Method for preparing cracking catalyst from waste catalyst, cracking catalyst and application of cracking catalyst

Through aluminum-soluble, silicon-soluble treatment and crystallization technology, the waste catalyst is converted into 13X molecular sieve, and high-efficiency cracking catalyst is prepared through two-step baking, which solves the problems of high catalyst cost and unenvironmental protection in the existing technology, and achieves high efficiency and economical And environmentally friendly cracking reaction.

CN118904385AActive Publication Date: 2024-11-08CHINA ENERGY GRP NINGXIA COAL IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410976181.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing cracking catalysts are costly and not environmentally friendly, making it difficult to effectively utilize waste catalyst resources, resulting in production interruptions and environmental pollution.

Method used

By dissolving the waste catalyst with aluminum and silicon dissolved treatment, silicon-rich liquid was prepared, and then mixed and added seeds to aged and crystallized to form a 13X molecular sieve, and mixed with a platinum precursor for two-step calcination. Produce efficient cracking catalyst.

Benefits of technology

The controllable specific surface area of ​​micro mesoporous pores and high hydrothermal stability are achieved, which reduces the production cost of catalysts, reduces the production of industrial waste, and improves the green sustainability of the cracking process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954578150000091
    Figure BDA0004954578150000091
  • Figure BDA0004954578150000102
    Figure BDA0004954578150000102
Patent Text Reader

Abstract

The invention provides a method for preparing a cracking catalyst from a waste catalyst, the cracking catalyst and application of the cracking catalyst. The method comprises the following steps: dissolving aluminum and silicon in a waste catalyst, adding a seed crystal, aging and crystallizing to obtain a 13X molecular sieve, mixing the 13X molecular sieve with a platinum precursor solution, filtering to obtain a catalyst precursor, pre-roasting the catalyst precursor in an inert gas atmosphere, and then roasting the catalyst precursor in an air atmosphere to obtain the cracking catalyst, wherein the waste catalyst comprises one or more of a waste Z-5 molecular sieve catalyst, a waste MTO catalyst, a waste molecular sieve adsorbent, fly ash, a waste FCC catalyst and a waste VOC adsorbent; the roasting temperature is higher than the pre-roasting temperature, and the temperature difference is 250-350 DEG C. The 13X molecular sieve is prepared from the waste catalyst resource, and the novel efficient cracking catalyst is prepared through two-step roasting, so that the production of industrial wastes can be reduced, the production cost of the catalyst is reduced, and the green sustainability of the cracking process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chemical synthesis, and in particular to a method for preparing a cracking catalyst from a waste catalyst, a cracking catalyst and an application thereof. Background Art

[0002] Cracking is a vital process in the petroleum refining and petrochemical industries. It converts heavier hydrocarbon feedstocks into lighter compounds with greater economic value, such as petroleum fuels, olefins and aromatics. The key to the cracking reaction is the use of efficient catalysts to promote the reaction.

[0003] Traditional cracking catalysts typically include acidic materials, such as zeolite molecular sieves, which can improve the selectivity and conversion rate of the reaction. However, over time, the catalysts will deactivate due to carbon and metal deposition, and need to be replaced, resulting in production interruptions and the generation of catalyst waste.

[0004] In addition, due to the limited fossil fuel resources and increasing environmental pressure, finding and developing more efficient, economical and environmentally friendly cracking catalysts has become an important issue in this field. Summary of the invention

[0005] The main purpose of the present invention is to provide a method for preparing a cracking catalyst from a waste catalyst, a cracking catalyst and application thereof, so as to solve the problems of high cost and environmental pollution of the cracking catalyst in the prior art.

[0006] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a cracking catalyst from a waste catalyst is provided, comprising the following steps: step S1, dissolving aluminum and silicon in the waste catalyst to obtain a silicon-rich liquid and an aluminum-rich liquid, mixing the silicon-rich liquid and the aluminum-rich liquid to obtain a gel-like mother liquor; adding seed crystals to the gel-like mother liquor, and then performing an aging treatment and a crystallization treatment in sequence, and obtaining a 13X molecular sieve after drying; step S2, mixing the 13X molecular sieve with a platinum precursor solution, stirring for 12 to 36 hours, and then filtering, and the filter cake is heated to 90°C. The catalyst precursor is dried at 130°C for 8 to 16 hours to obtain a catalyst precursor; in step S3, the catalyst precursor is pre-calcined in an inert gas atmosphere to obtain a pre-calcined product; in step S4, the pre-calcined product is calcined in an air atmosphere to obtain a cracking catalyst; wherein the waste catalyst includes one or more of waste Z-5 molecular sieve catalyst, waste MTO catalyst, waste molecular sieve adsorbent, fly ash, waste FCC catalyst and waste VOC adsorbent; wherein the calcination temperature is greater than the pre-calcination temperature, and the temperature difference is 250 to 350°C.

[0007] Furthermore, in step S3, the pre-calcination temperature is 450-550° C. and the time is 1-3 hours.

[0008] Furthermore, in step S4, the calcination temperature is 700-900° C. and the calcination time is 3-5 hours.

