Monolithic reversed-phase Ni-based catalyst for preparing methane through CO2 hydrogenation with low temperature, high activity and high selectivity as well as preparation method and application of monolithic reversed-phase Ni-based catalyst

By anchoring metal Ni on the foam metal support and loading nanooxides, an integral Ni-based catalyst with reverse phase interface active sites is constructed, and the low-temperature, high-activity and high-selective CO2 hydrogenation is achieved to generate methane, solving the existing catalyst The problem of insufficient activity at low temperatures is suitable for biogas upgrade process.

CN118904348APending Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH

Patent Information

Application Number
CN202410815523.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

It is difficult for existing catalysts to achieve efficient CO2 hydrogenation to produce methane at low temperatures, and traditional nickel-based catalysts are insufficient in activity at high temperatures, which cannot meet the requirements of the biogas upgrade process for methane yield.

Method used

Using an integral reverse phase Ni-based catalyst of low-temperature, high-activity, high-selective, and high-selective CO2 hydrogenation to methane, the reverse phase interface active site is constructed to achieve low-temperature and high conversion rate and high selectivity.

Benefits of technology

Under the conditions of 220℃~260℃, the CO2 conversion rate exceeds 95% and the methane selectivity is 100%. It is suitable for industrial biogas upgrade process, solving the problem of insufficient activity of traditional catalysts at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a monolithic reversed-phase Ni-based catalyst for preparing methane through low-temperature high-activity high-selectivity CO2 hydrogenation as well as a preparation method and application of the monolithic reversed-phase Ni-based catalyst, and relates to a strategy of in-situ construction of a Ni reversed-phase interface active site monolithic catalyst by taking porous foam metal as a substrate. High-temperature hot spots and reaction product water caused by methanation reaction in the biogas upgrading process are quickly removed by utilizing excellent thermal conductivity and abundant three-dimensional channels of a foamed nickel structured metal material, and the adverse effects of thermal effect in the reaction process and sintering, oxidation and the like of a large amount of product water on active sites are inhibited; the monolithic reverse catalyst prepared by the method is applied to CO2 hydrogenation methane preparation reaction in a methane-rich atmosphere, and under the conditions that the pressure is 0.1 MPa, the volume space velocity is 10000 h <-1 >, the ratio of H2 to CO2 to CH4 is 4: 1: 1 and the temperature is 220-260 DEG C, the CO2 conversion rate exceeds 95%, and the methane selectivity is 100%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a low-temperature, high-activity, high-selectivity CO 2 An integral reversed Ni-based catalyst for hydrogenating methane, and a preparation method and application thereof. Background Art

[0002] Currently, more than 85% of the world's energy needs are met by the use of fossil fuels, and the CO 2 About 2.5 billion tons of CO 2 80% of emissions are caused by greenhouse gases and are widely considered to be the main contributors to global warming and climate change. In addition, ensuring energy supply is a vital issue, considering that conventional energy sources (i.e., oil and gas reserves) are mainly located in politically unstable regions. Therefore, in order to address these critical issues, a lot of efforts are aimed at effectively developing renewable energy sources such as geothermal, wind, solar, and biomass. In this race, biogas, which is usually produced by anaerobic digestion of biodegradable waste and substrates, is widely considered to be one of the most promising renewable energy sources. Methane (about 40-75 vol%) and carbon dioxide (25-60 vol%) are the main components of biogas, and biogas also contains N 2 , O 2 , H 2 S and other pollutants, the content of which depends on the different production plants. Therefore, before use, biogas must be upgraded to make methane (CH 4 ) content exceeds 90%. Generally, biogas upgrading technology uses carbon dioxide (CO 2 ) is removed, and then CO 2 To achieve clean biogas utilization, the CO in biogas is 2 Converted into valuable biofuels such as CH 4 , is an alternative method with promising applications. 2 It is a covalent molecule with a linear molecular configuration, and its standard Gibbs free energy of formation Δ f G 298K =-396 kJmol -1 , the single C=O bond length is The bond energy is 799 kJ mol -1 , so CO 2 The molecule has high thermodynamic stability and chemical inertness and is not easily activated. The introduction of hydrogen as a high-energy substance can make CO 2 The conversion of CO is relatively easy to carry out. 2 There are three main competing reactions in the hydrogenation process:

[0003]

[0004] The methanation reaction (1) is an exothermic reaction with a decrease in molecular weight under standard conditions. Low temperature and high pressure are conducive to the forward progress of the reaction. However, lower reaction temperature affects CO 2 The reverse water-gas shift reaction (2) and the methane cracking reaction (3) are endothermic reactions, and high temperatures are conducive to the forward reaction. However, the temperature required to achieve full activity of traditional nickel-based catalysts is about 593K, which is not thermodynamically favorable. Therefore, it is impossible to achieve a methane yield of more than 95%, which is difficult to meet the needs of the biogas upgrading process. Therefore, the development of a suitable low-temperature, high-conversion, and high-selectivity catalytic system is the key to realizing the biogas upgrading process.

