Application of fullerene composite material in photocatalytic production of hydrogen-rich water

Through the application of fullerene composite materials in photocatalysis, the existing high production costs and pollution problems of hydrogen-rich water are solved, and safe, efficient and low-cost production of hydrogen-rich water is achieved, and metal pollution is avoided.

CN118904389APending Publication Date: 2024-11-08INST OF CHEM CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410841174.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing hydrogen-rich water production methods are costly, inefficient and prone to metal pollutants, which pose low efficiency and pollution risks.

Method used

Fullerene composite materials, including fullerene or its derivatives and photocatalyst materials, are used for photocatalytic production of hydrogen-rich water, through fullerene derivatives such as amyotrophy, carboxylation, hydroxylated derivatives and carbon quantum Point composite materials improve photocatalytic hydrogen production efficiency and stability.

Benefits of technology

It realizes safe, low-cost, pollution-free and efficient hydrogen-rich water production, and the composite material has a stable structure and is easy to recycle, reducing the risk of metal pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004914414950000021
    Figure BDA0004914414950000021
  • Figure BDA0004914414950000081
    Figure BDA0004914414950000081
  • Figure BDA0004914414950000082
    Figure BDA0004914414950000082
Patent Text Reader

Abstract

The invention belongs to the field of photocatalysis, and particularly relates to application of a fullerene composite material in photocatalytic production of hydrogen-rich water. The fullerene composite material comprises a fullerene (derivative) semiconductor composite material and a fullerene (derivative) photosensitizer (derivative) composite material. The fullerene photocatalytic material has a wide spectral absorption range, the utilization efficiency of light is increased, the separation efficiency of electrons and holes is increased by fullerene, and the photocatalytic performance is greatly improved. The fullerene photocatalytic material can safely, efficiently and stably decompose water to prepare hydrogen under the irradiation of sunlight, and safe, green, efficient and low-cost production of hydrogen-rich water can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photocatalysis, and specifically relates to the application of fullerene composite materials in photocatalytic production of hydrogen-rich water. Background Art

[0002] As people's health awareness increases, hydrogen-rich water has attracted widespread attention due to its physiological effects such as anti-oxidation, anti-inflammatory, anti-aging and anti-apoptosis. Hydrogen-rich water, that is, water containing a high concentration of hydrogen, has become a hot topic in research. At present, there are three main methods for preparing hydrogen-rich water on the market: high-pressure gas injection, hydrogen production by hydrogen rods, and hydrogen production by water electrolysis.

[0003] High-pressure inflation hydrogen production can produce hydrogen-rich water by injecting high-pressure hydrogen into water. The bagged or canned hydrogen-rich water on the market currently adopts this method. The dissolved hydrogen concentration is high during filling, but it is not easy to preserve. The principle of hydrogen production by hydrogen rod is to use the reaction of metal magnesium rod and water to produce hydrogen to prepare hydrogen-rich water. The hydrogen concentration produced by this method mainly depends on factors such as the number of uses, whether the container is airtight, and the reaction time. The magnesium particles on the hydrogen rod are easily oxidized. As the number of uses increases, the effect decreases significantly, and a certain amount of magnesium ions will be introduced into the water. The principle of hydrogen production by water electrolysis is that water is decomposed into hydrogen ions and oxygen ions under the action of electric current. Under the action of the electric field, negative oxygen ions move toward the anode, lose electrons at the anode, and form oxygen to be discharged; hydrogen passes through the ion membrane in the form of hydrated ions, reaches the cathode and obtains electrons to form hydrogen to generate hydrogen-rich water. This method is the most commonly used hydrogen production principle for products currently on the market such as hydrogen-rich water machines, hydrogen-rich water cups and hydrogen-rich beauty devices. The amount of hydrogen produced is related to factors such as the electrodes for electrolyzing water, electrolysis time, electrolytic cell structure, and water quality. The key technology lies in the electrodes. Poor-quality electrodes are easily oxidized and may cause increased heavy metal pollution in the water.

[0004] Existing hydrogen-rich water production methods face challenges such as high cost, low efficiency, and easy generation of metal pollutants. Therefore, the development of a safe, efficient, and low-cost hydrogen-rich water production technology has important practical significance and market demand. Summary of the invention

[0005] In order to solve the problems of high cost, easy generation of metal pollutants, high energy consumption and low efficiency in the existing hydrogen-rich water production, the present invention provides an application of a fullerene (derivative) semiconductor or a small molecule photosensitizer composite material in the production of hydrogen-rich water. In another aspect, a composite material of fullerene-derived carbon quantum dots with a novel structure and a preparation method thereof are provided.

[0006] One aspect of the present invention provides an application of a fullerene composite material in photocatalytic production of hydrogen-rich water, wherein the composite comprises fullerene or a derivative thereof and a photocatalyst material.

[0007] One aspect of the present invention provides an application of a fullerene composite material in photocatalytic water hydrogen production, wherein the composite comprises fullerene or a derivative thereof and a photocatalyst material.

[0008] In one embodiment, the fullerene derivatives include one or more of fullerene amino derivatives, fullerene carboxyl derivatives, fullerene hydroxylation derivatives, ethylenediamine-modified fullerene derivatives, and imidazole-modified fullerene derivatives.

[0009] In one embodiment, the fullerene derivative is a hydrophilic fullerene derivative, which helps to improve the dispersibility of fullerene in water.

[0010] In one embodiment, the fullerene derivative is a fullerene modified with a hydrophilic group or a derivative thereof.

[0011] In one embodiment, the hydrophilic group is selected from one or more of hydroxyl, carboxyl, amino, ethylenediamine and imidazole.

[0012] In one embodiment, the hydrophilic group is a positively charged group (eg, an amino group) to help improve the separation efficiency of the photogenerated charges.

[0013] In one embodiment, the fullerene is at least one of a hollow fullerene, a metallofullerene, a heterocyclic fullerene and an endohedral fullerene.

[0014] In one embodiment, the fullerene is C 2a 、M@C 2a 、M2@C 2a 、MA@C 2a 、M3N@C 2a 、M2C2@C 2a 、M2S@C 2a 、M2O@C 2a and M x A 3-x N@C 2a Any one or a mixture thereof, wherein M and A are both metal elements, and M and A are both selected from any one of Sc, Y and lanthanide metal elements, 30≤a≤60; 0≤x≤3.

[0015] In one embodiment, the fullerene is selected from hollow fullerene C 2a Any one of; wherein 30≤a≤60, preferably 30, 35, 38, 39, 41 or 42; more preferably 30 or 35.

[0016] In one embodiment, the fullerene is a metallofullerene, which helps to increase the charge separation rate of the composite material and promote the efficiency of photocatalytic hydrogen production.

[0017] In one embodiment, the fullerene is selected from metallofullerene M2C2@C 2b or metallofullerene M'3N@C 2b Any one of; wherein 39≤b≤54, preferably 40, 41 or 42.

[0018] In one embodiment, M is at least one of Sc, La, Y, and Dy; M' is at least one of Sc, La, Y, Ho, Lu, Dy, or Er; and M and M' are preferably Sc.

[0019] In one embodiment, the amino derivative of fullerene has a structure as shown in formula (I):

[0020]

[0021] Wherein R is an amino modification group of the fullerene, one end of R is bonded to the fullerene through one or more of a nitrogen-containing group, a phenyl group, and a thiol group, and the other end of R is any nitrogen-containing group, and the nitrogen-containing group includes any one or more of a primary amine, a secondary amine, a tertiary amine, and a quaternary amine;

[0022] Preferably, R is -NR 1 -R'-NR 2 R 3 , where R 1 , R 2 , R 3 may be independently or simultaneously hydrogen, or substituted or unsubstituted C1-C6 alkyl, C3-C6 cycloalkyl, C1-C6 alkyl containing heteroatoms, C3-C6 heterocycloalkyl, aryl, heteroaryl, or R 1 and R 2 and / or R 3 together to form a cyclized substituent, where R 1 and R 2 and / or R 3 When R′ is absent when the substituents are combined to form a cyclized group, R′ is absent; preferably, R 2 , R 3 At the same time, it is hydrogen;

[0023] R' is a substituted or unsubstituted C1-C6 alkyl group, a C3-C6 cycloalkyl group, a C1-C6 alkyl group containing a heteroatom, a C3-C6 heterocycloalkyl group, an aryl group, a heteroaryl group, or R 1 Together with R', it forms a cyclized substituent;

[0024] wherein m is selected from an integer of 1-12.

[0025] In one embodiment, the amino derivative of fullerene of formula (I), wherein the amino modification group R of the fullerene is selected from one or more of (2-aminoethyl)amino, (3-aminopropyl)amino, (4-aminobutyl)amino, (5-aminopentyl)amino, (2-aminophenyl)amino, (3-aminophenyl)amino, (4-aminophenyl)amino, (methylaminophenyl)amino, (4-amino)piperidinyl, piperazinyl, 4-aminophenyl, (4-aminomethyl)phenyl, (4-aminophenyl)thiol, (4-aminocyclohexyl)thiol, 4-piperidinylthiol, (1-aminoethyl)thiol, (1-aminopropyl)thiol, (1-aminobutyl)thiol, (1-aminopentyl)thiol;

[0026] Wherein m is selected from an integer of 1-12, preferably 3, 4, 5, 6, 10.

[0027] In one embodiment, the fullerene carboxyl derivative comprises a hollow fullerene carboxyl derivative or a metal fullerene carboxyl derivative, wherein: the hollow fullerene carboxyl derivative comprises, C 2a (C(COOH)2)n1, wherein 30≤a≤60, n1=1-10, preferably 1-4, and can further be 1, 2, 3 or 4.

[0028] In one embodiment, the hollow fullerene carboxylated derivative comprises C 60 (C(COOH)2)n1、C 70 (C(COOH)2)n1、C 76 (C(COOH)2)n1、C 78 (C(COOH)2)n1、C 84 At least one of (C(COOH)2)n1.

[0029] In one embodiment, the metallofullerene carboxyl derivative is M2C2@C 2b (C(COOH)2)n1 or M'3N@C 2b (C(COOH)2)n1, wherein 39≤b≤54, n1=1-10, preferably 1-4, and can further be 1, 2, 3 or 4.

[0030] In one embodiment, the fullerene carboxyl derivative comprises C 60 (C(COOH)2)2, C 70 (C(COOH)2)2、Sc3N@C 80 At least one of (C(COOH)2)2.

[0031] In one embodiment, the fullerene hydroxylated derivative comprises C 2a (OH)n2, preferably C60 (OH)n2 or C 70 (OH)n2, wherein n2 is 1 to 10, preferably 6 to 10.

[0032] In one embodiment, the fullerene amino derivative comprises C 2a (NH2)n3, preferably C 60 (NH2)n3 or C 70 (NH2)n3, n3 is 1 to 10, preferably 6 to 10.

[0033] The use of n1, n2, and n3 is to clearly distinguish the selected values ​​of the subscripts of various substances. However, in this article, when specific substances are involved in different positions, since they can be distinguished by the type of fullerene and the type of derivative, the subscript can all be represented by n.

[0034] In one embodiment, the carboxyl fullerene and / or hydroxy fullerene is a fullerene derivative described in the document “Huo, J.; Li, J.; Liu, Y.; Yang, L.; Cao, X.; Zhao, C.; Lu, Y.; Zhou, W.; Li, S.; Liu, J.; Wang, C.; Bai, C., Amphiphilic Aminated Derivatives of

[60] Fullerene as Potent Inhibitors of Tumor Growth and Metastasis. Advanced Science 2022, 2201541.).

