Beneficiation process for efficiently recovering micro-fine particle specularite
Through ultrasonic dispersion and pregelatinized cassava starch flocculation technology, the problem of fine particle loss and low recovery in high-gradient magnetic separation of micro-iron is solved, which improves the recovery rate of iron concentrate and reduces cost and environmental impact.
Patent Information
- Application Number
- CN202411180347.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
AI Technical Summary
Due to the weak magnetic properties of mirror iron ore, it is difficult to efficiently dress ore, and during the high-gradient magnetic separation process, fine-grain iron ore loss, ore mud cover and surface coagulation are prone to problems, resulting in a low recovery rate of magnetic concentrate.
Ultrasonic wave is used to pre-distribute the ore slurry, and pre-gelatinized cassava starch is used as a flocculant to selectively flocculate the fine-grained mirroferous iron ore, increasing its apparent size and improving magnetic separation efficiency.
It improves the recovery rate of fine-grained microscopic iron ore, reduces the loss of iron concentrate, increases the recovery rate of iron concentrate by 8 percentage points compared with conventional strong magnetic separation, and reduces the use of agents and environmental pollution.
Smart Images

Figure CN118904530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing, and relates to a high-gradient strong magnetic separation process for fine-grained specularite using ultrasonic waves to pre-disperse ore pulp and pregelatinized cassava starch as a flocculant. Background Art
[0003] High gradient magnetic separation technology is a physical ore separation method that separates materials according to their magnetic properties. It uses effective electric and permanent magnets to generate a strong background magnetic field, and at the same time generates a high magnetic field gradient through a magnetic medium to enhance the capture ability of magnetic particles, thereby achieving the purpose of separating materials. It is an efficient and important means of selecting fine-grained weak magnetic minerals. Specularite is a subspecies of hematite, which is mainly found in sedimentary metamorphic deposits and contact metasomatic-hydrothermal iron deposits. Due to its weak magnetism, it is a traditional ore that is difficult to select and difficult to utilize. In addition, specularite is often mixed with some gangue minerals. At present, high-quality iron concentrate can only be obtained by fine grinding. However, during the grinding process, specularite minerals are severely crushed, and the iron mineral particles become finer and finer, which also leads to the aggravation of the loss of fine iron minerals during high gradient magnetic separation. At the same time, due to the characteristics of small particle size, large specific surface area and small specific magnetic susceptibility of fine-grained weak magnetic iron minerals, it is easy to form ore mud cover, surface mutual coagulation and magnetic agglomeration inclusions, resulting in a low recovery rate of magnetic concentrate. Summary of the invention
[0004] In view of the above problems, the present invention provides a beneficiation process for efficiently recovering fine-grained specular iron ore. The process first uses ultrasound to disperse the fine-grained minerals in the slurry, and then uses pre-gelatinized starch to selectively flocculate the fine-grained specular iron ore by means of flocculation and agglomeration, thereby increasing the apparent size of the fine-grained specular iron ore and meeting the particle size requirements of subsequent separation operations. At the same time, it can eliminate unfavorable factors such as mechanical entrainment and ore mud covering. The process can efficiently beneficiate low-grade fine-grained specular iron ore, and can make the iron recovery rate in the iron concentrate reach more than 60% when the iron grade of the iron ore is above 40%, which is 8 percentage points higher than that of conventional high-intensity magnetic separation. The method comprises the following steps:
[0005] (1) Weigh an appropriate amount of specularia ore into a beaker and add water to form a slurry with a concentration of 15-20 wt%;
[0006] (2) using ultrasound to disperse the slurry prepared in step (1) for 0 to 1 minute to fully disperse the mineral particles;
[0007] (3) adjusting the pH value of the slurry obtained in step (2) to 9.0-11.0 with a sodium hydroxide solution;
[0008] (4) adding pregelatinized cassava starch to the resultant of step (3) and stirring, wherein the amount of pregelatinized cassava starch added is 10 to 50 g / t, the stirring speed is maintained at 200 to 300 r / min, and the stirring is performed at a uniform speed for 3 to 5 min;
[0009] (5) The pretreated slurry is subjected to strong magnetic separation using a periodic pulse high gradient magnetic separator to obtain a strong magnetic separation concentrate product.