[0005] Generally, noble metal-based catalysts exhibit efficient CO 2 Methanation has low-temperature performance, but is not suitable for large-scale application due to cost and other reasons. In addition, nickel-based catalysts show high CO 2 Methanation performance. In order to improve its activity, researchers have adopted a variety of strategies, such as increasing the nickel loading, changing the nickel particle size, doping a second metal, improving the strong metal-support interaction (SMSI), etc. Among them, adjusting the properties of the support, such as crystal phase, specific surface area, surface pH, pore structure, support particle size and oxygen vacancies, can significantly affect CO 2 However, to date, these reported CO 2 The optimal reaction temperature of methanation catalysts is still higher than 300°C, and the conversion rate is limited by thermodynamic equilibrium and is difficult to meet process requirements.

[0006] To this end, the present invention provides a low-temperature, high-activity, high-selectivity CO 2 The monolithic reverse Ni-based catalyst for hydrogenation to methane and its preparation method and application are expected to be used for industrial biogas upgrading and quality improvement. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention proposes a low-temperature, high-activity, and high-selectivity CO 2 The preparation method and application of the monolithic reversed Ni-based catalyst for hydrogenation to methane, wherein the metal Ni that dissociates hydrogen is evenly anchored on the surface of the foam metal carrier, nano-oxides are loaded on it, and reversed interface active sites are constructed, which can achieve low-temperature high conversion rate, high selectivity, and high stability of CO 2 Hydrogenation to produce methane.

[0008] The technical solution of the present invention is as follows:

[0009] A low-temperature, high-activity, high-selectivity CO 2The monolithic reverse Ni-based catalyst for hydrogenation to methane is characterized in that the metal Ni that dissociates hydrogen is evenly anchored on the surface of a foam metal carrier, and nano-oxides are further loaded thereon to construct reverse interface active sites, wherein the foam metal carrier is one of foam nickel, foam cobalt, foam aluminum, and foam copper; and the loaded phase nano-oxides are selected from one or more of yttrium oxide, zirconium oxide, cerium oxide, aluminum oxide, and magnesium oxide.

[0010] Furthermore, based on the total molar amount of the metal in the supported phase, the molar fraction of the metal in the supported phase is 0.01 to 30%.

[0011] The present invention also proposes a low-temperature, high-activity, high-selectivity CO 2 The preparation method of the monolithic reversed phase Ni-based catalyst for hydrogenation to methane comprises the following steps:

[0012] 1) Treatment of foam metal: The foam metal sheet was sanded to remove part of the surface oxide, and a foam metal disc with a radius of 2 to 3 mm was cut out with a puncher. The cut disc was placed in a 100 mL beaker, and an acetone solution was added for ultrasonic treatment. The treated foam metal was washed with anhydrous ethanol for several times, and then a hydrochloric acid solution was added for ultrasonic treatment to remove surface oxides and organic impurities. The treated foam metal was washed with anhydrous ethanol for several times; finally, it was placed in a vacuum oven at 60° C. and dried for 12 h. The dried foam metal carrier was recorded as M-foam;

[0013] 2) Preparation of NiO / M-foam: A precursor salt corresponding to the metal Ni that dissociates hydrogen is added to a solvent and stirred until completely dissolved. A precipitant solution is added dropwise to the precursor salt solution under vigorous stirring. After the dropwise addition is completed, the solution stirred until completely dissolved and the foam metal after the pretreatment in step 1) are added to the lining of a hydrothermal kettle, and then the lining of the hydrothermal kettle is installed in the hydrothermal kettle. The hydrothermal kettle is tightened and installed in a homogeneous reactor for hydrothermal treatment. After the hydrothermal treatment is completed, the sample is taken out and washed several times. After the washing is completed, the sample is taken out and vacuum dried. After vacuum drying, it is calcined. After calcination, a foam metal carrier loaded with NiO can be obtained, which is recorded as NiO / M-foam;