[0009] Further, in step S1, dissolving aluminum includes: mixing the spent catalyst with NaCO 3 The mixture is mixed, calcined at 550-800°C for 60-120 min, and then the calcined product is dissolved with a monobasic acid and filtered to obtain an aluminum-rich liquid and an aluminum-dissolving filter residue; preferably, the spent catalyst is mixed with NaCO 3 The mass ratio of is 1:(0.5-1:5); and / or the mass concentration of monobasic acid is 10-35%; silicon dissolving comprises: mixing the aluminum dissolving residue with NaOH, H 2 O mixed, filtered to obtain silicon-rich liquid; preferably, the aluminum-dissolving filter residue is mixed with NaOH, H 2 The mass ratio of O is (2~100):(40~60):(50~400).

[0010] Furthermore, in step S1, the molar ratio of the components in the gel mother solution is: SiO 2 / Al 2 O 3 =(0.5~6.0):1,Na 2 O / SiO 2 =(0.5~6.0):1,H 2 O / SiO 2 =(10-100):1; Preferably, the amount of seed crystal added accounts for 5-20wt% of the gel mother liquor by weight percentage.

[0011] Furthermore, in step S1, aging is carried out under stirring conditions at a temperature of 20 to 100° C. for 0.1 to 24 h; and / or crystallization is carried out at a temperature of 60 to 105° C. for 0.1 to 36 h.

[0012] Furthermore, the silicon-aluminum ratio of 13X molecular sieve is 2.2-2.9, and the pore volume is 0.3-0.5 cm 3 / g, specific surface area is 700~950m 2 / g.

[0013] Furthermore, the molar ratio of each component in the seed crystal is: SiO 2 / Al 2 O 3 =(0.1~2.5):1,Na 2 O / SiO 2 =(0.1~4.0):1,H 2 O / SiO 2 =(1.0~40.0):1.

[0014] Furthermore, in step S1, the seed crystal is prepared using the following method: step S11, mixing a silicon source and water to obtain a silicon-containing material; mixing an aluminum source and water to obtain an aluminum-containing material; step S12, adding the aluminum-containing material dropwise to the silicon-containing material, stirring, to obtain a mixture gel; adjusting the pH value of the mixture gel to 8.5-12.5, and then performing two-stage hydrothermal crystallization treatment to obtain a seed crystal.

[0015] Further, in step S11, the silicon source includes one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash and white carbon black; the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; and / or in step S12, the stirring temperature is 20-100°C, and the time is 0.1-24h; and / or two-stage hydrothermal crystallization is carried out in a hydrothermal reactor, including a first stage hydrothermal crystallization and a second stage hydrothermal crystallization carried out in sequence, the temperature of the second stage hydrothermal crystallization is greater than that of the first stage hydrothermal crystallization, and the temperature difference is 50-60°C; preferably, the temperature of the first stage hydrothermal crystallization is 20-60°C, and the time is 4-24h; the temperature of the second stage hydrothermal crystallization is 80-120°C, and the time is 6-48h.

[0016] According to another aspect of the present invention, there is provided a cracking catalyst, which is prepared by the above-mentioned preparation method of the present invention.

[0017] According to another aspect of the present invention, there is provided the use of the above-mentioned cracking catalyst of the present invention in cracking reactions in the fields of petrochemical industry, coal chemical industry and waste plastic treatment.

[0018] By applying the technical solution of the present invention, waste catalyst resources are used to prepare 13X molecular sieves, which have controllable micro-mesopore specific surface area and large pore volume, high hydrothermal stability, a wide silicon-aluminum ratio range, and controllable morphology; and then a new type of high-efficiency cracking catalyst is prepared through a two-step roasting process, which can not only reduce the generation of industrial waste, but also help to reduce the production cost of the catalyst while ensuring the catalytic cracking effect, thereby improving the green sustainability of the cracking process. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0020] As described in the background of the present invention, the prior art has the problem of high cost and environmental pollution of cracking catalysts. In order to solve the above problems, in a typical embodiment of the present invention, a method for preparing cracking catalysts from waste catalysts is provided, comprising the following steps: Step S1, dissolving aluminum and silicon in the waste catalyst to obtain silicon-rich liquid and aluminum-rich liquid, mixing the silicon-rich liquid and the aluminum-rich liquid to obtain a gel-like mother liquor; adding seed crystals to the gel-like mother liquor, and then performing aging and crystallization treatments in sequence, and drying to obtain 13X molecular sieves; Step S2, mixing the 13X molecular sieve with a platinum precursor solution, stirring for 12 to 36 hours, and then filtering, and the filter cake is 9 The step of drying the catalyst precursor at 0 to 130° C. for 8 to 16 hours obtains a catalyst precursor; in step S3, pre-calcining the catalyst precursor in an inert gas atmosphere to obtain a pre-calcined product; in step S4, calcining the pre-calcined product in an air atmosphere to obtain a cracking catalyst; wherein the waste catalyst comprises one or more of a waste Z-5 molecular sieve catalyst, a waste MTO catalyst, a waste molecular sieve adsorbent, fly ash, a waste FCC catalyst and a waste VOC adsorbent; wherein the calcination temperature is greater than the pre-calcination temperature, and the temperature difference is 250 to 350° C.