[0010] In the above-mentioned flocculation and strong magnetic separation process of fine-grained specularite, the total iron grade of the specularite sample used is 26.00-28.00%, D 50 6.952μm, D 90 23.921μm;
[0011] In the above-mentioned process step (2) of flocculation and strong magnetic separation of fine-grained specularite, the ultrasonic instrument is a KQ3200E ultrasonic cleaner; in the above-mentioned process step (4) of flocculation and strong magnetic separation of fine-grained specularite, the pregelatinized cassava starch can be prepared according to the following method: weigh the pregelatinized cassava starch in a beaker, add water to make a solution with a concentration of 1%, place the beaker in a water bath with a magnetic stirrer, set the water bath temperature to 85-90°C, set the speed to 200-250r / min, and keep the water bath at a constant temperature for 20-30min until the solution is completely dissolved and becomes transparent, and take out the prepared pregelatinized cassava starch solution and place it at room temperature for use.
[0012] In the above-mentioned flocculation and strong magnetic separation process step (5) of fine-grained specular iron ore, the high gradient magnetic separation operation is: under the conditions of a background magnetic field of 300-700mT, a pulsation stroke of 4-24mm, and a pulsation frequency of 0-200r / min, the pretreated slurry is uniformly fed into the magnetic separator for separation.
[0013] The present invention has the following beneficial effects:
[0014] In the slurry treatment stage before the high gradient magnetic separation operation, the present invention uses ultrasound instead of dispersants to disperse the fine mineral particles in the slurry, which reduces the use of reagents and greatly reduces costs. In addition, ultrasound does not produce harmful chemicals and has no negative impact on the environment and humans. Secondly, ultrasound can quickly disperse the fine mineral particles in the slurry into single particles, improve the dispersion effect, and also promote the selective adsorption of subsequent flocculants on iron mineral particles. Using ultrasound to disperse mineral particles is a very effective, economical and practical method.
[0015] Since the particle size of fine iron mineral particles is small and the specific magnetic susceptibility is low, the magnetic force received during the magnetic separation process is weak, resulting in the loss of ultrafine iron minerals into the tailings, making the magnetic separation efficiency of fine minerals low. In order to solve this problem, the present invention adds pre-gelatinized cassava starch as a flocculant to the slurry before the high-gradient strong magnetic separation operation. The pre-gelatinized cassava starch is adsorbed on the surface of the specularite particles in a "chain" shape through the complexation of the terminal hydroxyl and carboxyl groups with iron atoms, and plays an adsorption and bridging role between the specularite particles, so that the fine specularite particles are selectively flocculated into agglomerates, increasing the apparent size of the target mineral. Compared with high-gradient magnetic separation without adding flocculants, the recovery rate of fine specularite is increased by about 8%, the recovery rate of fine specularite is increased, and the loss of fine specularite in the tailings is reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The present invention is a ore dressing process flow chart for efficiently recovering fine-grained specularite.
[0017] Figure 2 The ore pulp of specularite without ultrasonic treatment (left) and the ore pulp of specularite after ultrasonic treatment (right);
[0018] Figure 3 Metallographic microscope images of fine-grained quartzite ore without pregelatinized cassava starch (left) and with pregelatinized cassava starch (right).
[0019] Figure 4 These are metallographic microscope images of fine-grained mirror iron ore high-gradient magnetic separation concentrate, where the left one is the magnetic separation concentrate without the addition of pregelatinized cassava starch, and the right one is the magnetic separation concentrate with the addition of pregelatinized starch.