[0035] In one embodiment, the photocatalyst material is selected from semiconductor materials and / or photosensitizer derivatives.

[0036] In one embodiment, the semiconductor material is selected from one or more of titanium dioxide, bismuth tungstate, bismuth oxide, tungsten oxide, molybdenum oxide, zirconium oxide, graphite carbon nitride, carbon quantum dots, manganese oxide, bismuth vanadate, zinc oxide and tin oxide.

[0037] In one embodiment, the semiconductor material is selected from one or more of titanium dioxide, bismuth tungstate, carbon nitride, manganese oxide, bismuth vanadate, zinc oxide and tin oxide.

[0038] In one embodiment, the photosensitizer derivative is selected from one or more of non-metal porphyrin derivatives, metal porphyrin or its derivatives, metal phthalocyanine or its derivatives, bipyridine ruthenium, chlorophyll, eosin, porphyrine, rose bengal, rhodamine B, and methylene blue.

[0039] In one embodiment, the photosensitizer derivative is selected from one or more of tetracarboxylate phthalocyanine zinc, tetraphenyl zinc porphyrin, tetraphenyl copper porphyrin, and tetrakis (4-carboxyphenyl) cobalt porphyrin.

[0040] In one embodiment, the composite material is a composite material formed by fullerene or its derivatives and carbon quantum dots.

[0041] In one embodiment, the composite material fullerene and carbon quantum dots are combined through electrostatic interaction or hydrogen bonding interaction.

[0042] When the fullerene derivative is negatively charged, the surface of the carbon quantum dots is negatively charged;

[0043] Alternatively, when the fullerene derivative is positively charged, the surface of the carbon quantum dots is negatively charged;

[0044] Alternatively, when the fullerene derivative carries a hydrogen bond donor, the surface of the carbon quantum dots carries a hydrogen bond acceptor;

[0045] Alternatively, when the fullerene derivative carries a hydrogen bond acceptor, the surface of the carbon quantum dots carries a hydrogen bond donor;

[0046] In one embodiment, the fullerene derivative is carboxyl fullerene, and the carbon quantum dots are quantum dots with positive surface charges, wherein the fullerene and the quantum dots are preferably bound by electrostatic interaction;

[0047] And / or, the fullerene derivative is aminofullerene, the carbon quantum dots are quantum dots with negative surface charge, wherein the fullerene and the quantum dots are preferably combined by electrostatic interaction;

[0048] And / or, the fullerene derivative is a fullerene with a hydrogen bond donor on the surface, and the carbon quantum dot is a quantum dot with a hydrogen bond acceptor on the surface, wherein the fullerene and the quantum dot are preferably combined through a donor-acceptor interaction;

[0049] And / or, the fullerene derivative is a fullerene with a hydrogen bond acceptor on the surface, and the carbon quantum dot is a quantum dot with a hydrogen bond donor on the surface, wherein the fullerene and the quantum dot are preferably combined through a donor-acceptor interaction;

[0050] In one embodiment, the hydrogen bond donor is a hydroxyl group and the hydrogen bond acceptor is a fluorine or trifluoromethyl group.

[0051] In one embodiment, the composite material is TCPC Composite materials with carbon quantum dots.

[0052] In one embodiment, the preparation of the composite material comprises: mixing 0.5-2 mg / mL of TCPC and 0.5-2 mg / mL of carbon quantum dots.

[0053] Preferably, the concentration of TCPC and carbon quantum dots is 1 mg / mL.

[0054] Furthermore, the preparation further comprises: performing ultrasonic treatment, wherein the time for the ultrasonic treatment is 2-12 hours, preferably 6 hours.

[0055] Furthermore, the preparation also includes: performing dialysis treatment.

[0056] Furthermore, the preparation further comprises: freeze-drying to obtain the composite material.

[0057] In one embodiment, the preparation comprises: preparing 5 mL of a 1 mg / mL aqueous solution of water-soluble fullerene TCPC, adding the TCPC aqueous solution to 10 mL of a 1 mg / mL PT2 carbon dot solution, and mixing them thoroughly by ultrasonication for 6 hours, then dialyzing with ultrapure water for 48 hours, and freeze-drying to obtain a composite material.

[0058] In one embodiment, in the composite material, the mass ratio of carbon quantum dots to TCPC is 1:(0.1-10), preferably 1:(0.5-2), and further can be 1:0.5, 1:1, 1:1.5 or 1:2.

[0059] In one embodiment, the composite material is TAPC Composite materials with carbon quantum dots.

[0060] In one embodiment, the composite material is THPC Composite materials with carbon quantum dots.

[0061] In one embodiment, the composite material is C 60 Composite materials of (C(COOH)2)2 and carbon quantum dots.

[0062] In one embodiment, the composite material is C 70 Composite materials of (C(COOH)2)2 and carbon quantum dots.

[0063] In one embodiment, the composite material is Sc3N@C 80 (C(COOH)2)2 Composite materials with carbon quantum dots.

[0064] In one embodiment, the preparation of the composite material comprises: adding 0.5-2 mg / mL of Sc3N@C 80 (C(COOH)2)2 and 0.5-2 mg / mL carbon quantum dots were mixed.

[0065] Preferably, the Sc3N@C 80The concentration of (C(COOH)2)2 and carbon quantum dots was 1 mg / mL.

[0066] Furthermore, the preparation further comprises: performing ultrasonic treatment, wherein the time for the ultrasonic treatment is 2-12 hours, preferably 6 hours.

[0067] Furthermore, the preparation also includes: performing dialysis treatment.

[0068] Furthermore, the preparation further comprises: freeze-drying to obtain the composite material.

[0069] In one embodiment, the preparation comprises: 80 (C(COOH)2)2 was prepared into 5 mL of 1 mg / mL aqueous solution. 80 The (C(COOH)2)2 aqueous solution was added to 10 mL of 1 mg / mL PT2 carbon dot solution and mixed thoroughly by ultrasonication for 6 h. The solution was then dialyzed with ultrapure water for 48 h and freeze-dried to obtain the composite material.

[0070] In one embodiment, the composite material is a composite material of TCPC and carbon quantum dots, a composite material of TAPC and carbon quantum dots, a composite material of THPC and carbon quantum dots, a composite material of TCPC and TiO2, a composite material of TAPC and TiO2, a composite material of THPC and TiO2, a composite material of C 60 Composite materials of (C(COOH)2)2 and carbon quantum dots, C 70 Composite materials of (C(COOH)2)2 and carbon quantum dots, Sc3N@C 80 Composite materials of (C(COOH)2)2 and carbon quantum dots, C 60 Composite materials with TiO2, C 60 Composite materials of (OH)n2 and TiO2, Sc3N@C 80 Composite materials with TiO2, C 60 Composite materials of (EDA)n3 and TiO2, C 70 Composite materials of (EDA)n3 and TiO2, composite materials of TAPC and zirconia, C 70 (C(COOH)2)n1-ZnPc-TiO2 Composites 70 (C(COOH)2)n-tetracarboxylate phthalocyanine zinc-TiO2), C 60 Composite materials of (C(COOH)2)2 and g-C3N4, C 60 Composite materials of (C(COOH)2)2 and Bi2WO6, C 60 Composite materials with SnO2, C 70Composite materials of TAPC and CuTPP (tetraphenyl copper porphyrin), composite materials of TAPC and CoTCPP (tetrakis (4-carboxyphenyl) cobalt porphyrin), ImC 70 Composite materials with CoPc (cobalt phthalocyanine), ImC 60 (Imidazole-modified C 60 ) and ZnTPP (tetraphenyl zinc porphyrin) composites, Sc3N@C 80 Composite materials with ZnTPP (tetraphenyl zinc porphyrin);

[0071] n1=1-10, preferably 1-4; n2 is 1-10, preferably 6-10; n3 is 1-10, preferably 6-10.

[0072] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and carbon quantum dots. The hydrophilic fullerene derivative is selected from one or more of fullerene amino derivatives, fullerene carboxyl derivatives, and fullerene hydroxylation derivatives.

[0073] In one embodiment, the hydrophilic fullerene derivative is selected from the group consisting of fullerene carboxyl derivatives TCPC, C 60 (C(COOH)2)2, C 70 (C(COOH)2)2 or Sc3N@C 80 (C(COOH)2)2, fullerene amino derivative TAPC or fullerene hydroxylation derivative THPC.

[0074] In one embodiment, the composite material of the hydrophilic fullerene derivative and carbon quantum dots is selected from a composite material of TCPC and carbon quantum dots, a composite material of TAPC and carbon quantum dots, a composite material of THPC and carbon quantum dots, a composite material of C 60 Composite materials of (C(COOH)2)2 and carbon quantum dots, C 70 Composite materials of (C(COOH)2)2 and carbon quantum dots and Sc3N@C 80 One or more composite materials of (C(COOH)2)2 and carbon quantum dots.

[0075] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and a semiconductor; preferably, the composite material is a composite material of a hydrophilic fullerene and one or more selected from titanium dioxide, zirconium oxide, carbon nitride (such as graphene carbon nitride), and bismuth tungstate.

[0076] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and titanium dioxide.

[0077] In one embodiment, the composite material of the hydrophilic fullerene derivative and titanium dioxide is selected from the composite material of TCPC and TiO2, the composite material of TAPC and TiO2, the composite material of THPC and TiO2, the composite material of C 60 Composite materials of (OH)n2 and TiO2, C 60 Composite materials of (EDA)n3 and TiO2 and C 70 One or more composite materials of (EDA)n3 and TiO2.

[0078] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and zirconium oxide.

[0079] Preferably, the composite material is a composite material of TAPC and zirconia.

[0080] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and carbon nitride; preferably, the composite material is C 60 Composite materials of (C(COOH)2)2 and g-C3N4.

[0081] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and bismuth tungstate (Bi2WO6); preferably, the composite material is C 60 Composite materials of (C(COOH)2)2 and Bi2WO6.

[0082] In one embodiment, the composite material is a composite material of a hydrophilic fullerene derivative and a photosensitizer derivative;

[0083] Preferably, the photosensitizer derivative is selected from one or more of tetrakis(4-carboxyphenyl)cobaltporphyrin, cobalt phthalocyanine, tetraphenylzincporphyrin, and tetraphenylzincporphyrin;

[0084] Preferably, the composite material is a composite material of TAPC and CoTCPP (tetrakis (4-carboxyphenyl) cobalt porphyrin), ImC 70 (Imidazole-modified C 70 ) and CoPc (cobalt phthalocyanine) composite materials.

[0085] In one embodiment, the composite material is a ternary composite material of a hydrophilic fullerene derivative, a photosensitizer derivative, and titanium dioxide;

[0086] Preferably, the photosensitizer derivative is selected from one or more of tetrakis(4-carboxyphenyl)cobaltporphyrin, cobalt phthalocyanine, tetraphenylzincporphyrin, and tetraphenylzincporphyrin;

[0087] Preferably, the composite material is C 70(C(COOH)2)n1-ZnPc-TiO2 Composites 70 (C(COOH)2)n-tetracarboxylate zinc phthalocyanine-TiO2).