[0021] The present invention firstly dissolves aluminum and silicon in one or more waste catalysts including waste Z-5 molecular sieve catalyst, waste MTO catalyst, waste molecular sieve adsorbent, fly ash, waste FCC catalyst and waste VOC adsorbent, recycles the active components aluminum and silicon therein, obtains silicon-rich liquid and aluminum-rich liquid, mixes them to obtain gel mother liquor, adds crystal seeds, and performs aging treatment and crystallization treatment in sequence to shape its structure, and obtains 13X molecular sieve after drying, which has controllable micro-mesoporous specific surface area and large pore volume, high water content, and high molecular weight. Thermal stability, a wide range of silicon-aluminum ratios, and controllable morphology; then the 13X molecular sieve is mixed with a platinum precursor solution, stirred for 12 to 36 hours for preliminary platinum loading, and the filter cake is dried at 90 to 130°C for 8 to 16 hours after filtration to obtain a catalyst precursor; finally, the catalyst precursor is pre-baked in an inert gas atmosphere, and then calcined in an air atmosphere at a temperature of 250 to 350°C, and the platinum precursor is converted into highly dispersed metal oxide platinum or platinum metal by high-temperature oxidation calcination to obtain a cracking catalyst. The inert gas can be conventional nitrogen, argon, etc. in the art. The platinum precursor includes hexachloroplatinic acid dihydrate.

[0022] The present invention utilizes waste catalyst resources to prepare a new type of high-efficiency cracking catalyst through regeneration or modification, which can not only reduce the generation of industrial waste, but also help to reduce the production cost of the catalyst and improve the green sustainability of the cracking process.

[0023] In a preferred embodiment, in step S2, the mass ratio of 13X molecular sieve to platinum precursor is 100:(0.8-1.2), which can make the material containing catalytic metal platinum more fully loaded in the molecular sieve.

[0024] To further improve the low-temperature inert calcination effect, in a preferred embodiment, in step S3, the pre-calcination temperature is 450-550° C. and the time is 1-3 hours.

[0025] Accordingly, in order to more fully convert the platinum precursor into highly dispersed active platinum, in a preferred embodiment, in step S4, the calcination temperature is 700-900°C and the time is 3-5 hours, which can further improve the high-temperature oxidation calcination effect.

[0026] In a preferred embodiment, in step S1, dissolving aluminum includes: mixing the spent catalyst with NaCO 3 The mixture is mixed, calcined at 550-800°C for 60-120 min, and then the calcined product is dissolved with a monobasic acid and filtered to obtain an aluminum-rich liquid and an aluminum-dissolving filter residue; preferably, the spent catalyst is mixed with NaCO 3 The mass ratio of is 1:(0.5-1:5); and / or the mass concentration of monobasic acid is 10-35%; silicon dissolving comprises: mixing the aluminum dissolving residue with NaOH, H 2 O mixed, filtered to obtain silicon-rich liquid; preferably, the aluminum-dissolving filter residue is mixed with NaOH, H 2 The mass ratio of O is (2-100):(40-60):(50-400). Under the above conditions, the active components of aluminum and silicon in the spent catalyst can be more fully recycled, reducing the production cost of the catalyst and improving the green sustainability of the cracking process. Wherein, the monoacid uses the conventional definition in the art, such as hydrochloric acid, nitric acid, etc.

[0027] In order to improve the preparation effect of 13X molecular sieve, in a preferred embodiment, in step S1, the molar ratio of each component in the gel mother solution is: SiO 2 / Al 2 O 3 =(0.5~6.0):1,Na 2 O / SiO 2 =(0.5~6.0):1,H 2 O / SiO 2 =(10-100):1; Preferably, the amount of seed crystal added accounts for 5-20wt% of the gel mother liquor by weight percentage.

[0028] Based on similar reasons, in a preferred embodiment, in step S1, aging is carried out under stirring conditions at a temperature of 20 to 100°C for 0.1 to 24 hours; and / or the crystallization temperature is 60 to 105°C for 0.1 to 36 hours.

[0029] As described above, the 13X molecular sieve prepared by the present invention has controllable micro-mesoporous specific surface area and large pore volume, high hydrothermal stability, wide range of silicon-aluminum ratio, and controllable morphology. In a preferred embodiment, the silicon-aluminum ratio of the 13X molecular sieve is 2.2-2.9, and the pore volume is 0.3-0.5 cm 3 / g, specific surface area is 700~950m 2 / g, can provide more adsorption sites, introduce mesoporous channels, increase the pore volume inside the molecular sieve crystal, improve the flow and diffusion performance of the guest molecules inside the molecular sieve, have high silicon source utilization rate and good selectivity, and can be regulated according to different adsorption molecules, thereby significantly reducing the carbon deposition rate of the molecular sieve and facilitating the preparation of subsequent cracking catalysts.