[0014] 3) Preparation of monolithic reversed Ni-based catalyst The NiO / M-foam metal foam carrier prepared in step 2) was dispersed in a deoxygenated nitrogen-protected solution, and then the adsorption activated CO 2The precursor salt of the nano-oxide and the precipitant are added, and the mixed solution is transferred to the lining of the hydrothermal kettle and then ultrasonically treated to make the oxide precursor salt evenly dispersed, the hydrothermal kettle is tightened, and the hydrothermal kettle is installed in the homogeneous reactor, and then the hydrothermal kettle is transferred to the homogeneous reactor for hydrothermal treatment. After the hydrothermal treatment, the prepared sample is vacuum dried to completely remove the moisture in the sample, and finally the dried sample is calcined again. After the calcination, the monolithic reverse Ni-based catalyst can be obtained, which is denoted as M n O x / NiO / M-foam.

[0015] Furthermore, in step 2), the precursor salt is selected from one or more of nickel nitrate, nickel chloride, nickel sulfate, nickel acetate, and nickel acetylacetonate; the solvent is selected from one or more of water, methanol, ethanol, butanol, tetrahydrofuran, and methyl tert-butyl ether;

[0016] Step 2) The concentration of the precursor salt of metal Ni used to dissociate hydrogen is 0.01-5 mol / L.

[0017] Further, in step 2), the foamed metal and the precursor salt solution are subjected to hydrothermal etching, and the specific process is as follows:

[0018] The foamed metal after the pretreatment in step 1) is fully mixed with the precursor salt solution of metal Ni, transferred to the lining of the hydrothermal kettle and placed in a homogeneous reactor, and subjected to hydrothermal treatment at 160-220° C. for 12-20 hours, and then the foamed metal etched and loaded with metal Ni is dried in a vacuum oven for 12 hours, and then calcined at 250-350° C. for 0.5-2 hours to obtain the foamed metal carrier, which is recorded as NiO / M-foam;

[0019] The precipitant is selected from urea, ammonium fluoride, ammonium chloride, ammonium oxalate and oxalic acid.

[0020] Further, in step 3), the precursor salt is selected from one or more of aluminum nitrate, aluminum chloride; cerium nitrate, cerium chloride; zirconium nitrate, zirconium chloride, zirconium oxychloride; yttrium nitrate, yttrium chloride, yttrium acetylacetonate; magnesium nitrate, magnesium sulfate, magnesium chloride; and the solvent used to dissolve the oxide precursor salt and the precipitant is selected from one or more of water, ethanol, butanol, and ethylene glycol;

[0021] Step 3) The concentration of the precursor salt of the oxide that generates oxygen vacancies to adsorb and activate carbon dioxide is 0.01-5 mol / L.

[0022] Furthermore, in step 3), the hydrothermal temperature is 160-200° C.; the hydrothermal time is 12-20 h; the drying temperature is 40-100° C., and the drying time is 6-12 h.

[0023] Furthermore, in step 3), the feed ratio of the foam metal carrier to the nano-oxide precursor salt is 20:1-1:20; and the stirring time is 1 to 3 hours.

[0024] Furthermore, in step 3), the calcination temperature is 300-500° C. and the calcination time is 1-4 h.

[0025] The invention also proposes the use of an integral reversed-phase Ni catalyst in a biogas upgrading process.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] 1) The present invention uses porous foam metal as a substrate to in-situ construct a Ni reverse-phase interface active site monolithic catalyst, and utilizes the excellent thermal conductivity and rich three-dimensional channels of the foam nickel structured metal material to quickly remove the high-temperature hot spots and reaction product water caused by the methanation reaction in the biogas upgrading process, thereby inhibiting the thermal effect of the reaction process and the adverse effects of sintering and oxidation of a large amount of product water on the active site. It is a new type of monolithic reverse-phase catalyst;

[0028] 2) The monolithic reversed Ni-based catalyst prepared by the method of the present invention is applied to CO in a methane-rich atmosphere 2 Hydrogenation to methane reaction, at 0.1MPa, volume space velocity 10000h -1 , H 2 / CO 2 / CH 4 =4:1:1, 220°~260℃, CO 2 The conversion rate exceeds 95% and the methane selectivity is 100%, which is expected to be used in industrial biogas upgrading processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 For Example 16 to Example 23 at 220°C, 11000h -1 CO under the conditions of space velocity and 0.1 MPa nickel deposition on different metal oxides 2 Conversion vs. methane selectivity plot;