[0088] In one embodiment, the composite material is a composite material of imidazole-modified fullerene and a photosensitizer derivative;

[0089] Preferably, the imidazole-modified fullerene is an imidazole-modified hollow fullerene;

[0090] Preferably, the imidazole-modified fullerene is imidazole-modified fullerene C 60 or imidazole-modified fullerene C 70 ;

[0091] Preferably, the composite material is ImC 60 (Imidazole-modified C 60 ) and ZnTPP (tetraphenyl zinc porphyrin) composites or ImC 70 Composite materials with CoPc (cobalt phthalocyanine).

[0092] Preferably, the photosensitizer derivative is tetraphenyl zinc porphyrin or dihydrochlorin e6;

[0093] Preferably, the composite material is Sc3N@C 80 Composite materials with ZnTPP (tetraphenylzinc porphyrin).

[0094] In one embodiment, the composite material is C 60 In one embodiment, the composite material is C 60 Composite material of (OH)n2 and TiO2.

[0095] In one embodiment, the composite material is Sc3N@C 80 Composite materials with TiO2.

[0096] In one embodiment, the composite material is C 70 (C(COOH)2)n1-ZnPc(zinc phthalocyanine)-TiO2 composite material.

[0097] In one embodiment, the composite material is C 60 Composite materials of (C(COOH)2)2 and g-C3N4.

[0098] In one embodiment, the composite material is C 60 Composite materials of (C(COOH)2)2 and Bi2WO6.

[0099] In one embodiment, the composite material is C60 Composite materials with SnO2.

[0100] In one embodiment, the composite material is C 70 Composites with CuTPP.

[0101] In one embodiment, the composite material is a composite material of TAPC and CoTCPP.

[0102] In one embodiment, the composite material is ImC 70 Composites with CoPc.

[0103] In one embodiment, the composite material is ImC 60 Composite materials with ZnTPP.

[0104] In one embodiment, the composite material is SA-Sc3N@C 80 Composite materials with ZnTPP.

[0105] In one embodiment, the composite material is SA-C 60 -Ce6 composite material.

[0106] In one embodiment, the composite material is SA-C 60 -Ce6, SA-C 60 -Ce6-Cl, SA-C 70 -Ce6-CN or composite material SA-C 60 -Ce6-OH composite material.

[0107] In one embodiment, n1 is selected from 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or a range between any two thereof; n2 is selected from 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or a range between any two thereof; n3 is selected from 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or a range between any two thereof.

[0108] In one embodiment, the photocatalyst material is a hydrophilic material, which helps to improve the hydrogen production performance of photocatalytic water to produce hydrogen.

[0109] In one embodiment, the hydrophilic material is hydrophilic carbon quantum dots.

[0110] In one embodiment, the particle size of the carbon quantum dots is preferably 1 to 10 nm.

[0111] In one embodiment, the carbon quantum dots are formed by hydrothermal sintering of precursors containing carbon and other heteroatoms, and have a core-shell structure, wherein the core is crystalline carbon with a graphite-like structure, and the shell is a hydrophilic group, such as hydroxyl, carboxyl, amino, ethylenediamine, etc.

[0112] In one embodiment, a precursor containing carbon and heteroatoms is dispersed in water (e.g., deionized water) to obtain a mixed solution; the obtained mixed solution is subjected to a hydrothermal reaction at 160-180° C. for 3-24 hours to obtain the carbon quantum dots. The carbon quantum dots are then washed and dried to obtain solid carbon quantum dots for further reaction.

[0113] In one embodiment, the carbon quantum dot precursor is selected from small molecule organic substances such as monosaccharides and polysaccharides such as citric acid, ethylenediamine, o-phenylenediamine, fructose, glucose, sucrose, citric acid, oxalic acid and other organic acids, urea, etc.; conjugated polymers, polythiophenes (PT), poly(phenylethylene) (PPE), polyparaphenylene vinylene (PPV), etc.

[0114] In one embodiment, the small molecule precursor portion is exemplified as follows:

[0115]

[0116] In one embodiment, the conjugated polymer portion is exemplified as follows:

[0117]

[0118] Wherein n is a natural number; wherein: R1, R2, R3, R4, R5, R6 are respectively or independently hydrogen, alkyl, hydroxyl, carboxyl, amino, amide, anhydride, cyano, alkenyl, alkynyl, aryl, ester, ether, quaternary ammonium salt, polyethylene glycol or other conjugated polymer derivatives.

[0119] In one embodiment, the carbon quantum dots are carbon quantum dots described in the document “Jiechao Ge, Pengfei Wang et al. A Graphene Quantum Dot Photodynamic Therapy Agent with High Singlet Oxygen Generation Nat. Commun. 2014, 5, 4596-4603.”

[0120] In one embodiment, the carbon quantum dots are in the form of a polymer

[0121] Wherein, n is the number of times the repeating units (or chain links) appear consecutively.

[0122] In one embodiment, the photocatalysis comprises the following steps: adding the fullerene composite material photocatalyst to an aqueous solution containing a sacrificial agent, evacuating the solution, and irradiating the solution with a xenon lamp;

[0123] In one embodiment, the wavelength band of the light is sunlight AM 1.5.

[0124] In one embodiment, the wavelength of the light is in the range of 420 to 800 nm.

[0125] In one embodiment, the photocatalytic time is 1 to 24 hours.

[0126] Another aspect of the present invention provides a fullerene carbon quantum dot composite material, wherein the fullerene includes fullerene and fullerene derivatives, the fullerene derivatives include one or more of fullerene amino derivatives, fullerene carboxyl derivatives, and fullerene hydroxylated derivatives; and the carbon quantum dots are the quantum dots described above.

[0127] In one embodiment, the carbon quantum dots are hydrophilic carbon quantum dots, and the particle size of the carbon quantum dots is preferably 1 to 10 nm.

[0128] Preferably, the carbon quantum dots have a core-shell structure, wherein the core is crystalline carbon with a graphite-like structure, and the shell is a hydrophilic group; the hydrophilic group is preferably selected from hydroxyl, carboxyl, amino or ethylenediamine.

[0129] In one embodiment, the composite material is obtained by mixing the fullerene or fullerene derivative and carbon quantum dots.

[0130] In one embodiment, the mass ratio of the carbon quantum dots to the fullerene derivative is 1:(0.1-10), preferably 1:(0.5-2).

[0131] Another aspect of the present invention provides a method for preparing the fullerene carbon quantum dot composite material, which comprises: mixing the fullerene or fullerene derivative and carbon quantum dots.

[0132] In one embodiment, the preparation of the composite material comprises: mixing 0.5-2 mg / mL of fullerene or its derivatives and 0.5-2 mg / mL of carbon quantum dots.

[0133] Preferably, the concentration of the fullerene or its derivative is 1 mg / mL.

[0134] Preferably, the concentration of the carbon quantum dots is 1 mg / mL.

[0135] Furthermore, the preparation further comprises: performing ultrasonic treatment, wherein the time for the ultrasonic treatment is 2-12 hours, preferably 6 hours.

[0136] Furthermore, the preparation also includes: performing dialysis treatment.

[0137] Furthermore, the preparation further comprises: freeze-drying to obtain the composite material.

[0138] In one embodiment, the preparation comprises: preparing fullerene or its derivatives into 5 mL of an aqueous solution with a concentration of 1 mg / mL. Adding the aqueous solution of fullerene or its derivatives into 10 mL of a 1 mg / mL carbon quantum dot solution, and mixing them thoroughly by ultrasonication for 6 hours. Thereafter, dialyzing with ultrapure water for 48 hours, and freeze-drying to obtain a composite material.

[0139] Furthermore, the preparation method comprises:

[0140] a) The above fullerene derivative is fully dissolved in water to a concentration of 0.5-1 mg / mL to obtain a solution 1.

[0141] b) A carbon quantum dot solution of about 1 mg / mL was mixed thoroughly with solution 1 at a volume ratio of 1:(0.5-10), and ultrasonicated for 6 h to obtain solution 2.

[0142] c) Solution 2 was dialyzed against deionized water for 48 h with a molecular weight cutoff of 3000 Da, and freeze-dried to obtain a composite material.

[0143] In another aspect of the present invention, a method for photocatalytically producing hydrogen-rich water is provided, the method comprising the following steps:

[0144] 1-1000 mg (eg 2 mg) of fullerene photocatalytic material is added to deionized water as a photocatalyst, and a hole sacrificial agent and / or a promoter is added. After vacuuming and deoxygenation, an AM 1.5 full-band light source is used for irradiation.

[0145] In one embodiment, the hole sacrificial agent is selected from at least one of ascorbic acid, triethanolamine, methanol, formic acid, and NaHCO3; the co-catalyst is selected from at least one of chloroplatinic acid, a metal co-catalyst, a transition metal sulfide, a transition metal phosphide, and a composite co-catalyst;

[0146] In one embodiment, the promoter is selected from at least one of Pt, Au, Ag, and Pd;

[0147] In one embodiment, the co-catalyst loading is 1 wt% to 10 wt%, optionally 1 wt% to 3 wt%.

[0148] In one embodiment, the light source is a 300W xenon lamp, including at least one of a visible light source and simulated natural light.

[0149] In one embodiment, the intensity of the light source is selected from 300 to 500 mW / cm 2 .

[0150] In one embodiment, the light irradiation time may be 0.5 to 20 hours, optionally 3 to 6 hours, and preferably 3 hours.

[0151] Beneficial Effects

[0152] 1. The fullerene photocatalytic material provided by the present invention can reduce the production cost of hydrogen-rich water and realize safe, pollution-free, green and efficient preparation of hydrogen-rich water.

[0153] 2. The fullerene photocatalytic material provided by the present invention has a stable structure, good cycle stability, is easy to recycle, and can be recycled multiple times.

[0154] 3. The fullerene photocatalytic material structure provided by the present invention has a simple production process, mild conditions, low cost, high yield, easy operation, and is non-toxic and non-hazardous.

[0155] 4. The present invention constructs a composite material based on fullerene and carbon quantum dots. The carbon quantum dots have a stable fullerene structure and excellent electron accepting ability. The carbon quantum dots have a wide light absorption range and are stable in solution. Among them, the carbon quantum dot composite material uses carbon quantum dots with small size and good dispersibility in water as photosensitizers to help reduce problems such as catalyst agglomeration and enhance its contact with water, compared with the problem of poor dispersibility in water of traditional organic photocatalytic materials.

[0156] 5. Fullerene has a stable structure and a large conjugated structure, and is a commonly used electron acceptor; carbon quantum dots are new members of the carbon nanomaterial family, with adjustable luminescence, high fluorescence quantum efficiency, good anti-photobleaching performance, good biocompatibility, non-toxicity, easy functionalization, and high-yield preparation. It is expected to show broad application prospects in the fields of optoelectronic devices, nanocatalysts, bioanalysis, fluorescence imaging, and photothermal cancer therapy. The combination of fullerene and carbon quantum dots can improve the visible light absorption capacity, promote the separation of photogenerated charges, inhibit the recombination of photogenerated electrons and holes, and enhance the photocatalytic activity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0157] Figure 1 This is the TCPC mass spectrum of the carboxyl fullerene derivative prepared in Example 1 of the present invention.

[0158] Figure 2 A is the ultraviolet visible absorption spectrum of the carbon quantum dot PT2 prototype and the fullerene derivative TCPC and carbon quantum dot PT2 composite material in Example 1 of the present invention, Figure 2 B is the fluorescence spectrum.