[0030] To further promote the smooth formation of the structure of 13X molecular sieve, in a preferred embodiment, the molar ratio of each component in the seed crystal is: SiO 2 / Al 2 O 3 =(0.1~2.5):1,Na 2 O / SiO 2 =(0.1~4.0):1,H 2 O / SiO 2 =(1.0~40.0):1.

[0031] In a preferred embodiment, in step S1, the seed crystal is prepared using the following method: step S11, mixing a silicon source and water to obtain a silicon-containing material; mixing an aluminum source and water to obtain an aluminum-containing material; step S12, adding the aluminum-containing material dropwise to the silicon-containing material, stirring, to obtain a mixture gel; adjusting the pH value of the mixture gel to 8.5-12.5, and then performing two-stage hydrothermal crystallization treatment to obtain a seed crystal, which is more suitable for the preparation process of the 13X molecular sieve of the present invention.

[0032] To further improve the diffusion performance of 13X molecular sieve, in a preferred embodiment, in step S11, the silicon source includes one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash and white carbon black; the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; and / or the silicon source and water are generally stirred at 20-60° C. for 0.1-12 h, and the stirring speed is maintained at 200-800 rpm; the aluminum source and water are generally stirred at 20-60° C. for 0.1-12 h, and the stirring speed is preferably maintained at 200-800 rpm, the mass concentration of the silicon-containing material is 28-99 wt%, and the mass concentration of the aluminum-containing material is 15-99 wt%. And / or in step S12, the stirring temperature is 20-100° C. and the time is 0.1-24 h.

[0033] And / or two-stage hydrothermal crystallization is carried out in a hydrothermal reactor, including a first stage hydrothermal crystallization and a second stage hydrothermal crystallization carried out in sequence, the temperature of the second stage hydrothermal crystallization is greater than that of the first stage hydrothermal crystallization, and the temperature difference is 50-60°C; preferably, the temperature of the first stage hydrothermal crystallization is 20-60°C, and the time is 4-24h; the temperature of the second stage hydrothermal crystallization is 80-120°C, and the time is 6-48h. More preferably, the temperature of the first stage hydrothermal crystallization is 35-45°C, and the time is 11-13h; the temperature of the second stage hydrothermal crystallization is 90-100°C, and the time is 22-26h.

[0034] Through precise control of pH, crystallization temperature, raw material ratio, etc., the uniform arrangement of pores, specific surface area, and pore capacity can be more accurately controlled, thereby facilitating the preparation of molecular sieves with better performance.

[0035] In another typical embodiment of the present invention, a cracking catalyst is provided, which is prepared by the above-mentioned preparation method of the present invention, has significantly reduced production costs and can improve the green sustainability of the cracking process.

[0036] In another typical embodiment of the present invention, there is also provided the use of the above-mentioned cracking catalyst of the present invention in cracking reactions in the fields of petrochemical industry, coal chemical industry and waste plastic treatment.

[0037] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0038] Example 1

[0039] Seed preparation: 21.0g silica sol (mass fraction of 30%) was dissolved in 36.0g deionized water, and pretreated in a closed reactor at 25°C and 500rpm for 1 hour to obtain a dispersed phase aqueous solution of the silicon source; 24g aluminum sulfate was dissolved in 18.0g deionized water, and stirred at 25°C and 500rpm for 1h to obtain a dispersed phase aqueous solution of the aluminum source; the aqueous solution of the aluminum source was slowly added dropwise to the aqueous solution of the silicon source, and continued to stir at 60°C for 8h to obtain a gel solution; 6.74g sodium hydroxide was dissolved in 36g deionized water dispersion and added to the gel solution, and the pH value was controlled to be maintained at 12.2. The obtained gel solution was placed in a hydrothermal reactor and subjected to two-stage temperature-controlled crystallization. The first stage was at a crystallization temperature of 40°C and a time of 12 hours, and the second stage was at a crystallization temperature of 95°C and a time of 24 hours. Deionized water was added as needed during the crystallization process to obtain a seed solution.

[0040] Step S1, waste Z-5 molecular sieve catalyst and NaCO 3 The mixture was mixed in a mass ratio of 1:1, calcined at 700°C for 90 min, and then the calcined product was dissolved with a monobasic acid having a mass concentration of 20%, and filtered to obtain an aluminum-rich liquid and an aluminum-dissolving residue; the aluminum-dissolving residue was mixed with NaOH and H 2 O are mixed in a mass ratio of 50:50:200, filtered to obtain a silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a gel mother liquid; seed crystals accounting for 15wt% of the gel mother liquid are added to the gel mother liquid, and then aging treatment and crystallization treatment are performed in sequence, the aging temperature is 60°C, the time is 12h; the crystallization temperature is 80°C, the time is 18h, and after drying, a 13X molecular sieve is obtained;

[0041] Step S2, take 100 g of 13X molecular sieve and dry it at 110°C for 4 hours to remove the adsorbed water. After completion, cool it to room temperature. 2 PtCl 6 ·2H 2 O) was dissolved in 500 mL of deionized water to form a platinum precursor solution. The dried 13X molecular sieve was added to the prepared platinum precursor solution and stirred for 24 hours using a magnetic stirrer. Then, the filtered molecular sieve was placed in a drying oven and further dried at 110°C for 12 hours to obtain a catalyst precursor;

[0042] Step S3, placing the catalyst precursor in a molybdenum cloth furnace and pre-baking it in an inert gas atmosphere at a temperature of 500° C. for 2 hours to obtain a pre-baked product;

[0043] Step S4, calcining the pre-calcined product in an air atmosphere at a temperature of 800° C. for 4 hours to obtain a cracking catalyst.