[0030] Figure 2 For Example 1 to Example 4 at 220°C, 11000h -1 air velocity, 0.1Mpa, step (3) selects CO under different hydrothermal temperature conditions 2 Conversion vs. methane selectivity plot;

[0031] Figure 3 For example 1, example 5-example 8 at 220°C, 11000h -1 air velocity, 0.1Mpa, step (3) selects CO under different hydrothermal time conditions2 Conversion vs. methane selectivity plot;

[0032] Figure 4 For Example 1, Example 9-Example 12 at 220°C, 11000h -1 Space velocity, 0.1Mpa, CO under different precipitants 2 Conversion vs. methane selectivity plot;

[0033] Figure 5 CO under different carrier conditions selected from Example 1, Example 12 to Example 15 at 220°C, 11000h-1 air velocity, and 0.1Mpa 2 Conversion vs. methane selectivity plot;

[0034] Figure 6 For Example 1, Comparative Examples 1 to Comparative Examples 4, at 220°C, 11000h -1 Space velocity, 0.1Mpa, CO under different carrier conditions 2 Conversion vs. methane selectivity plot;

[0035] Figure 7 For Example 1, Example 24-Example 27 at 220°C, 0.1 MPa, CO under different space velocity conditions 2 Conversion vs. methane selectivity plot;

[0036] Figure 8 The CO in Example 1, Example 28-Example 29 at 220°C and 0.1 MPa with different methane concentrations 2 Conversion rate and methane selectivity, the optimal reaction atmosphere is CO 2 :H 2 :CH 4 =1:4:1. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with the accompanying drawings and embodiments, but the scope of protection of the present invention is not limited to the described scope.

[0038] Example 1

[0039] 1) Take a Ni-foam sheet with a thickness of 2 mm and a porosity of 100 PPI, polish it with sandpaper to remove some oxides on the surface, cut out a small nickel foam disc with a length and width of about 2 to 3 mm with a puncher, put the small disc into a beaker, add 50 mL of a 25% acetone dilution solution and ultrasonically treat it for 10 minutes, wash the treated nickel foam with anhydrous ethanol for several times, then add 50 mL of a 3.6% hydrochloric acid dilution solution and ultrasonically treat it for 10 minutes, wash the treated nickel foam with anhydrous ethanol for several times, and put the treated nickel foam into an oven for drying;

[0040] 2) Dissolve 0.436185g nickel nitrate hexahydrate in 32mL deionized water at 0.04687mol / L, add 0.8g urea, stir until completely dissolved, add to the 50mL hydrothermal kettle lining containing 0.4g nickel foam, then install the lining into the hydrothermal kettle, tighten the hydrothermal kettle, install the hydrothermal kettle into the homogeneous reactor, heat to 160℃ and hydrothermal for 6h. Pour out the green liquid in the hydrothermal kettle lining after hydrothermal, take out the nickel foam with green flocs in the hydrothermal kettle lining, put it in a 70℃ oven to dry overnight, and calcine at 250℃ for 2h. The obtained nickel foam is recorded as NiO / Ni-foam;

[0041] 3) Dissolve 0.8832g of cerium nitrate hexahydrate and 0.4332g of zirconium nitrate pentahydrate in 32mL of deionized water, then add 0.8g of urea, stir until completely dissolved, and add to the 50mL hydrothermal kettle lining containing 0.4g of NiO / Ni-foam foam metal carrier, then install the lining into the hydrothermal kettle, tighten the hydrothermal kettle, install the hydrothermal kettle into the homogeneous reactor, heat to 200℃ and hydrothermal for 16h. Pour out the liquid in the hydrothermal kettle lining after hydrothermal treatment, take out the nickel foam in the hydrothermal kettle lining, dry it in a 70℃ oven for 12h, add the dried nickel foam to a muffle furnace and calcine it at 400℃ for 3h, take it out and place it in a gas-solid phase reactor and pass 20% H 2 With 80% N 2 The mixture was reduced at 450℃ for 3h, and then carbon dioxide was hydrogenated to produce methane. The molar ratio of CO 2 :H 2 :CH 4 =1:4:1 reaction gas, space velocity is 10000h -1 -70000h -1 , the reaction pressure is 0.1MPa, and the reaction temperature is 160℃-300℃.