[0159] Figure 3 A and Figure 3 B are the Mott-Schottky curves of the carbon quantum dot PT2 prototype and the fullerene derivative TCPC and carbon quantum dot PT2 composite material.

[0160] Figure 4 A and Figure 4 B are transmission electron microscopy images of the carbon quantum dot PT2 prototype and the fullerene derivative TCPC and carbon quantum dot PT2 composite material.

[0161] Figure 5 A and Figure 5 B are the photocurrent comparison diagram and electrochemical impedance comparison diagram of the carbon quantum dot PT2 prototype and the fullerene derivative TCPC and carbon quantum dot PT2 composite material, respectively. DETAILED DESCRIPTION

[0162] I. Definitions

[0163] In the present invention, unless otherwise specified, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. In addition, the relevant terms and laboratory procedures used herein are terms and conventional procedures widely used in the corresponding fields. At the same time, in order to better understand the present invention, the definitions and explanations of the relevant terms are provided below.

[0164] As used herein and unless otherwise specified, the term "about" or "approximately" means within plus or minus 10% of a given value or range. Where an integer is required, the term means within plus or minus 10% of a given value or range, rounded up or down to the nearest integer.

[0165] In the description of this document, reference is made to “some embodiments”, “some implementation schemes” or “some implementation plans”, which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0166] As used herein and unless otherwise specified, the terms "comprising", "including", "having", "containing", including grammatical equivalents thereof, should generally be understood as open and non-limiting, for example, not excluding other unlisted elements or steps.

[0167] Herein, the term "semiconductor" refers to a material whose conductivity at room temperature is between that of a conductor and an insulator. The term "semiconductor" is interpreted in the broadest sense as a material that is not a conductor in its natural state but can be activated into a conducting state.

[0168] Herein, the “photosensitizer” refers to a molecule having a π-conjugated structure that can effectively absorb ultraviolet and visible light.

[0169] In this article, TiO2 is titanium dioxide, Bi2WO3 is bismuth tungstate, and SnO2 is tin dioxide. TPP is tetraphenylporphyrin; ZnTPP, CoTPP, and CuTPP are tetraphenylporphyrins containing zinc ions, cobalt ions, and copper ions, respectively; ZnTCPP is tetracarboxyphenyl zinc porphyrin; CuPc is copper phthalocyanine; ZnPC is zinc phthalocyanine; In this article, SA before the material is the abbreviation of self-assembly, which means that the material is self-assembled through intermolecular interactions.

[0170] Herein, the "hole sacrificial agent" refers to an agent that can consume photogenerated holes and leave electrons to react with water to generate hydrogen.

[0171] The term "amide" refers to a amide of the form -R a C(O)NH2、-R a C(O)NHR b or -R a C(O)NR b R c A group in which R a , R b and R c are each independently selected from hydrogen, alkyl, alkanoyl, alkenyl, alkoxy, alkynyl, aryl, carboxyl, cycloalkyl, ester, ether, heterocyclic, hydroxyl, ketone, thio, and sulfonyl, and R a is selected from hydrogen, alkyl, alkoxy, amide, amino, aryl, cycloalkyl, ester, ether, heterocyclic, halogen, hydroxyl, ketone and thio. The amide can be formed by carbon, nitrogen, R a , R b or R c Attached to another group. The term "amido" includes groups such as alkanoylaminoalkyl, amidoalkyl (bonded to the parent molecular group through the alkyl group), alkylamido (bonded to the parent molecular group through the amido group), arylamido, amidoaryl, sulfonamide, etc. The term "amido" also includes groups such as urea, carbamate, and cyclic forms thereof.

[0172] The term "anhydride" refers to the general structure -C(=O)-OC(=O)R a A compound wherein R a Same definition as above.

[0173] The term "carbon quantum dot (CQD)" refers to a carbon nanotube 2 / sp 3The carbon core (the chemical structure of carbon quantum dots usually includes amorphous and crystalline carbon cores) and an outer layer of oxygen / nitrogen functional groups (such as hydroxyl, carboxyl and amino groups, etc.), the particle size is usually less than 10nm, and it is monodisperse. Carbon quantum dots have a strong absorption peak in the ultraviolet region and a long tail in the visible region, which makes them potentially valuable in optical applications.

[0174] Since carbon quantum dots do not involve the use of heavy metals in the preparation process and can be extracted from food or biomass, they have high biocompatibility and low cytotoxicity, and have less impact on the environment. This makes carbon quantum dots have broad application prospects in medical imaging, biosensing, photocatalytic reactions and other fields.

[0175] There are various methods for synthesizing carbon quantum dots, including top-down synthesis and bottom-up synthesis. Specific methods include arc discharge, laser ablation, electrochemical method, chemical oxidation, combustion method, solvent thermal synthesis (such as hydrothermal method), microwave synthesis and template method.

[0176] Herein, "fullerene amino derivative" refers to a fullerene derivative in which the end of the modification group connected to the fullerene body, which is far away from the fullerene body, is an amino group. 60 (NH2) n3 Refers to the fullerene body using C 60 The amino derivatives, C 70 (NH2) n3 Refers to the fullerene body using C 70 In the process of synthesis, compounds with amino groups at both ends such as ethylenediamine, propylenediamine, and butylenediamine can be used to combine with fullerene, where the amino group at one end is connected to the fullerene and the amino group at the other end is exposed. For example: C 60 (EDA)n3 is C 60 The fullerene derivative obtained by bonding the fullerene body with ethylenediamine has a modified group far away from C 60 The terminal end is an amino group, which also belongs to the amino derivative of fullerene C 60 One of the (NH2)n3, the composite material obtained by modifying TiO2 is C 60 (NH2)n3 / TiO2、C 70 (EDA)n3 and C 70 The same applies to (NH2)n3 / TiO2.

[0177] Herein, "fullerene carboxyl derivative" refers to a fullerene derivative in which the end of the modification group connected to the fullerene body away from the fullerene body is a carboxyl group, such as: 60 The modification group of (C(COOH)2)n1 is far away from C 60The terminal of C is a carboxyl group, which is a carboxyl derivative of fullerene; 70 The modification group of (C(COOH)2)n1 is far away from C 70 The terminal of the fullerene is a carboxyl group, which is a carboxyl derivative of fullerene.

[0178] Herein, "fullerene hydroxylated derivative" refers to a fullerene derivative in which the end of the modification group connected to the fullerene body away from the fullerene body is a hydroxyl group, such as: 60 ( OH )n2's modification group is far away from C 60 The terminal of C is a hydroxyl group, which is a hydroxylated fullerene derivative; 70 The modification group of (OH)n2 is far away from C 70 The terminal of the fullerene is a hydroxyl group, which is a hydroxylated fullerene derivative.

[0179] Hydroxyl: -OH;

[0180] Carboxyl: -COOH;

[0181] Amino group: -NH2;

[0182] Cyano: -CN.

[0183] II. Embodiment

[0184] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below. The described embodiments should not be regarded as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0185] Before further describing the embodiments of the present invention in detail, the nouns and terms involved in the embodiments of the present invention are described. The nouns and terms involved in the embodiments of the present invention are subject to the following interpretations.

[0186] The raw materials and equipment used in the specific embodiments of the present disclosure are all known products, which are obtained by purchasing commercially available products.

[0187] Some of the instrument models used in the specific implementation of the present disclosure are as follows:

[0188] Transmission electron microscope: Hitachi transmission electron microscope HT7700;

[0189] UV spectrophotometer: Shimadzu UV-2550;

[0190] Example 1: Preparation of a composite material of fullerene derivative TCPC and PT2 carbon quantum dots

[0191] 1.1 Composite material preparation

[0192] (1) Water-soluble carboxyl fullerene TCPC was prepared according to “(Huo, J.; Li, J.; Liu, Y.; Yang, L.; Cao, X.; Zhao, C.; Lu, Y.; Zhou, W.; Li, S.; Liu, J.; Wang, C.; Bai, C., Amphiphilic Aminated Derivatives of

[60] Fullerene as Potent Inhibitors of Tumor Growth and Metastasis. Advanced Science 2022, 2201541.)”. The preparation method is as follows:

[0193] C 60 (5 g) and 4-N-BOC-aminopiperidine (13 g) were dissolved in chlorobenzene (625 mL), and cumene hydroperoxide (5 mL, 80%) was added. The reaction progress was monitored by HPLC. After stirring at room temperature (600 rpm) for 48 h, C 60 The reaction was almost completely consumed. The reaction was stopped with dimethyl sulfide (10 mL), washed with a saturated aqueous solution of NH4Cl (300 mL) and NaHCO3 (300 mL), and dried over anhydrous Na2SO4. The crude product was evaporated at 60°C as a reddish brown solid. The Boc-protected TCPC was purified by silica gel column chromatography (Rf: 0.3, 25-30% ethyl acetate in toluene as mobile phase).

[0194] The product was obtained by stirring in 50% TFA / CHCl3 at room temperature for 6 h to remove the tert-butyl group, and then dissolved in an aqueous solution of NaOH (100 μM) after drying, dialyzed with ultrapure water for 48 h, and vacuum dried to obtain a water-soluble fullerene derivative TCPC.

[0195] The chemical structure of the fullerene derivative TCPC is:

[0196] (2) Preparation of carbon quantum dots Referring to the literature "(Jiechao Ge, Pengfei Wang et al. "A GrapheneQuantum Dot Photodynamic Therapy Agent with High Singlet Oxygen Generation" Nat. Commun. 2014, 5, 4596-4603.)", the preparation method is:

[0197] 30 mg of PT2 polymer was dispersed in 30 mL of water, 20 μL of 1 mg / mL NaOH solution was added, and the mixture was reacted at 170 °C for 24 h to obtain PT2 carbon quantum dots (P-dots).

[0198] The structure of the PT2 polymer is:

[0199] (3) Preparation of water-soluble fullerene derivative TCPC and PT2 positive carbon quantum dot composite materials:

[0200] The water-soluble fullerene TCPC was prepared into 5 mL of an aqueous solution with a concentration of 1 mg / mL. The TCPC aqueous solution was added to 10 mL of a 1 mg / mL PT2 carbon dot solution and mixed thoroughly by ultrasonication for 6 h. The solution was then dialyzed with ultrapure water for 48 h and freeze-dried to obtain a composite material.

[0201] 1.2 Material characterization

[0202] The mass spectrum of TCPC prepared in step 1 of Example 1 is as follows: Figure 1 As shown, the transmission electron microscopy image of the carbon dots prepared in step 2 of Example 1 is as follows Figure 4 As shown in A.

[0203] The UV-visible absorption spectrum of the PT2-TCPC composite material measured at room temperature is as follows Figure 2 A shows the fluorescence spectrum. Figure 2 As shown in B. The composite material has a certain absorption in the range of 300-700nm. Compared with the single P-dots, the introduction of fullerene broadens the light absorption range and improves the light utilization rate.

[0204] The transmission electron microscopy (TEM) of the prepared PT2-TCPC composite material is as follows: Figure 4 In Figure 4 As shown in B, the morphology and size of PT2-TCPC can be intuitively observed, and the size of PT2-TCPC is about 40nm.