[0020] Figure 5 These are metallographic microscope images of fine-grained mirror iron ore high-gradient magnetic separation tailings, where the left one is the magnetic separation tailings without the addition of pregelatinized cassava starch, and the right one is the magnetic separation tailings with the addition of pregelatinized starch. DETAILED DESCRIPTION
[0021] The technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0022] The test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0023] In the embodiment of the present invention, a SN-OES-60SH cantilever electric stirrer is used to stir the slurry.
[0024] In the example of the present invention, a KQ3200E ultrasonic cleaner is used to disperse the slurry.
[0025] The periodic pulse high gradient magnetic separator used in the embodiment of the present invention has a specification of SSS-I-Φ145.
[0026] The method for preparing the pregelatinized cassava starch solution used in the examples of the present invention is:
[0027] Weigh 1 g of pregelatinized cassava starch into a beaker, add water to make a solution with a concentration of 1%, place the beaker in a water bath with a magnetic stirrer, set the water bath temperature to 90° C., set the speed to 250 r / min, and keep the constant temperature water bath for 30 minutes until the solution is completely dissolved and becomes transparent. Take out the prepared pregelatinized cassava starch solution and place it at room temperature for use.
[0028] Example 1
[0029] (1) Take two 100g samples of specularite with a TFe grade of 27.82% and place them in a glass beaker, add water to make a slurry with a concentration of 15%, stir evenly, and then use ultrasonic dispersion treatment for one of them for 30 seconds. The other group is not subjected to ultrasonic treatment.
[0030] (2) Under the condition of stirring speed of 500 r / min, sodium hydroxide solution was added to the slurry to adjust the pH value of the slurry to 10.0.
[0031] (3) Reduce the stirring speed to 300 r / min, add 10 g / t pregelatinized cassava starch solution to both slurries, and stir at a constant speed for 3 min.
[0032] (4) The pulse frequency of the periodic pulse high gradient magnetic separator was adjusted to 170r / min, the discharge volume of the magnetic separator was 50ml / s, and the background field strength of the magnetic separation was 500mT. The treated slurry was slowly added to the high gradient magnetic separator for magnetic separation. The slurry treated with ultrasound obtained a magnetic concentrate with an iron grade of 41.64% and an iron recovery rate of 60.62%; while the slurry not treated with ultrasound obtained a magnetic concentrate with an iron grade of 35.88% and an iron recovery rate of 62.25%.
[0033] The specularite slurry with and without ultrasonic treatment in Example 1 was observed using a metallographic microscope. The results are as follows: Figure 2 As shown. Figure 2In the figure, the left picture shows the original specularite pulp without ultrasonic treatment, and the right picture shows the original specularite pulp after ultrasonic treatment. By comparison, it can be seen that before ultrasonic treatment, the specularite particles in the pulp are adhered to the gangue minerals, and there is also a phenomenon of wrapping and being wrapped, which has an adverse effect on the subsequent strong magnetic separation operation; after ultrasonic treatment, most of the mineral particles in the pulp are dispersed and evenly distributed in the pulp in the form of monomers, which enhances the effect of subsequent selective flocculation operations, improves the quality of high-gradient magnetic separation concentrates, and reduces the inclusion of gangue minerals.
[0034] Example 2
[0035] (1) Two 100 g samples of specularite with a TFe grade of 27.82% were placed in a glass beaker, and water was added to form a slurry with a concentration of 15%. After stirring evenly, both slurries were subjected to ultrasonic treatment for 30 seconds.
[0036] (2) Under the condition of stirring speed of 500 r / min, sodium hydroxide solution was added to the slurry to adjust the pH value of the slurry to 10.0.
[0037] (3) Reduce the stirring speed to 300 r / min, add 10 g / t pregelatinized cassava starch solution to one group of slurries, and stir at a constant speed for 3 min. Do not add pregelatinized cassava starch solution to the other group, and stir at a constant speed for 3 min.