[0044] Example 2

[0045] The difference from Example 1 is that

[0046] Seed preparation: 1g silicon powder was dissolved in 18g deionized water, and pretreated in a closed reactor at 25°C and 500rpm for 1 hour to obtain a dispersed phase aqueous solution of silicon source; 12g aluminum nitrate was dissolved in 18.0g deionized water, and stirred at 35°C and 500rpm for 1 hour to prepare a dispersed phase aqueous solution of aluminum source. The prepared aluminum source aqueous solution was slowly added to the silicon source aqueous solution, and continued to stir at 50°C for 6 hours to obtain a gel solution; 2g sodium hydroxide was dissolved in 36g deionized water to obtain a dispersion, which was slowly added to the gel solution, and the pH value was controlled at 11.8, and then the mixed gel solution was transferred to a hydrothermal reactor to perform a two-stage temperature-controlled crystallization process: the first stage crystallization temperature was set at 50°C and lasted for 14 hours; the second stage crystallization temperature was controlled at 100°C and maintained for 18 hours. Deionized water was added as needed during the crystallization process to obtain a seed solution.

[0047] Example 3

[0048] The difference from Example 1 is that

[0049] Seed preparation: 0.17g silicon powder was dissolved in 6g deionized water, and pretreated in a closed reactor at 25°C and 200rpm for 1 hour to obtain a dispersed phase aqueous solution of silicon source; 12g aluminum nitrate was dissolved in 18.0g deionized water, and stirred at 35°C and 200rpm for 1 hour to prepare a dispersed phase aqueous solution of aluminum source. The aluminum source solution was slowly added to the silicon source solution, and stirred at 100°C for 24 hours to obtain a gel solution; 0.9g sodium hydroxide was dissolved in 6g deionized water to obtain a dispersion, and then slowly added to the gel solution E, and the pH value was adjusted to 12.5. After that, the prepared gel was poured into a hydrothermal reactor for two-stage crystallization. First, crystallization lasted for 24 hours at 60°C, and then the temperature was raised to 120°C for crystallization reaction for 48 hours. Deionized water was added as needed during the crystallization process to obtain a seed solution.

[0050] Step S1, waste FCC catalyst and NaCO 3 The mixture was mixed in a mass ratio of 1:0.5, calcined at 550°C for 120 min, and then the calcined product was dissolved with a monobasic acid with a mass concentration of 10%, filtered to obtain an aluminum-rich liquid and an aluminum-dissolving residue; the aluminum-dissolving residue was mixed with NaOH and H 2O are mixed in a mass ratio of 2:40:50, filtered to obtain a silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a gel mother liquor; 5 wt% of seed crystals are added to the gel mother liquor, and then aging and crystallization are performed in sequence, the aging temperature is 20° C., the time is 24 h; the crystallization temperature is 60° C., the time is 36 h, and 13X molecular sieve is obtained after drying;

[0051] Step S2, take 100 g of 13X molecular sieve and dry it at 110°C for 4 hours to remove the adsorbed water. After completion, cool it to room temperature. 2 PtCl 6 ·2H 2 O) was dissolved in 500 mL of deionized water to form a platinum precursor solution. The dried 13X molecular sieve was added to the prepared platinum precursor solution and stirred for 12 hours using a magnetic stirrer. Then, the filtered molecular sieve was placed in a drying oven and further dried at 90° C. for 16 hours to obtain a catalyst precursor.

[0052] Example 4

[0053] The difference from Example 1 is that

[0054] Seed preparation: 14.65g of ethyl orthosilicate was mixed with 36g of deionized water, and pretreated in a closed reactor at 25°C and 800rpm for 1 hour to obtain a dispersed phase aqueous solution of the silicon source; 12g of aluminum nitrate was dissolved in 18.0g of deionized water, and stirred at 35°C and 800rpm for 1 hour to obtain a dispersed phase aqueous solution of the aluminum source. The aluminum source solution was gradually added dropwise to the silicon source solution, and mixed and stirred at 20°C for 0.1 hour to prepare a gel solution; 0.56g of sodium hydroxide was dissolved in 6g of deionized water as a dispersion liquid, and slowly poured into the gel solution, maintaining the pH value at 8.5, and the prepared gel was introduced into the hydrothermal reactor to perform a segmented crystallization reaction: first, the crystallization temperature was set to 20°C for 4 hours; then it was raised to 80°C and maintained for 6 hours. During the crystallization process, deionized water was added as needed to obtain a seed solution.