[0042] Embodiment 2-4

[0043] Except that the hydrothermal temperatures selected in step 3) are 160° C., 180° C., and 220° C. respectively, the rest are the same as in Example 1.

[0044] Embodiment 5-8

[0045] Except that the hydrothermal time selected in step 3) is 12 h, 14 h, 18 h, and 20 h respectively, the rest is the same as in Example 1.

[0046] Examples 9-12

[0047] Except that the precipitants selected in step 3) are ammonium chloride, ammonium fluoride, ammonia water, and oxalic acid dihydrate, the rest are the same as those in Example 1.

[0048] Examples 13-15

[0049] Except that the carrier selected in step 1) is foamed cobalt, foamed aluminum, or foamed copper, the rest is the same as in Example 1.

[0050] Example 16

[0051] In addition to the step 3) the metal oxide selected is ZrAlO x , except that the added oxide precursor salt is 0.4332g of zirconium nitrate pentahydrate and 0.7630g of aluminum nitrate nonahydrate, the rest is the same as Example 1.

[0052] Embodiment 17

[0053] In addition to the step 3) the metal oxide selected is ZrYO x , except that the metal oxide precursor salt added in step 3) is 0.4332 g of zirconium nitrate pentahydrate and 0.7057 g of yttrium nitrate tetrahydrate, the rest is the same as in Example 1.

[0054] Embodiment 18

[0055] In addition to the step 3) the selected metal oxide is MgAlO x , except that the metal oxide precursor salt added in step 3) is 0.5215 g of magnesium nitrate hexahydrate and 0.3872 g of aluminum nitrate nonahydrate, the rest is the same as in Example 1.

[0056] Embodiment 19

[0057] In addition to the step 3) the metal oxide selected is CeO 2 , except that the metal oxide precursor salt added in step 3) is 1.3314 g of cerium nitrate hexahydrate, the rest is the same as in Example 1.

[0058] Embodiment 20

[0059] In addition to the step 3) the metal oxide selected is ZrO 2 Except that the metal oxide precursor salt added in step 3) is 1.3164 g of zirconium nitrate hexahydrate, the rest is the same as in Example 1.

[0060] Embodiment 21

[0061] In addition to the step 3) the metal oxide selected is Al 2 O 3 , except that the metal oxide precursor salt added in step 3) is 1.1502 g of aluminum nitrate nonahydrate, the rest is the same as in Example 1.

[0062] Embodiment 22

[0063] In addition to the step 3) the metal oxide selected is Y 2 O 3 , except that the metal oxide precursor salt added in step 3) is 1.0639 g of yttrium nitrate tetrahydrate, the rest is the same as in Example 1.

[0064] Embodiment 23

[0065] Except that the metal oxide selected in step 3) is MgO and the metal oxide precursor salt added in step 3) is 0.7861 g of magnesium nitrate hexahydrate, the rest is the same as Example 1.

[0066] Examples 24-27

[0067] In addition to the selected test airspeed of 25000h -1 , 45000h -1 , 60000h -1 , 70000h -1 Except for this, the rest are the same as in Example 1.

[0068] Examples 28-29

[0069] In addition to the reaction atmosphere selected in step 3), CO 2 :H 2 :CH 4 =1:4:1.5, CO 2 :H 2 :CH 4 =1:4:3, the rest are the same as in Example 1.

[0070] Comparative Example 1

[0071] Preparation of conventional powder normal phase catalyst by coprecipitation method

[0072] Nickel nitrate hexahydrate was used as the nickel source of the catalyst, and a nickel-based catalyst was prepared by a coprecipitation method. The method was as follows: 0.8723 g of nickel nitrate hexahydrate, 1.5197 g of cerium nitrate hexahydrate, 1.5026 g of zirconium nitrate pentahydrate and 100 mL of anhydrous ethanol were added to a beaker, 50 mL of anhydrous ethanol was added to 2.7 g of anhydrous oxalic acid, the two prepared solutions were placed on a six-paddle and stirred evenly, the oxalic acid solution was added dropwise to the metal salt solution at a flow rate of 60 mL / h using a syringe pump, after the addition was completed, the metal salt solution was continued to be placed on the six-paddle and stirred for 2 h to completely precipitate the metal salt, the precipitated metal salt solution was vacuum filtered, washed with anhydrous ethanol to obtain a filter cake, dried in an oven at 80°C overnight, ground the dried solid into powder in a mortar, and finally calcined at 400°C for 3 h in a muffle furnace to obtain Ni / CeZrO x Powder catalyst.