[0205] The impedance-potential test structure of the prepared PT2-TCPC composite material is shown in Figure 5 , with silver / silver chloride as the reference electrode and platinum wire as the counter electrode, the Mott-Schottky curve was obtained by conversion ( Figure 3 ), the conduction band potential of the composite was calculated to be about -1.13 V, and combined with its UV-visible diffuse reflectance spectrum, its band gap was calculated to be about 1.77 eV, which theoretically confirmed that the PT2-TCPC composite material has the ability to reduce H in water. + Ability to produce hydrogen.

[0206] Example 2: Metallofullerene derivative Sc3N@C80 Preparation of (C(COOH)2)2 and PT2 Carbon Quantum Dot Composite Materials

[0207] 2.1 Preparation of carboxylated metallofullerene derivatives

[0208] 1 mg Sc3N@C 80 and 8μl of diethyl bromomalonate were dissolved in 3ml of o-dichlorobenzene to form solution A, 5ul of DBU (1,8-diazabicycloundec-7-ene) was added to solution A to form a mixed solution B, the mixed solution B was reacted at room temperature under Ar for 5h, and then the solvent was removed under N2 protection, the obtained solid product was dissolved in toluene and filtered to obtain solution C, and solution C was passed into HPLC for analysis, wherein toluene was used as the mobile phase in the experiment, the flow rate of toluene was 2ml / min, the injection concentration was 1mg / ml, 12ml was fixedly injected each time, and a UV monitoring wavelength of 310nm was used. At the same time, matrix-assisted laser desorption ionization time-of-flight mass spectrometry was combined with each chromatographic peak in the separation process to analyze the time corresponding to the peak position of the chromatographic peak was 40-45min, and the separated product was immediately rotary evaporated and dried in a vacuum drying oven at 60℃ for 20h to obtain solid D, and then 5mg of solid D and 18mg of The NaH solution was added to 30 ml toluene, and the mixture was stirred at 80 ° C under Ar for 10 h, then 1 ml methanol was added dropwise to the mixture, and then 20 ml HCl was added. The obtained precipitate was filtered and washed with toluene, 2 mol / L HCl, H2O, and benzene in sequence. The final solid was dissolved in methanol, centrifuged to remove the solid, and then the solution was rotary evaporated and vacuum dried at 50 ° C for 24 h to obtain the metal fullerene carboxylation derivative Sc3N@C 80 (C(COOH)2)2, the structure is:

[0209]

[0210] 2.2 Metallofullerene derivatives Sc3N@C 80 Preparation of (C(COOH)2)2 and PT2 Carbon Quantum Dot Composite Materials

[0211] The metallofullerene derivative Sc3N@C 80 Prepare 5 mL of 1 mg / mL aqueous solution of (C(COOH)2). 80 The (C(COOH)2)2 aqueous solution was added to 10 mL of 1 mg / mL PT2 carbon quantum dot solution and mixed thoroughly by ultrasonication for 6 h. The solution was then dialyzed with ultrapure water for 48 h and freeze-dried to obtain a composite material.

[0212] Example 3: Preparation of composite materials of fullerene derivatives and carbon quantum dots with different forces

[0213] According to the preparation method of Example 1, fullerene derivatives with surface amino and hydroxyl groups were synthesized to explore the effects of different forces on the hydrogen production performance of fullerene derivative carbon quantum dot composite materials; wherein:

[0214] The structure of TAPC, a fullerene derivative with amino groups on the surface, is:

[0215] The structure of THPC, a fullerene derivative with hydroxyl groups on the surface, is:

[0216] The structures of the different polymers PT4 and PT5 combined with it are as follows:

[0217] The structure of PT4 polymer is:

[0218] The structure of PT5 polymer is:

[0219] Among them, TAPC (with positive charge on the surface) is combined with PT4 carbon quantum dots (with negative charge on the surface) in aqueous solution according to the preparation method in Example 1 to form a composite material; among them, THPC (with hydrogen bond donor on the surface) is combined with PT5 carbon quantum dots (with hydrogen bond acceptor on the surface) in aqueous solution according to the preparation method in Example 1 to form a composite material.

[0220] Example 4: Photocatalytic hydrogen production performance of fullerene derivative TCPC and PT2 carbon quantum dot composite material

[0221] 4.1 Photocatalytic performance test

[0222] 2 mg of the PT2-TCPC composite material prepared in Example 1 was added to 20 ml of distilled water, and 0.05 mg of chloroplatinic acid (catalyst mass fraction was 1% or 3%) was added as a co-catalyst, and 350 mg of ascorbic acid was added as a hole sacrificial agent. After the air in the system was exhausted, a full-band AM1.5 filter was used to simulate sunlight to carry out photocatalytic hydrogen production reaction.

[0223] The hydrogen production reaction was carried out in a glass-enclosed gas system (Lab solar-6A), providing constant temperature and vacuum conditions for photolysis of water. The generated hydrogen was passed into an online gas chromatograph GC910 to determine the hydrogen production by integrating the area. The gas chromatograph detection parameters were set as follows: TCD thermal conductivity detector 110°C, vaporization chamber temperature 130°C, column furnace temperature 60°C, bridge current 60mA, argon carrier gas, The molecular sieve column was used to detect hydrogen production every 30 minutes to obtain the hydrogen production performance of the catalyst. The results are shown in Table 1.

[0224] As can be seen from Table 1, TCPC alone and PT2 carbon quantum dots alone produce less hydrogen under the same test conditions. However, the PT2-TCPC composite material can promote the separation of photogenerated charges, inhibit the recombination of photogenerated electrons and holes, form a charge transfer channel, and allow photogenerated electrons to reach the catalyst surface and generate hydrogen.

[0225] After 12 hours of photocatalytic reaction, the PT2-TCPC composite material still has a high catalytic ability. After the catalyst cycle stability test, the morphology and structure of the sample remain consistent with those before the reaction, and the catalyst has good stability.

[0226] Table 1: Photocatalytic performance test of PT2-TCPC composite materials

[0227]

[0228] 4.2 Effects of composite ratio and ultrasonic time on catalytic performance

[0229] The following experiments test the effects of different assembly conditions, including the ratio of PT2 to TCPC, ultrasonic time, etc. on the hydrogen production performance of PT2-TCPC composite materials, for different precursor ratios:

[0230] Precursor ratio experiment: 5 groups of TCPC and PT2 containing different masses were mixed by ultrasonic mixing according to Example 1 to obtain PT2-TCPC composite materials, and the hydrogen production performance was tested. The results are shown in Table 2.

[0231] It can be seen from Table 2 that when the mass ratio is PT2:TCPC=1:0.5, there is a higher photocatalytic hydrogen production performance, and when the mass ratio is 1:(0.5-2), a PT2-TCPC composite material with better photocatalytic performance can be obtained.

[0232] Table 2: Photocatalytic hydrogen production performance test of materials obtained with different PT2-TCPC composite precursor concentrations

[0233] PT2:TCPC (mass ratio) Photocatalytic hydrogen production performance (mmol / g / h) 1:0.2 40.32 1:0.5 92.20 1:1 86.07 1:1.5 82.32 1:2 76.43

[0234] Example 5: Photocatalytic hydrogen production from different types of fullerene derivative carbon quantum dot composite materials

[0235] Prepare C according to the preparation method of Example 2 60 (C(COOH)2)2,C 70 (C(COOH)2)2,Sc3N@C 80Fullerene derivatives such as (C(COOH)2)2 were prepared into composite materials with PT2 carbon quantum dots according to the above preparation method. The hydrogen production performance is shown in Table 3 below:

[0236] Table 3: Hydrogen production performance of composite materials of different fullerene derivatives and PT2 carbon quantum dots

[0237] Fullerene derivatives Photocatalytic hydrogen production performance (mmol / g / h) <![CDATA[C 60 (C(COOH)2)2-PT2]]> 80.91 <![CDATA[C 70 (C(COOH)2)2-PT2]]> 90.23 <![CDATA[Sc3N@C 80 (C(COOH)2)2-PT2]]> 122.54

[0238] From the results in Table 3, we can see that C 60 (C(COOH)2)2, C 70 (C(COOH)2)2 and Sc3N@C 80 (C(COOH)2)2 all have good photocatalytic hydrogen production performance, and the photocatalytic performance of metal fullerene derivative composite materials is better than that of hollow fullerene derivatives and carbon quantum dots. This is because the photocatalytic hydrogen production performance is closely related to the rate of photogenerated charge separation and transmission. The charge separation rate of metal fullerene composite materials is faster, which promotes the efficiency of photocatalytic hydrogen production.

[0239] Table 4: Hydrogen production performance of different fullerene derivative carbon quantum dot composite materials

[0240] Composite material name Photocatalytic hydrogen production performance (mmol / g / h) TCPC 0 PT2 1.02 PT4 0.96 PT5 1.04 TCPC (negatively charged surface)-PT2 90.08 TAPC (positively charged surface)-PT4 100.84 THPC (with hydrogen bond donor on the surface)-PT5 92.21

[0241] From the results in Table 4, it can be seen that TCPC-PT2, TAPC-PT4, and THPC-PT5 composite materials all have good photocatalytic hydrogen production performance. Among them, the positively charged groups on the surface of aminofullerene are more conducive to accepting photogenerated electrons, improving the efficiency of photogenerated charge separation, and thus improving the activity of photocatalytic hydrogen production.

[0242] Example 6: Comparison of hydrogen production performance of different fullerene composite photocatalytic materials

[0243] Some representative fullerene photocatalytic materials were selected for performance comparison, and the particle sizes of different materials in water and the hydrophilic angles of different materials were tested using dynamic light scattering (DLS). The results are shown in Table 5 below, where the preparation method or source of the composite material is as follows.

[0244] Control group C 60 -TiO2: 4 mg C 60 Add 2 ml of xylene and dissolve it in ultrasonic. Then, add 1.7 ml of tetrabutyl titanate to the mixture containing C under stirring. 60 Then, 30 mL of water was added to the xylene solution and stirred for 1 h. The resulting suspension was transferred to a 100 ml reactor and kept at 180 °C for 10 h. After the reaction, the temperature was lowered to obtain a suspension containing C 60 Supported titanium dioxide composite C 60-TiO2 solution, the solution was centrifuged and filtered, washed with toluene 3 times, then washed with anhydrous ethanol 3 times, and dried in a vacuum drying oven at 40 ° C overnight to obtain C 60 -TiO2 nanoparticles.

[0245] Control group C 60 -PVP assembly preparation: Refer to the published literature Bhullar, N., Sharma, A. Clean and dry route of synthesis of C60 / polyvinylpyrrolidone composite using supercritical carbon dioxide. Polym. Bull. 76, 5939–5956 (2019).

[0246] Control group C 60 -β-cyclodextrin preparation: Refer to published literature Zhang, Y., Ye, D., Gao,

[0247] Preparation of TAPC-citric acid-ethylenediamine carbon dots :First, citric acid (72 mg) was dissolved in deionized water (10 mL), and different amounts of ethylenediamine (25, 50, 75, 100, 150 μL) were added and mixed evenly. The solution was transferred to a polytetrafluoroethylene (Teflon) lined autoclave, placed in an oven at different temperatures (150, 200, 250 ° C), and the reaction was continued for 8 hours. After the reaction, the autoclave was taken out and cooled naturally. The obtained solution was loaded into a dialysis bag with a molecular weight cutoff of 500-1000 Da, and dialyzed for 48 hours to completely remove small molecules to obtain carbon quantum dots. Take 5 mL of the dialyzed carbon quantum dot aqueous solution and 5 mL of 1 mg / mL TAPC aqueous solution and mix them evenly by ultrasonication for 3 hours. Since the carbon quantum dots have carboxyl groups on the surface and TAPC has amino groups, the two are fully combined through electrostatic interaction, and then dialyzed for 48 hours with a molecular weight cutoff of 3000 Da to remove unbound TAPC to obtain a composite material.