[0055] Step S1, waste molecular sieve adsorbent and NaCO 3 The mixture was mixed in a mass ratio of 1:1.5, calcined at 800°C for 60 min, and then the calcined product was dissolved with a monobasic acid having a mass concentration of 35%, and filtered to obtain an aluminum-rich liquid and an aluminum-dissolving residue; the aluminum-dissolving residue was mixed with NaOH and H 2O are mixed in a mass ratio of 100:60:400, filtered to obtain a silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a gel mother liquid; crystal seeds accounting for 20wt% of the gel mother liquid are added to the gel mother liquid, and then aging treatment and crystallization treatment are performed in sequence, the aging temperature is 100°C, the time is 0.1h; the crystallization temperature is 105°C, the time is 0.1h, and after drying, a 13X molecular sieve is obtained;

[0056] Step S2, take 100 g of 13X molecular sieve and dry it at 110°C for 4 hours to remove the adsorbed water. After completion, cool it to room temperature. 2 PtCl 6 ·2H 2 O) was dissolved in 500 mL of deionized water to form a platinum precursor solution. The dried 13X molecular sieve was added to the prepared platinum precursor solution and stirred for 36 hours using a magnetic stirrer. Then, the filtered molecular sieve was placed in a drying oven and further dried at 130° C. for 8 hours to obtain a catalyst precursor.

[0057] Example 5

[0058] Seed preparation: 21.0g silica sol (mass fraction of 30%) was dissolved in 36.0g deionized water, and pretreated in a closed reactor at 25°C and 500rpm for 1 hour to obtain a dispersed phase aqueous solution of the silicon source; 24g aluminum sulfate was dissolved in 18.0g deionized water, and stirred at 25°C and 500rpm for 1h to obtain a dispersed phase aqueous solution of the aluminum source; the aqueous solution of the aluminum source was slowly added dropwise to the aqueous solution of the silicon source, and continued to stir at 60°C for 8h to obtain a gel solution; 6.74g sodium hydroxide was dissolved in 36g deionized water dispersion and added to the gel solution, and the pH value was controlled to be maintained at 12.2. The obtained gel solution was placed in a hydrothermal reactor and subjected to two-stage temperature-controlled crystallization. The first stage was at a crystallization temperature of 40°C and a time of 12 hours, and the second stage was at a crystallization temperature of 95°C and a time of 24 hours. Deionized water was added as needed during the crystallization process to obtain a seed solution.

[0059] Step S1, waste Z-5 molecular sieve catalyst and NaCO 3 The mixture was mixed in a mass ratio of 1:1, calcined at 700°C for 90 min, and then the calcined product was dissolved with a monobasic acid having a mass concentration of 20%, and filtered to obtain an aluminum-rich liquid and an aluminum-dissolving residue; the aluminum-dissolving residue was mixed with NaOH and H 2O are mixed in a mass ratio of 50:50:200, filtered to obtain a silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a gel mother liquid; seed crystals accounting for 15wt% of the gel mother liquid are added to the gel mother liquid, and then aging treatment and crystallization treatment are performed in sequence, the aging temperature is 60°C, the time is 12h; the crystallization temperature is 80°C, the time is 18h, and after drying, a 13X molecular sieve is obtained;

[0060] Step S2, take 100 g of 13X molecular sieve and dry it at 110°C for 4 hours to remove the adsorbed water. After completion, cool it to room temperature. 2 PtCl 6 ·2H 2 O) was dissolved in 500 mL of deionized water to form a platinum precursor solution. The dried 13X molecular sieve was added to the prepared platinum precursor solution and stirred for 24 hours using a magnetic stirrer. Then, the filtered molecular sieve was placed in a drying oven and further dried at 110°C for 12 hours to obtain a catalyst precursor;

[0061] Step S3, placing the catalyst precursor in a molybdenum cloth furnace, and pre-baking it in an inert gas atmosphere at a temperature of 450° C. for 3 hours to obtain a pre-baked product;

[0062] Step S4, calcining the pre-calcined product in an air atmosphere at a temperature of 700° C. for 5 hours to obtain a cracking catalyst.

[0063] Example 6

[0064] Seed preparation: 21.0g silica sol (mass fraction of 30%) was dissolved in 36.0g deionized water, and pretreated in a closed reactor at 25°C and 500rpm for 1 hour to obtain a dispersed phase aqueous solution of the silicon source; 24g aluminum sulfate was dissolved in 18.0g deionized water, and stirred at 25°C and 500rpm for 1h to obtain a dispersed phase aqueous solution of the aluminum source; the aqueous solution of the aluminum source was slowly added dropwise to the aqueous solution of the silicon source, and continued to stir at 60°C for 8h to obtain a gel solution; 6.74g sodium hydroxide was dissolved in 36g deionized water dispersion and added to the gel solution, and the pH value was controlled to be maintained at 12.2. The obtained gel solution was placed in a hydrothermal reactor and subjected to two-stage temperature-controlled crystallization. The first stage was at a crystallization temperature of 40°C and a time of 12 hours, and the second stage was at a crystallization temperature of 95°C and a time of 24 hours. Deionized water was added as needed during the crystallization process to obtain a seed solution.