[0038] (4) The pulse frequency of the periodic pulse high gradient magnetic separator was adjusted to 170 r / min, the displacement of the magnetic separator was 50 ml / s, and the background field strength of the magnetic separation was 500 mT. The treated slurry was slowly added to the high gradient magnetic separator for magnetic separation. The slurry with 10 g / t pregelatinized cassava starch solution added obtained a magnetic concentrate with an iron grade of 41.47% and an iron recovery rate of 61.22%; while the slurry without the addition of pregelatinized cassava starch solution obtained a magnetic concentrate with an iron grade of 42.87% and an iron recovery rate of 52.44%.
[0039] The high gradient magnetic separation ore and product in Example 2 were observed using a metallographic microscope. The results are as follows: Figure 3 , Figure 4 and Figure 5 As shown. Figure 3 In the figure, the left picture shows the high gradient magnetic separation ore without adding pregelatinized cassava starch, and the right picture shows the high gradient magnetic separation ore with adding pregelatinized cassava starch. It can be found that when pregelatinized cassava starch is not added, the specularite particles are dispersed in the slurry and the ultrafine particles are clearly visible. After adding pregelatinized cassava starch, the specularite particles flocculate and the apparent size increases significantly. Figure 4The left picture shows the high-gradient magnetic concentrate without adding pregelatinized cassava starch, and the right picture shows the high-gradient magnetic concentrate with adding pregelatinized cassava starch. It can be seen from the figure that after adding pregelatinized cassava starch, the number of small-sized specularite particles in the magnetic concentrate increased significantly. This is mainly because the bridging effect of pregelatinized cassava starch increases the apparent size of fine specularite particles, generates higher magnetic force, and makes it easier to be captured in the magnetic field. Figure 5 The left picture shows the high gradient magnetic separation tailings without the addition of pregelatinized cassava starch, and the right picture shows the high gradient magnetic separation tailings with the addition of pregelatinized cassava starch. After adding pregelatinized cassava starch, the iron mineral particles in the magnetic separation tailings are significantly reduced, and are mainly composed of quartz and other gangue minerals.
Claims
1. A ore dressing process for efficiently recovering fine-grained specularite, the process mainly comprises the following steps: (1) Weigh an appropriate amount of specularia ore into a beaker and add water to form a slurry with a concentration of 15-20 wt%; (2) using ultrasound to disperse the slurry prepared in step (1) for 0 to 1 minute to fully disperse the mineral particles; (3) adjusting the pH value of the slurry obtained in step (2) to 9.0-11.0 with a sodium hydroxide solution; (4) adding pregelatinized cassava starch to the resultant of step (3) and stirring, wherein the amount of pregelatinized cassava starch added is 10 to 50 g / t, the stirring speed is maintained at 200 to 300 r / min, and the stirring is performed at a uniform speed for 3 to 5 min; (5) The pretreated slurry is subjected to strong magnetic separation using a periodic pulse high gradient magnetic separator to obtain a strong magnetic separation concentrate product.
2. The ore dressing method according to claim 1, characterized in that The total iron grade of the specularite sample is 26.00-28.00%, D 50 6.952μm, D 90 It is 23.921μm.
3. The ore dressing method according to claim 1, characterized in that The ultrasonic instrument is a KQ3200E ultrasonic cleaner.
4. The ore dressing method according to claim 1, characterized in that The preparation process of the pregelatinized cassava starch is as follows: weighing the pregelatinized cassava starch in a beaker, adding water to form a solution with a concentration of 1%, placing the beaker in a water bath pot with a magnetic stirrer, setting the temperature of the water bath pot to 85-90 DEG C, setting the rotation speed to 200-250r / min, and keeping the water bath at a constant temperature for 20-30 minutes until the solution is completely dissolved and becomes transparent, and taking out the prepared pregelatinized cassava starch solution and placing it at room temperature for use.
5. The ore dressing method according to claim 1, characterized in that The high gradient magnetic separation operation is: under the conditions of a background magnetic field of 300-700 mT, a pulsation stroke of 4-24 mm, and a pulsation frequency of 0-200 r / min, the pretreated slurry is uniformly fed into a magnetic separator for separation.