[0248] Preparation of TCPC-ethylenediamine-o-phenylenediamine carbon dots:First, o-phenylenediamine (30 mg) was dissolved in 1 mmol HCl (30 mL), and different amounts of ethylenediamine (25, 50, 75, 100, 150 μL) were added respectively and mixed evenly. The solution was transferred to a polytetrafluoroethylene (Teflon) lined autoclave, placed in an oven at different temperatures (150, 200, 250 ° C), and the reaction was continued for 12 hours. After the end, the autoclave was taken out and cooled naturally. The obtained solution was loaded into a dialysis bag with a molecular weight cutoff of 500-1000 Da, and dialyzed for 48 hours to completely remove small molecules to obtain carbon quantum dots. Take 5 mL of the dialyzed carbon quantum dot aqueous solution and 5 mL of 1 mg / mL TCPC aqueous solution and mix them evenly by ultrasonication for 3 hours. Since the carbon quantum dots have amino groups on the surface and TCPC has carboxyl groups, the two are fully combined through electrostatic interaction, and then dialyzed for 48 hours with a molecular weight cutoff of 3000 Da to remove unbound TCPC to obtain a composite material.

[0249] C 60 Preparation of (OH)n: 7 mL of 30% hydrogen peroxide solution and 3 mL of 40% sodium hydroxide were added to a 100 mL round bottom flask, and 200 mg of fullerene C was added. 60 , then add a magnetic stirrer, stir with a magnetic stirrer for 24 hours (temperature: 70℃, speed: 1000r / min), and filter with a filter to obtain a brown-yellow solution. Add the above brown-yellow solution to a 50ml centrifuge tube, and then add an excess of 95% ethanol. After centrifugation (speed: 10000r / min, time: 4min), remove the upper colorless solution, dissolve the collected precipitate in ultrapure water to obtain a yellow clear solution. Put the above yellow clear solution into a dialysis bag (cutoff molecular weight is 3500) and dialyze it in ultrapure water to obtain a yellow solution. The obtained yellow solution is placed in a 50mL plastic centrifuge tube, frozen with liquid nitrogen, and then placed in a freeze dryer for freeze drying (you can get the fullerene hydroxyl derivative C 60 (OH)n.

[0250] C 60 (OH)n-TiO2 nanoparticles: Under ultrasonic conditions, 1 mg C 60 Hydroxylated derivative C 60 (OH)n, 99 mg (1.24 mmol) granular titanium dioxide and 50 mL ethanol were mixed to obtain a mixed solution, which was placed in a 100 mL reactor and kept at 100 °C for 12 h. After cooling, a mixture containing C 60 Titanium dioxide composites modified by hydroxylated derivatives C 60 The (OH)n-TiO2 solution was centrifuged and filtered, washed three times with deionized water, then washed three times with anhydrous ethanol, and dried in a vacuum oven at 40°C overnight to obtain C 60 (OH)n-TiO2 nanoparticles.

[0251] C 60 (OH)n-TiO2 nanosheets: Under ultrasonic conditions, 1 mg C 60 Hydroxylated derivative C 60 (OH)n, 99 mg (1.24 mmol) of flaky titanium dioxide and 50 mL of ethanol were mixed to obtain a mixed solution, which was placed in a 100 mL reactor and kept at 100 °C for 12 h. After cooling, a mixture containing C 60 Titanium dioxide composites modified by hydroxylated derivatives C 60 The (OH)n-TiO2 solution was centrifuged and filtered, washed three times with deionized water, then washed three times with anhydrous ethanol, and dried in a vacuum oven at 40°C overnight to obtain C 60 (OH)n-TiO2 nanosheets.

[0252] TAPC-TiO2 nanosheets: 90 ml of tetrabutyl titanate was poured into a 1 L beaker, and 450 mL of deionized water was also poured into the beaker under magnetic stirring to mix evenly. Subsequently, 20 mL of 5 mg / mL TAPC aqueous solution was poured into the system, and stirring was continued for 2 h. The resulting suspension was transferred to a 1000 mL reactor and kept at 160 ° C for 6 h. After the reaction, the solution was cooled to obtain a solution containing the composite material. The solution was centrifuged and filtered, washed 3 times with deionized water, and then washed 3 times with anhydrous ethanol. After drying in an oven at 80 ° C overnight, TAPC-TiO2 nanosheets were obtained.

[0253] C 60 or C 70 Amination derivative C 60 (EDA) n or C 70 (EDA) n Preparation: Weigh 50 mg (0.069 mmol) C 60 or 58.3 mg C 70 (0.069mmol) powder was dissolved in 25mL o-xylene solution, ultrasonically dispersed for 30min, 50mL ethylenediamine was added to a 100mL conical flask, and magnetically stirred for 24h (room temperature, 1000r / min). The reactant was filtered to obtain a brown-red solution. The components of the solution were mainly ethylenediamine and C 60 (EDA) n or C 70 (EDA) nand solvent o-xylene. Add the obtained solution to a 250ml round-bottom flask, and completely dry the filtrate by rotary evaporation (temperature: 60°C, speed: 80r / min). Add ultrapure water to dissolve. If there is a small amount of insoluble matter, add a little dilute hydrochloric acid (concentration: 1 mol / L) to the round-bottom flask, and shake the flask to dissolve the evaporated matter on the inner wall in dilute hydrochloric acid to obtain a brown-red clear solution. Use NaOH aqueous solution (concentration: 10 mol / L) to neutralize the solution to a pH of 5 to ensure that the excess ethylenediamine exists in the form of chloride and can be fully removed in the subsequent dialysis step. Put the neutralized solution into a dialysis bag (cut-off molecular weight of 3500) and dialyze it in ultrapure water for 48 hours.

[0254] C 60 (EDA) n Preparation of TiO2 nanosheets: 90 ml of tetrabutyl titanate was poured into a 1L beaker, and 450 mL of deionized water was also poured into the beaker under magnetic stirring to mix evenly; then, 20 mL of 5 mg / mL of the above-prepared C 60 (EDA) n The aqueous solution was added to the system and stirred for 2 h. The resulting suspension was transferred to a 1000 mL reactor and kept at 160 °C for 6 h. After the reaction, the temperature was lowered to obtain a composite material solution. The solution was centrifuged and filtered, washed with deionized water for 3 times, then washed with anhydrous ethanol for 3 times, and dried in an oven at 80 °C overnight to obtain C 60 (EDA) n / TiO2 nanosheets.

[0255] C 70 (EDA) n / TiO2 nanosheets: 90 ml of tetrabutyl titanate was poured into a 1 L beaker, and 450 mL of deionized water was also poured into the beaker under magnetic stirring to mix evenly; then, 20 mL of 5 mg / mL of the prepared C 70 (EDA) n The aqueous solution was added to the system and stirred for 2 h. The resulting suspension was transferred to a 1000 mL reactor and kept at 160 °C for 6 h. After the reaction, the temperature was lowered to obtain a composite material solution. The solution was centrifuged and filtered, washed with deionized water for 3 times, then washed with anhydrous ethanol for 3 times, and dried in an oven at 80 °C overnight to obtain C 70 (EDA) n / TiO2 nanosheets.

[0256] C 70 (C(COOH)2)n-ZnPc-TiO2 nanosheets: Synthetic C 70(C(COOH)2)n: 25mg was dispersed evenly in a mixture of 35mL methanol and 70mL deionized water by ultrasonication for 15min. A mixture of 6.8ml (19.92mmol) of tetrabutyl titanate and 35mL ethanol was added dropwise under stirring. Stirring was continued for 2h to obtain a suspension after uniform dispersion. The suspension was transferred to a 200mL hydrothermal reactor and reacted at 180℃ for 10h, wherein: tetrabutyl titanate was first hydrolyzed to TiO2 in the hydrothermal reaction and then continued to react with fullerene carboxylic acid derivatives. After the reaction was completed, the solution was filtered to obtain a light brown sample. Wash with water and alcohol three times each, and finally dry in a vacuum oven at 80℃ for 12h to obtain a light brown solid C 70 (C(COOH)2)n--TiO2. 100mg C 70 (C(COOH)2)n-TiO2 was stirred in the dark for 12 hours in a solution of zinc phthalocyanine tetracarboxylate (ZnPc) in N,N-dimethylformamide, wherein: zinc phthalocyanine tetracarboxylate ZnPc was 17.65 mg, 0.033 mmol, and the solution was filtered after the reaction to obtain a green sample. The sample was washed with water and alcohol three times each, and finally dried in a vacuum oven at 80°C for 12 hours to obtain a green solid.

[0257] Sc3N@C 80 -TiO2 Nanosheets: 6 mg Sc3N@C 80 2 mL of xylene was added and ultrasonically dissolved, and then 1.7 mL of tetrabutyl titanate was added to the Sc3N@C 80 Then 30 mL of water was added to the xylene solution and stirred for 1 h. The resulting suspension was transferred to a 100 ml reactor and kept at 180 °C for 10 h. After the reaction, the temperature was lowered to obtain Sc3N@C 80 -TiO2 nanosheet suspension, filtered to obtain a solid, washed three times with toluene, then washed three times with anhydrous ethanol, and dried in a vacuum oven at 40 °C overnight to obtain Sc3N@C 80 -TiO2 nanosheets.

[0258] <h2 style=";text-align:left;direction:ltr">C<h2 style=";text-align:left;direction:ltr"> 60 <h2 style=";text-align:left;direction:ltr"> (EDA)<h2 style=";text-align:left;direction:ltr"> n <h2 style=";text-align:left;direction:ltr"> -BiVO3: Under ultrasonic conditions, 5 mg C 60 (EDA) n , 50 mg BiVO3 (bismuth metavanadate) and 50 mL ethanol were mixed to obtain a mixed solution, which was placed in a 100 mL reactor and kept at 100 ° C for 12 h. After cooling, a composite material C was obtained. 60 (EDA) n -BiVO3 suspension, the suspension was centrifuged and filtered, washed 3 times with deionized water, then washed 3 times with anhydrous ethanol, and dried in a vacuum oven at 40 °C overnight to obtain C 60 (EDA) n / BiVO3.

[0259] TAPC-ZnO: Under ultrasonic conditions, 5 mg TAPC, 80 mg ZnO and 50 mL ethanol were mixed to obtain a mixed solution, which was placed in a 100 mL reactor and kept at 100°C for 12 h. After cooling, a suspension containing TAPC-ZnO was obtained. The solid was filtered and washed three times with deionized water and then washed three times with anhydrous ethanol. TAPC-ZnO was obtained after drying in a vacuum drying oven at 40°C overnight.

[0260] C 60 (C(COOH)2)2-g-C3N4: Under ultrasonic conditions, 5 mg C 60 (C(COOH)2)2, 36 mg g-C3N4 and 50 mL ethanol were mixed to obtain a mixed solution, which was placed in a 100 mL reactor and kept at 100 °C for 12 h. After cooling, the composite material C 60 The suspension of (C(COOH)2)2-g-C3N4 was centrifuged and filtered, washed three times with deionized water, then washed three times with anhydrous ethanol, and dried in a vacuum oven at 40°C overnight to obtain C 60 (C(COOH)2)2-g-C3N4.