[0073] Comparative Example 2

[0074] 1) Take a Ni-foam sheet with a thickness of 2 mm and a porosity of 100 PPI, polish it with sandpaper to remove some oxides on the surface, cut out a small nickel foam disc with a length and width of about 2 to 3 mm with a puncher, put the small disc into a beaker, add 50 mL of a 25% acetone dilution solution and ultrasonically treat it for 10 minutes, wash the treated nickel foam with anhydrous ethanol for several times, then add 50 mL of a 3.6% hydrochloric acid dilution solution and ultrasonically treat it for 10 minutes, wash the treated nickel foam with anhydrous ethanol for several times, and put the treated nickel foam into an oven for drying;

[0075] 2) Dissolve 0.8832g of cerium nitrate hexahydrate and 0.4332g of zirconium nitrate pentahydrate in 32mL of deionized water, then add 0.8g of urea, stir until completely dissolved, add to the 50mL hydrothermal kettle lining containing 0.4g of nickel foam, then install the lining into the hydrothermal kettle, tighten the hydrothermal kettle, install the hydrothermal kettle into the homogeneous reactor, heat to 160℃ and hydrothermal for 6h. Pour out the green liquid in the hydrothermal kettle lining after hydrothermal treatment, take out the nickel foam with green flocs in the hydrothermal kettle lining, put it in a 70℃ oven to dry overnight, and calcine at 250℃ for 2h. The obtained nickel foam is recorded as NiO / Ni-foam;

[0076] 3) Dissolve 0.436185 g nickel nitrate hexahydrate in 32 mL deionized water, add 0.8 g urea, stir until completely dissolved, and add to the mixture containing 0.4 g CeZrO x / Ni-foam foam metal carrier in a 50mL hydrothermal kettle lining, then install the lining into the hydrothermal kettle, tighten the hydrothermal kettle, install the hydrothermal kettle into the homogeneous reactor, heat it to 200℃ and hydrothermal for 16h. Pour out the liquid in the hydrothermal kettle lining after hydrothermal, take out the nickel foam in the hydrothermal kettle lining, dry it in a 70℃ oven for 12h, add the dried nickel foam to a muffle furnace and calcine it at 400℃ for 3h, take it out and place it in a gas-solid phase reactor and pass 20% H 2 With 80% N 2 The mixture was reduced at 450℃ for 3h, and then carbon dioxide was hydrogenated to produce methane. The molar ratio of CO 2 :H 2 :CH 4 =1:4:1 reaction gas, space velocity is 10000h -1 -70000h -1 , the reaction pressure is 0.1MPa, and the reaction temperature is 160℃-300℃.

[0077] Comparative Example 3

[0078] In addition to step 3) metal oxides loaded with metals to form a solid catalyst Ni / CeO on a nickel foam substrate with a normal phase interface2 / Ni-foam, the rest are the same as those in Example 2.

[0079] Comparative Example 4

[0080] In addition to step 3) metal oxide loaded metal forms a solid catalyst Ni / ZrO on a nickel foam substrate to construct a normal phase interface 2 / Ni-foam, the rest are the same as those in Example 2.

[0081] Table 1 Catalysts for CO 2 CO in the hydrogenation reaction to produce methane 2 Conversion and methane selectivity

[0082]

[0083]

[0084] Compared with the comparative example, Examples 1 to 29 in Table 1 show higher CO 2 The activity of hydrogenation to methane reflects the superiority of the reverse metal oxide / metal / foam substrate catalyst over the conventional forward metal / metal oxide / foam substrate catalyst. 2 Advantages of hydrogenation to produce methane.

[0085] Depend on Figure 1 It can be seen that Examples 16 to 23 at 220°C and 11000h -1 CO under the conditions of space velocity and 0.1 MPa nickel deposition on different metal oxides 2 Conversion rate and methane selectivity, the preferred metal oxide is CeZrO x .

[0086] Depend on Figure 2 It can be seen that in Examples 1 to 4, at 220°C, 11000 h-1 air velocity, and 0.1 MPa, step (3) selected CO under different hydrothermal temperature conditions. 2 Conversion rate and methane selectivity, step 3) select CO under different hydrothermal temperature conditions 2 Conversion rate and methane selectivity, the preferred hydrothermal temperature is 200°C.