[0065] Step S1, waste Z-5 molecular sieve catalyst and NaCO 3The mixture was mixed in a mass ratio of 1:1, calcined at 700°C for 90 min, and then the calcined product was dissolved with a monobasic acid having a mass concentration of 20%, and filtered to obtain an aluminum-rich liquid and an aluminum-dissolving residue; the aluminum-dissolving residue was mixed with NaOH and H 2 O are mixed in a mass ratio of 50:50:200, filtered to obtain a silicon-rich liquid; the silicon-rich liquid and the aluminum-rich liquid are mixed to obtain a gel mother liquid; seed crystals accounting for 15wt% of the gel mother liquid are added to the gel mother liquid, and then aging treatment and crystallization treatment are performed in sequence, the aging temperature is 60°C, the time is 12h; the crystallization temperature is 80°C, the time is 18h, and after drying, a 13X molecular sieve is obtained;

[0066] Step S2, take 100 g of 13X molecular sieve and dry it at 110°C for 4 hours to remove the adsorbed water. After completion, cool it to room temperature. 2 PtCl 6 ·2H 2 O) was dissolved in 500 mL of deionized water to form a platinum precursor solution. The dried 13X molecular sieve was added to the prepared platinum precursor solution and stirred for 24 hours using a magnetic stirrer. Then, the filtered molecular sieve was placed in a drying oven and further dried at 110°C for 12 hours to obtain a catalyst precursor;

[0067] Step S3, placing the catalyst precursor in a molybdenum cloth furnace and pre-baking it in an inert gas atmosphere at a temperature of 550° C. for 1 hour to obtain a pre-baked product;

[0068] Step S4, calcining the pre-calcined product in an air atmosphere at a temperature of 900° C. for 3 hours to obtain a cracking catalyst.

[0069] Comparative Example 1

[0070] The difference from Example 1 is that no pre-baking was performed.

[0071] Comparative Example 2

[0072] The difference from Example 1 is that

[0073] Step S3, placing the catalyst precursor in a molybdenum cloth furnace, and pre-baking it in an inert gas atmosphere at a temperature of 350° C. for 3 hours to obtain a pre-baked product;

[0074] Step S4, calcining the pre-calcined product in an air atmosphere at a temperature of 950° C. for 5 hours to obtain a cracking catalyst.

[0075] Comparative Example 3

[0076] The difference from Example 1 is that

[0077] Step S3, placing the catalyst precursor in a molybdenum cloth furnace, and pre-baking it in an inert gas atmosphere at a temperature of 650° C. for 1 hour to obtain a pre-baked product;

[0078] Step S4, calcining the pre-calcined product in an air atmosphere at a temperature of 600° C. for 3 hours to obtain a cracking catalyst.

[0079] The molar ratios of the components in the seed crystals and the gel-like mother liquor, and the performance test results of the 13X molecular sieve and the cracking catalyst in the above examples and comparative examples are shown in Tables 1 and 2.

[0080] Test method:

[0081] Molar ratio, silicon-aluminum ratio: X-ray fluorescence spectrometry (XRF);

[0082] Pore ​​volume, specific surface area: BET test method.

[0083] Catalytic rate, selectivity, and total triene yield: The cracking catalyst is used in the reaction of preparing trienes (trienes are ethylene, propylene, and butadiene) by steam cracking of naphtha. The specific reaction conditions are: reaction temperature is 550°C, reaction pressure is 80KPa, reaction time is set to 2 hours, and water-oil mass ratio is 0.6.

[0084] Table 1

[0085]

[0086]

[0087] Table 2

[0088]

[0089] As can be seen from the above, compared with the comparative example, the embodiments of the present invention use waste catalyst resources to prepare 13X molecular sieves, which have controllable micro-mesoporous specific surface area and large pore volume, high hydrothermal stability, wide silicon-aluminum ratio range, and controllable morphology; and then prepare a new type of high-efficiency cracking catalyst through two-step roasting, which can not only reduce the generation of industrial waste, but also help reduce the production cost of the catalyst and improve the green sustainability of the cracking process. In addition, it can be seen that when all process parameters are within the preferred range of the present invention, the comprehensive performance of the prepared catalyst is better.