[0261] C 60 (C(COOH)2)2-Bi2WO6 super hydrophobic carbon film: Preparation of super-hydrophobic carbon film: ultrasonically clean the FTO conductive glass with water, ethanol, acetone, and isopropanol for 30 minutes in sequence. After cleaning, place the FTO conductive glass on a candle for calcination. After the soot is evenly deposited on the FTO surface, place the FTO conductive glass on a 200°C electric heating plate and heat it for a period of time. Mix 1% octadecyltrichlorosilane with toluene (1% means that the volume of octadecyltrichlorosilane accounts for 1% of the volume of toluene) to form solution A. Take 60 μL of solution A and spread it evenly on the entire cooled FTO conductive glass (width 0.9 cm * length 4 cm). Then place the conductive glass on a 150°C electric heating plate and heat it for 5 hours, then remove it for use. Immobilize C on the super-hydrophobic carbon film 60 (C(COOH)2)2 modified granular Bi2WO6 or C 60 (C(COOH)2)2 modified Bi2WO6 flakes: C immobilized on superhydrophobic carbon film 60 (C(COOH)2)2 modified granular Bi2WO6: 2.8 μL of octadecyltrichlorosilane was dissolved in 5 ml of ethanol to form solution A, and then 10 mg of C 60 (C(COOH)2)2: The modified granular Bi2WO6 was added to 100 μL of ethanol, and then 100 μL of solution A was added to form a mixture solution B. Then 60 μL of the mixture solution B (containing 3 mg C 60(C(COOH)2)2 modified granular Bi2WO3, 10 mg / 200 μL x 60 μL = 3 mg) was evenly drop-coated on the 0.9 cm*2 cm area (i.e. only part of the area was drop-coated) of the obtained super-hydrophobic carbon film. After the solvent evaporated, the cured sample was placed in an oven at 110°C for overnight insulation to obtain C 60 (C(COOH)2)2, modified granular Bi2WO6 / superhydrophobic film composites.

[0262] C 60 Self-assembled nanotubes-SnO2: Carbon tetrachloride was selected as the good solvent and isopropanol as the poor solvent. 10 mL of 0.5 mg / mL C 60 When the mesitylene solution was quickly injected into 40 mL of isopropanol with a syringe, the mixed solution was dispersed by ultrasound for 10 minutes and then allowed to stand for 12 hours. The precipitate was centrifuged at 11k in a high-speed centrifuge, the supernatant was poured off, and the solid precipitate at the bottom was collected. It was washed with isopropanol three times and dried in a vacuum drying oven at 40°C overnight to obtain C 60 Solid powder of nanotubes. SnO2 modified C 60 Preparation of nanotube composite materials: Take the prepared C 60 0.014mmol of solid powder of nanotubes was ultrasonically dispersed in a small amount of water to obtain a dispersion. Then 20mL of a mixed solution containing 0.022mmol SnCl2 and 0.026mmol citric acid was added to the dispersion, the mixed solution was placed in a 250mL round-bottom flask, heated to 120°C on an oil bath, and 20mL of a NaBH4 solution containing 1.32mmol was gradually added. Finally, the reaction was stirred under reflux for 6h. After the reaction was completed, the heating was stopped, and after the liquid in the flask was cooled to room temperature, the solid was separated on a high-speed centrifuge and washed 3 times with deionized water. After vacuum drying at 40°C, SnO2 and modified C 60 Solid powder of nanosheet composite material.

[0263] C 70 -CuTPP Nanorods: 10mgC 70 5 mg CuTPP (tetraphenyl copper porphyrin) was dissolved in 10 mL mesitylene, and ultrasonically mixed for 30 min to ensure uniform mixing. The insoluble matter was then removed by filter. 20 mL of n-hexane was added to the mixed solution at low temperature, and the mixture was allowed to stand for 8 h before being filtered to obtain C 70 -CuTPP nanorods, vacuum dried at 60 °C for 12 h.

[0264] TAPC-CoTCPP nanosheets:10 mg TAPC was dissolved in 5 mL 1 mmol / L dilute hydrochloric acid, and 10 mg CoTCPP was dissolved in 5 mL 1 mmol / L NaOH solution. After fully dissolved, the two solutions were ultrasonically mixed for 8 h to obtain blue-green solid TAPC-CoTCPP nanosheets, which were filtered and vacuum dried at 60 °C for 12 h.

[0265] Imidazole-modified C 60 or C 70 (ImC 60 / ImC 70 ) Preparation: Take 100mgC 60 or 120mgC 70 The product was dissolved in 60 mL of toluene, and 10 mg of sarcosine and 36 mg of 4-imidazole-1-ylbenzaldehyde were added. The reaction was carried out at 125° C. for 4 h under a nitrogen atmosphere. The solvent was evaporated to dryness and column chromatography was performed (eluent: toluene: triethylamine = 100:1) to obtain a brown solid.

[0266] I C 70 -CoPc Nanorods: 10 mg ImC 70 8 mg of cobalt phthalocyanine CoPc was dissolved in 5 mL of chloroform in a 20 mL sample bottle, and the solution was fully dissolved by ultrasonication for 20 min. The insoluble matter was removed by filter membrane, and 15 mL of isopropanol was slowly added to the bottle and allowed to stand for 6 h. The solid was filtered and vacuum dried at 60 ° C for 12 h to obtain ImC 70 -CoPc nanorods.

[0267] I C 60 -ZnTPP nanosheets : 10mg ImC 70 5mg tetraphenyl zinc porphyrin ZnTPP was dissolved in 5mL chloroform in a 20mL sample bottle, ultrasonicated for 20min to fully dissolve, insoluble matter was removed by filter membrane, 15mL isopropanol was slowly added to the bottle, and it was allowed to stand for 6h. The solid was filtered and dried in vacuum at 60℃ for 12h to obtain ImC 60 -ZnTPP nanosheets.

[0268] Sc3N@C 80 -ZnTPP nanosheets :10mg Sc3N@C 80 5 mg ZnTPP was dissolved in 10 mL mesitylene, and ultrasonically mixed for 30 min to ensure uniform mixing. The insoluble matter was then removed by filtering. 20 mL of n-hexane was added dropwise to the mixed solution, and the mixture was allowed to stand for 8 h before being filtered to obtain Sc3N@C 80 -ZnTPP nanosheets were dried under vacuum at 60 °C for 12 h.

[0269] The synthesis of fullerene-Ce6 derivatives was based on the published literature Di Sante M, Kaltenbrunner A, Lombardo M, Danielli A, Costantini PE, Di Giosia M, Calvaresi M. Putting a "C60 Ball" and Chain to Chlorin e6 Improves Its Cellular Uptake and Photodynamic Performances. Pharmaceuticals (Basel). 2023 Sep 20; 16(9): 1329.

[0270] SA-C 60 -Ce6 nanosheets; 10 mg C 60 -Ce6 was dissolved in 5 mL of chloroform in a 20 mL sample bottle, and fully dissolved by ultrasonication for 20 min. Insoluble matter was removed by filter membrane, and 15 mL of isopropanol was slowly added to the bottle and allowed to stand for 6 h. The solid was filtered and vacuum dried at 60 °C for 12 h to obtain SA-C 60 -Ce6.

[0271] SA-C 60 -Ce6-Cl nanosheets: 10 mg C 60 -Ce6-Cl was dissolved in 5 mL of chloroform in a 20 mL sample bottle, and fully dissolved by ultrasonication for 20 min. Insoluble matter was removed by filter membrane, and 15 mL of isopropanol was slowly added to the bottle and allowed to stand for 6 h. The solid was filtered and vacuum dried at 60 °C for 12 h to obtain SA-C 60 -Ce6-Cl.

[0272] SA-C 70 -Ce6-CN nanosheets: 10 mg C 70 -Ce6-CN was dissolved in 5 mL of chloroform in a 20 mL sample bottle, and fully dissolved by ultrasonication for 20 min. Insoluble matter was removed by filter membrane, and 15 mL of isopropanol was slowly added to the bottle and allowed to stand for 6 h. The solid was filtered and vacuum dried at 60 °C for 12 h to obtain SA-C 70 -Ce6-CN.

[0273] SA-C 60 -Ce6-OH nanosheets: 10 mg C 60 -Ce6-OH was dissolved in 5 mL of chloroform in a 20 mL sample bottle, and fully dissolved by ultrasonication for 20 min. Insoluble matter was removed by filter membrane, and 15 mL of isopropanol was slowly added to the bottle and allowed to stand for 6 h. The solid was filtered and vacuum dried at 60 °C for 12 h to obtain SA-C 60 -Ce6-OH.

[0274] Table 5: Dispersibility of different fullerene composite photocatalytic materials in water

[0275]

[0276]

[0277] It can be seen from the table that the fullerene quantum dot composite material has the smallest particle size and the smallest hydrophilic angle in water, and its dispersibility in water is better than that of other composite materials.

[0278] Table 6: Hydrogen production performance of different fullerene composite photocatalytic materials

[0279]

[0280]

[0281] Fullerene quantum dot materials showed the best hydrogen production effect due to the significant increase in dispersibility in water.

[0282] Example 7: Preparation and hydrogen production performance of hydrophilic modified fullerene phylloline composite material and fullerene carbon quantum dot composite material

[0283] Take 10 mg of the above-mentioned assembly material, disperse it into 1 mg / mL dispersant solution (the dispersant is polyethylene glycol (PEG), polyimide (PEI), polysorbate 80 (Tween 80)), stir it thoroughly for 48 hours, and then filter and dry it to obtain a hydrophilic modified assembly material.

[0284] 5 mg of the fullerene porphyrin hydrophilic modified composite material prepared above was added to 20 ml of distilled water, and 0.05 mg of chloroplatinic acid (catalyst mass fraction was 1% or 3%) was added as a co-catalyst, and 350 mg of ascorbic acid was added as a hole sacrificial agent. After the air in the system was exhausted, a full-band AM1.5 filter was used to simulate sunlight to carry out photocatalytic hydrogen production reaction.

[0285] The hydrogen production reaction was carried out in a glass-enclosed gas system (Lab solar-6A), providing constant temperature and vacuum conditions for photolysis of water. The generated hydrogen was passed into an online gas chromatograph GC910 to determine the hydrogen production by integrating the area. The gas chromatograph detection parameters were set as follows: TCD thermal conductivity detector 110°C, vaporization chamber temperature 130°C, column furnace temperature 60°C, bridge current 60mA, argon carrier gas, The molecular sieve column was used to detect hydrogen production every 30 minutes to obtain the hydrogen production performance of the catalyst. The results are shown in Table 7.