[0087] Figure 3 It can be seen that Example 1, Example 5-Example 8 at 220°C, 11000h -1 air velocity, 0.1Mpa, step (3) selects CO under different hydrothermal time conditions 2 Conversion rate and methane selectivity, step 3) select CO under different hydrothermal time conditions 2 Conversion rate and methane selectivity, the preferred hydrothermal time is 16h.

[0088] Figure 4 It can be seen that Example 1, Example 9-Example 12 at 220°C, 11000h -1 Space velocity, 0.1Mpa, CO under different precipitants 2 Conversion rate and methane selectivity, the preferred precipitant in step 3) is urea.

[0089] Figure 5 It can be seen that Example 1, Example 13-Example 15 at 220°C, 11000h -1 Space velocity, 0.1Mpa, CO under different carrier conditions 2 Conversion rate and methane selectivity, the preferred carrier is nickel foam.

[0090] Figure 7 It can be seen that in Example 1, Example 24-Example 27 at 220°C, 0.1Mpa, and different CO 2 Conversion rate and methane selectivity at 11000h -1 -70000h -1 Within the air velocity range, the carbon dioxide conversion rate is above 88%.

[0091] Figure 8 It can be seen that the CO in Example 1, Example 28-Example 29 under different methane concentration atmosphere conditions of 220°C and 0.1MPa 2 Conversion rate and methane selectivity, the preferred reaction atmosphere is CO 2 :H 2 :CH 4 =1:4:1.

[0092] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A monolithic reversed-phase Ni-based catalyst for low-temperature, high-activity, and high-selectivity CO2 hydrogenation to methane, characterized in that The metal Ni that dissociates hydrogen is evenly anchored on the surface of the foam metal carrier, and nano-oxides are further loaded thereon to construct anti-phase interface active sites, wherein the foam metal carrier is one of foam nickel, foam cobalt, foam aluminum, and foam copper; the loaded phase nano-oxide is selected from one or more of yttrium oxide, zirconium oxide, cerium oxide, aluminum oxide, and magnesium oxide.

2. The monolithic reversed-phase Ni-based catalyst for low-temperature, high-activity, and high-selectivity CO2 hydrogenation to methane according to claim 1, characterized in that Based on the total molar amount of metal in the supported phase, the molar fraction of the metal in the supported phase is in the range of 0.01 to 30%.

3. A method for preparing a monolithic reversed-phase Ni-based catalyst for low-temperature, high-activity, and high-selectivity CO2 hydrogenation to methane as claimed in claim 1, characterized in that The steps include: 1) Treatment of foam metal: The foam metal sheet was sanded to remove some surface oxides, and a foam metal disc with a radius of 2-3 mm was cut out with a puncher. The cut disc was placed in a 100 mL beaker, and an acetone solution was added for ultrasonic treatment. The treated foam metal was washed with anhydrous ethanol for several times, and then a hydrochloric acid solution was added for ultrasonic treatment to remove surface oxides and organic impurities. The treated foam metal was washed with anhydrous ethanol for several times; finally, it was placed in a vacuum oven at 60°C for 12 hours for drying. The dried foam metal carrier was recorded as M-foam; 2) Preparation of NiO / M-foam: The precursor salt corresponding to the metal Ni that dissociates hydrogen is added to the solvent and stirred until completely dissolved. The precipitant solution is added dropwise to the precursor salt solution under vigorous stirring. After the dropwise addition is completed, the solution stirred until completely dissolved and the foam metal after the pretreatment in step 1) are added to the lining of the hydrothermal kettle, and then the lining of the hydrothermal kettle is installed in the hydrothermal kettle. The hydrothermal kettle is tightened and the hydrothermal kettle is installed in the homogeneous reactor for hydrothermal etching treatment. After the hydrothermal treatment is completed, the sample is taken out and washed several times. After the washing is completed, the sample is taken out and vacuum dried. After vacuum drying, it is calcined. After calcination, a foam metal carrier loaded with NiO can be obtained, which is recorded as NiO / M-foam; 3) Preparation of monolithic reversed Ni-based catalyst The NiO / M-foam metal foam carrier prepared in step 2) is dispersed in a deoxygenated nitrogen-protected solution, and then the precursor salt of the nano-oxide that adsorbs and activates CO2 and the precipitant are added, and then the mixed solution is transferred to the lining of the hydrothermal kettle and ultrasonically treated to evenly disperse the oxide precursor salt, and the hydrothermal kettle is tightened and installed in a homogeneous reactor, and then the hydrothermal kettle is transferred to the homogeneous reactor for hydrothermal treatment. After the hydrothermal treatment, the obtained sample is vacuum dried to completely remove the moisture in the sample, and finally the dried sample is calcined. After the calcination, a monolithic reversed Ni-based catalyst can be obtained, which is denoted as M n O x / NiO / M-foam.