[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a cracking catalyst from a waste catalyst, characterized in that: The following steps are involved: Step S1, dissolving aluminum and silicon in the waste catalyst to obtain silicon-rich liquid and aluminum-rich liquid, mixing the silicon-rich liquid and the aluminum-rich liquid to obtain a gel mother liquor; adding seed crystals to the gel mother liquor, and then performing aging and crystallization treatments in sequence, and obtaining a 13X molecular sieve after drying; Step S2, mixing the 13X molecular sieve with a platinum precursor solution, stirring for 12 to 36 hours, and then filtering, and drying the filter cake at 90 to 130° C. for 8 to 16 hours to obtain a catalyst precursor; Step S3, pre-calcining the catalyst precursor under an inert gas atmosphere to obtain a pre-calcined product; Step S4, calcining the pre-calcined product in an air atmosphere to obtain the cracking catalyst; Wherein, the waste catalyst includes one or more of waste Z-5 molecular sieve catalyst, waste MTO catalyst, waste molecular sieve adsorbent, fly ash, waste FCC catalyst and waste VOC adsorbent; Wherein, the calcination temperature is greater than the pre-calcination temperature, and the temperature difference is 250-350°C.

2. The method for preparing cracking catalyst from waste catalyst according to claim 1, characterized in that: In step S3, the pre-baking temperature is 450-550° C. and the time is 1-3 hours; and / or In the step S4, the calcination temperature is 700-900° C. and the calcination time is 3-5 hours.

3. The method for preparing cracking catalyst from waste catalyst according to claim 1 or 2, characterized in that: In the step S1, The aluminum dissolving process comprises: mixing the waste catalyst with NaCO3, calcining at 550-800°C for 60-120min, then dissolving the calcined product with a monoacid, filtering, and obtaining an aluminum-rich liquid and an aluminum-dissolving filter residue; preferably, the mass ratio of the waste catalyst to NaCO3 is 1:(0.5-1:5); and / or the mass concentration of the monoacid is 10-35%; The silicon dissolving process comprises: mixing the aluminum dissolving filter residue with NaOH and H2O, filtering and obtaining silicon-rich liquid; preferably, the mass ratio of the aluminum dissolving filter residue to NaOH and H2O is (2-100):(40-60):(50-400).

4. The method for preparing a cracking catalyst from a waste catalyst according to any one of claims 1 to 3, characterized in that: In the step S1, the molar ratio of the components in the gel mother solution is: SiO2 / Al2O3=(0.5-6.0):1, Na2O / SiO2=(0.5-6.0):1, H2O / SiO2=(10-100):1; Preferably, in terms of weight percentage, the amount of the seed crystals added is 5-20 wt % of the gel-like mother solution.

5. The method for preparing a cracking catalyst from a waste catalyst according to any one of claims 1 to 4, characterized in that: In the step S1, The aging is carried out under stirring conditions at a temperature of 20 to 100° C. for a time of 0.1 to 24 h; and / or The crystallization temperature is 60-105° C., and the crystallization time is 0.1-36 hours.

6. The method for preparing a cracking catalyst from a spent catalyst according to any one of claims 1 to 5, characterized in that: The 13X molecular sieve has a silicon-aluminum ratio of 2.2 to 2.9 and a pore volume of 0.3 to 0.5 cm 3 / g, specific surface area is 700~950m 2 / g; and / or The molar ratio of each component in the seed crystal is: SiO2 / Al2O3=(0.1-2.5):1, Na2O / SiO2=(0.1-4.0):1, H2O / SiO2=(1.0~40.0):

1.

7. The method for preparing a cracking catalyst from a waste catalyst according to any one of claims 1 to 6, characterized in that: In step S1, the seed crystal is prepared by the following method: Step S11, mixing a silicon source and water to obtain a silicon-containing material; mixing an aluminum source and water to obtain an aluminum-containing material; Step S12, adding the aluminum-containing material dropwise to the silicon-containing material, stirring, and obtaining a mixture gel; adjusting the pH value of the mixture gel to 8.5-12.5, and then performing two-stage hydrothermal crystallization treatment to obtain the seed crystal.

8. The method for preparing cracking catalyst from waste catalyst according to claim 7, characterized in that: In the step S11, the silicon source includes one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash and white carbon black; the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; and / or In the step S12, the stirring temperature is 20-100°C, and the time is 0.1-24h; and / or the two-stage hydrothermal crystallization is carried out in a hydrothermal reactor, including a first stage hydrothermal crystallization and a second stage hydrothermal crystallization carried out in sequence, the temperature of the second stage hydrothermal crystallization is greater than that of the first stage hydrothermal crystallization, and the temperature difference is 50-60°C; preferably, the temperature of the first stage hydrothermal crystallization is 20-60°C, and the time is 4-24h; the temperature of the second stage hydrothermal crystallization is 80-120°C, and the time is 6-48h.

9. A cracking catalyst, characterized in that: The cracking catalyst is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the cracking catalyst according to claim 9 in cracking reactions in the fields of petrochemical industry, coal chemical industry and waste plastic treatment.

Citation Information

Patent Citations

  • Method for preparing 13X zeolite molecular sieve by kaolin containing illite

    CN103073023A

  • Preparation method of hydrocracking catalyst

    CN104588077A

  • Method for preparing 13X molecular sieve by cooperation of coal gangue and coal ash desilication liquid

    CN105800643A

  • 13X zeolite molecular sieve, preparation method therefor and application of 13X zeolite molecular sieve

    CN106542542A

  • Monolithic catalyst and preparation and application thereof

    CN107694562A