[0286] Table 7: Comparison of hydrogen production performance of different materials

[0287] Composite material name Photocatalytic hydrogen production performance (mmol / g / h) TCPC-PT2 116.09 <![CDATA[ImC 60 -ZnTPP nanosheets]]> 80.95 <![CDATA[ImC 60 -ZnTPP Tween 80]]> 61.77 <![CDATA[ImC 60 -ZnTPP PEG]]> 40.22 <![CDATA[ImC 60 -ZnTPP PEI]]> 32.23 <![CDATA[SA-C 60 -TPP]]> 10.69 <![CDATA[SA-C 60 -TPP PEI]]> 5.72

[0288] It can be seen from the above table that after adding dispersant, ImC 60 -ZnTPP and SA-C 60 -TPP's hydrogen production performance has been reduced to varying degrees. The reason is that although the hydrophilicity of the material is enhanced after the hydrophilic polymer is wrapped, it affects the contact between the active site and water, which is not conducive to the occurrence of hydrogen production reaction. Due to the hydrophilicity of carbon quantum dots, they can fully contact and disperse fullerenes without the need for additional dispersants, which is conducive to high-activity hydrogen production performance.

[0289] Example 8: Performance of fullerene photocatalytic materials in producing hydrogen-rich water

[0290] After the photocatalytic hydrogen production experiment, the residual hydrogen concentration in the water was detected. The commercial CT-8023 hydrogen-rich test hydrogen pen was used to measure the hydrogen concentration in the water. According to the group standard T / NAHIEM 16-2019 "Hydrogen-containing packaged drinking water", it is mentioned that "during the shelf life of the product, the hydrogen content is not less than 0.6 mg / L" (about 600 ppb), and in the hydrogen content test, it is mentioned that "the hydrogen content is determined by gas chromatography (the detection of hydrogen concentration can also be carried out by a detection method with the same accuracy as gas chromatography)". Use gas chromatography and hydrogen pen to test and compare the difference in hydrogen content between the two.

[0291] Table 8: Concentration of water hydrogen in TCPC-PT2 under illumination obtained using different detection methods

[0292]

[0293] The concentration of hydrogen in water detected by the hydrogen pen is not much different from the concentration in gas chromatography, which shows that the detection results of the hydrogen pen are credible.

[0294] Table 9: Comparison of performance of different fullerene (derivative) composite materials in producing hydrogen-rich water

[0295]

[0296]

[0297] As can be seen from the table above, the hydrogen content in the water increases significantly after adding fullerene photocatalytic materials, and a very high hydrogen concentration can be reached in a short time, which matches and is positively correlated with the photocatalytic hydrogen production performance. For materials with higher hydrogen production performance, standard hydrogen-rich water can be stably produced within 1 hour, and the hydrogen concentration will continue to rise within 20 hours under continuous illumination. This method of producing hydrogen-rich water is in line with the concept of green, low-cost, pollution-free, and sustainable development.

[0298] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. Application of fullerene composite materials in photocatalytic production of hydrogen-rich water, including: The composite material comprises fullerene or its derivatives and a photocatalyst material.

2. The use according to claim 1, wherein: The fullerene derivative is selected from fullerene modified with a hydrophilic group; Preferably, the hydrophilic group is selected from one or more of hydroxyl, carboxyl, amino, ethylenediamine and imidazole; Preferably, the fullerene derivatives include one or more of fullerene amino derivatives, fullerene carboxyl derivatives, fullerene hydroxylation derivatives, ethylenediamine-modified fullerene derivatives, and imidazole-modified fullerene derivatives; The photocatalyst material is selected from semiconductor materials and / or photosensitizer derivatives; Preferably, the semiconductor material is selected from one or more of titanium dioxide, bismuth tungstate, bismuth oxide, tungsten oxide, molybdenum oxide, zirconium oxide, carbon nitride, carbon quantum dots, manganese oxide, bismuth vanadate, zinc oxide and tin oxide; Preferably, the photosensitizer derivative is selected from one or more of non-metal porphyrin derivatives, metal porphyrin or its derivatives, metal phthalocyanine or its derivatives, bipyridine ruthenium, chlorophyll, eosin, porphyrine, rose bengal, rhodamine B, and methylene blue; Preferably, the photosensitizer derivative is selected from one or more of tetracarboxylate phthalocyanine zinc, tetraphenylzinc porphyrin, tetraphenylcopper porphyrin, and tetrakis(4-carboxyphenyl)cobalt porphyrin.

3. The use according to claim 1 or 2, wherein: The fullerene is at least one of hollow fullerene, metallofullerene, heterocyclic fullerene and endohedral fullerene; Preferably, the fullerene is C 2a 、M@C 2a 、M2@C 2a 、MA@C 2a 、M3N@C 2a 、M2C2@C 2a 、M2S@C 2a 、M2O@C 2a and M x A 3-x N@C 2a Any one or a mixture thereof, wherein M and A are both metal elements, and M and A are both selected from any one of Sc, Y and lanthanide metal elements, 30≤a≤60; 0≤x≤3; Preferably, the fullerene is selected from hollow fullerene C 2a Any one of; wherein 30≤a≤60, preferably 30, 35, 38, 39, 41 or 42; more preferably 30 or 35; Alternatively, the fullerene is selected from metallofullerene M2C2@C 2b or metallofullerene M'3N@C 2b Any one of; wherein 39≤b≤54, preferably 40, 41 or 42; Preferably, M is at least one of Sc, La, Y, and Dy; M' is at least one of Sc, La, Y, Ho, Lu, Dy, or Er; and M and M' are preferably Sc.

4. The use according to any one of claims 1 to 3, wherein: The composite material is a composite material formed by fullerene or its derivatives and carbon quantum dots; the fullerene and carbon quantum dots in the composite material are preferably combined through electrostatic interaction or hydrogen bond interaction.

5. The use according to any one of claims 1 to 4, wherein: The composite material is a composite material of TCPC and carbon quantum dots, a composite material of TAPC and carbon quantum dots, a composite material of THPC and carbon quantum dots, a composite material of TCPC and TiO2, a composite material of TAPC and TiO2, a composite material of THPC and TiO2, a composite material of C 60 Composite materials of (C(COOH)2)2 and carbon quantum dots, C 70 Composite materials of (C(COOH)2)2 and carbon quantum dots, Sc3N@C 80 Composite materials of (C(COOH)2)2 and carbon quantum dots, C 60 Composite materials with TiO2, C 60 Composite materials of (OH)n2 and TiO2, Sc3N@C 80 Composite materials with TiO2, C 60 Composite materials of (EDA)n3 and TiO2, C 70 Composite materials of (EDA)n3 and TiO2, composite materials of TAPC and zirconia, C 70 (C(COOH)2)n1-ZnPc-TiO2 composite materials, C 60 Composite materials of (C(COOH)2)2 and g-C3N4, C 60 Composite materials of (C(COOH)2)2 and Bi2WO6, C 60 Composite materials with SnO2, C 70 Composite materials with CuTPP, composite materials with TAPC and CoTCPP, ImC 70 Composite materials with CoPc, ImC 60 Composite materials with ZnTPP, SA-Sc3N@C 80 Composites with ZnTPP or SA-C 60 -Ce6 composite material; n1=1-10, preferably 1-4; n2 is 1-10, preferably 6-10; n3 is 1-10, preferably 6-10; Preferably, the composite material is a composite material of a hydrophilic fullerene derivative and carbon quantum dots; the hydrophilic fullerene derivative is selected from one or more of fullerene amino derivatives, fullerene carboxyl derivatives, and fullerene hydroxylation derivatives; Preferably, the hydrophilic fullerene derivative is selected from the group consisting of fullerene carboxyl derivatives TCPC, C 60 (C(COOH)2)2, C 70 (C(COOH)2)2 or Sc3N@C 80 (C(COOH)2)2, fullerene amino derivative TAPC or fullerene hydroxylation derivative THPC; Preferably, the composite material of the hydrophilic fullerene derivative and carbon quantum dots is selected from a composite material of TCPC and carbon quantum dots, a composite material of TAPC and carbon quantum dots, a composite material of THPC and carbon quantum dots, a composite material of C 60 Composite materials of (C(COOH)2)2 and carbon quantum dots, C 70 Composite materials of (C(COOH)2)2 and carbon quantum dots and Sc3N@C 80 One or more composite materials of (C(COOH)2)2 and carbon quantum dots.

6. The use according to any one of claims 1 to 5, wherein: The photocatalyst material is a hydrophilic material; Preferably, the hydrophilic material is hydrophilic carbon quantum dots, and the particle size of the carbon quantum dots is preferably 1 to 10 nm; Preferably, the carbon quantum dots have a core-shell structure, wherein the core is crystalline carbon having a graphite-like structure, and the shell is a hydrophilic group; the hydrophilic group is preferably selected from hydroxyl, carboxyl and / or amino groups.

7. The use according to any one of claims 1 to 6, wherein: The photocatalysis comprises the following steps: adding the fullerene composite material photocatalyst into an aqueous solution containing a sacrificial agent, evacuating the solution, and irradiating the solution with a xenon lamp; Preferably, the wavelength of the light is sunlight AM 1.5; preferably, the wavelength of the light is in the range of 420 to 800 nm; Preferably, the photocatalytic time is 1 to 24 hours.

8. A fullerene carbon quantum dot composite material, wherein: The fullerene includes fullerene and fullerene derivatives, and the fullerene derivatives include one or more of fullerene amino derivatives, fullerene carboxyl derivatives, and fullerene hydroxylation derivatives; Preferably, the carbon quantum dots are hydrophilic carbon quantum dots, and the particle size of the carbon quantum dots is preferably 1 to 10 nm; Preferably, the carbon quantum dots have a core-shell structure, wherein the core is crystalline carbon having a graphite-like structure, and the shell is a hydrophilic group; the hydrophilic group is preferably selected from hydroxyl, carboxyl or amino groups.

9. The composite material according to claim 7, wherein: The composite material is obtained by mixing the fullerene or fullerene derivative and carbon quantum dots; Wherein, the mass ratio of the carbon quantum dots to the fullerene derivative is 1:(0.1-10), preferably 1:(0.5-2).

10. A method for producing hydrogen-rich water by photocatalysis, the method comprising the following steps: The fullerene composite material according to any one of claims 1 to 7 or the fullerene carbon quantum dot composite material according to claim 8 or 9 is added to water as a photocatalyst, and a hole sacrificial agent and / or a co-catalyst are added, and after vacuuming and deoxygenation, an AM1.5 full-band light source is used for irradiation; Preferably, the amount of the catalyst is 1 to 10 mg, preferably 2 mg; Preferably, the hole sacrificial agent is selected from at least one of ascorbic acid, triethanolamine, methanol, formic acid and NaHCO3; Preferably, the promoter is selected from at least one of chloroplatinic acid, a metal promoter, a transition metal sulfide, a transition metal phosphide and a composite promoter; Preferably, the promoter is selected from at least one of Pt, Au, Ag and Pd; Preferably, the co-catalyst loading is 1 wt% to 10 wt%, more preferably 1 wt% to 3 wt%; Preferably, the light source is a 300W xenon lamp, including at least one of a visible light source and simulated natural light; Preferably, the intensity of the light source is selected from 300 to 500 mW / cm 2 ; Preferably, the light irradiation time is 0.5 to 20 hours, more preferably 3 to 6 hours, more preferably 3 hours.

Citation Information

Patent Citations

  • Wavelength adjustable carbon quantum dots, preparation method and applications thereof

    CN105236383A

  • CD (carbon dot) / CdS quantum dot / C3N4 catalyst and preparation method thereof

    CN107597166A

  • High-fullerene based carbon quantum dot and preparation method thereof

    CN109266338A

  • Ternary photocatalyst as well as preparation method and application thereof

    CN113134369A

  • Application of fullerene donor-acceptor composite material in photocatalysis

    CN113828356A