4. The method for preparing a low-temperature, high-activity, high-selectivity, monolithic reversed-phase Ni-based catalyst for CO2 hydrogenation to methane according to claim 3, characterized in that Step 2) the precursor salt is selected from one or more of nickel nitrate, nickel chloride, nickel sulfate, nickel acetate, and nickel acetylacetonate; the solvent is selected from one or more of water, methanol, ethanol, butanol, tetrahydrofuran, and methyl tert-butyl ether; Step 2) The concentration of the precursor salt of metal Ni used to dissociate hydrogen is 0.01-5 mol / L.

5. The method for preparing a low-temperature, high-activity, high-selectivity, monolithic reversed-phase Ni-based catalyst for CO2 hydrogenation to methane according to claim 3, characterized in that Step 2) hydrothermally etching the metal foam and the precursor salt solution. The specific process is as follows: The foamed metal after the pretreatment in step 1) is fully mixed with the precursor salt solution of metal Ni, transferred to the lining of the hydrothermal reactor and placed in a homogeneous reactor, and subjected to hydrothermal treatment at 160-220° C. for 12-20 hours, and then the foamed metal loaded with metal Ni is dried in a vacuum oven for 12 hours, and then calcined at 250-350° C. for 0.5-2 hours to obtain the foamed metal carrier, which is recorded as NiO / M-foam; The precipitant is selected from urea, ammonium fluoride, ammonium chloride, ammonium oxalate and oxalic acid.

6. The method for preparing a low-temperature, high-activity, high-selectivity, monolithic reversed-phase Ni-based catalyst for CO2 hydrogenation to methane according to claim 3, characterized in that Step 3) the precursor salt is selected from one or more of aluminum nitrate, aluminum chloride; cerium nitrate, cerium chloride; zirconium nitrate, zirconium chloride, zirconium oxychloride; yttrium nitrate, yttrium chloride, yttrium acetylacetonate; magnesium nitrate, magnesium sulfate, magnesium chloride; the solvent used to dissolve the oxide precursor salt and the precipitant is selected from one or more of water, ethanol, butanol, and ethylene glycol; Step 3) The concentration of the precursor salt of the oxide that generates oxygen vacancies to adsorb and activate carbon dioxide is 0.01-5 mol / L.

7. The method for preparing a low-temperature, high-activity, high-selectivity, monolithic reversed-phase Ni-based catalyst for CO2 hydrogenation to methane according to claim 3, characterized in that Step 3) The hydrothermal temperature is 160-200°C; the hydrothermal time is 12-20 h; the drying temperature is 40~100°C and the drying time is 6~12 h.

8. The method for preparing a low-temperature, high-activity, high-selectivity, monolithic reversed-phase Ni-based catalyst for CO2 hydrogenation to methane according to claim 3, characterized in that Step 3) The feed ratio of the foam metal carrier to the nano-oxide precursor salt is 20:1-1:20; the stirring time is 1-3 h.

9. The method for preparing a low-temperature, high-activity, high-selectivity, monolithic reversed-phase Ni-based catalyst for CO2 hydrogenation to methane according to claim 3, characterized in that Step 3) The calcination temperature is 300-500°C and the calcination time is 1-4h.

10. Use of the monolithic reversed-phase Ni catalyst as claimed in claim 1 in a biogas upgrading process.

Citation Information

Patent Citations

  • Solid reverse catalyst, preparation method thereof and application of solid reverse catalyst in catalysis of low-temperature carbon dioxide methanation

    CN116060035A

Cited By

  • Catalyst for low-temperature methanation of CO2 as well as preparation method and application of catalyst

    CN120586891A

  • Solid-state metal catalyst insert, method for manufacturing the same, and microchannel reaction system thereof

    TWI926763B