are as follows: the molar ratio of H2 to CO2 in the raw gas is 1-10, preferably 3-5, the reaction temperature is 150-300°C, preferably 180-250°C, the reaction pressure is 1.0-10.0 MPa, preferably 2.0-4.0 MPa, and the raw gas gas space velocity is 2040-24000 ml / (h·g cat ).

Citation Information

Patent Citations

  • Copper-based hydrogenation catalyst prepared by flame jet cracking method and preparation and application thereof

    CN108144610A

  • Method for preparing tetragonal zirconium oxide in one step, supported copper-based catalyst and application of supported copper-based catalyst

    CN114713223A

  • Metal delivery system for nanoparticle manufacture

    CN1787964A

  • Flame spray pyrolysis with versatile precursors for metal oxide nanoparticle synthesis and applications of submicron inorganic oxide compositions for transparent electrodes

    US20100102700A1