Super-amphiphobic anticorrosive antibacterial aluminum alloy coating as well as preparation method and application thereof

Through the combination technology of micro-arc oxidation and modified coating on the surface of aluminum alloy, the problem of insufficient anti-corrosion and anti-bacterial performance of aluminum alloy in complex environments is solved, and an ultra-double-radiated, anti-corrosion and anti-bacterial coating is achieved, suitable for the ocean and other complex environments.

CN118904681APending Publication Date: 2024-11-08GUANGXI ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118178.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing aluminum alloy coatings have insufficient anti-corrosion and antibacterial properties in complex environments, especially in marine environments, and are prone to corrosion. The preparation process is complex and costly, making it difficult to achieve ultra-double sparse (hydrophobic and oleophobic) properties.

Method used

Microarc oxidation treatment was performed on the surface of aluminum alloy, and a super double-radiated curing coating was prepared using modified metal oxide nanoparticles, epoxy resin and curing agent. Sodium silicate, KOH and B in the electrolyte were oxidized by microarc oxidation of sodium silicate, KOH and B in the electrolyte The composition of diaminetetraacetate and other components is adjusted to form a coating with super-double sparse characteristics.

Benefits of technology

It significantly improves the hydrophobic and antibacterial properties of the coating, reduces the self-corrosion current density of aluminum alloys, is suitable for marine and other complex environments, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994251960000071
    Figure BDA0004994251960000071
Patent Text Reader

Abstract

The invention discloses a super-amphiphobic anticorrosive antibacterial aluminum alloy coating as well as a preparation method and application thereof. The preparation method comprises the following steps that the aluminum alloy surface is polished and then cleaned, then micro-arc oxidation treatment is carried out, and washing and drying are carried out after the reaction is finished; the super-amphiphobic curing coating is sprayed to the surface of the aluminum alloy, and the super-amphiphobic curing coating is obtained after curing; the super-amphiphobic curing coating comprises modified metal oxide nanoparticles, epoxy resin and a curing agent, the metal oxide nano particles comprise TiO2 nano particles. The coating prepared by the invention has the characteristics of super-amphiphobic property, corrosion resistance, antifouling property, antibacterial property and self-cleaning property, not only can be applied to marine corrosion resistance, but also can be applied to the fields of buildings, photovoltaics, furniture and the like needing corrosion resistance and antibacterial property, and is also suitable for acid-base, high-temperature and other complex environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum alloy coating, and in particular to a super-amphiphobic anticorrosive and antibacterial aluminum alloy coating and a preparation method and application thereof. Background Art

[0002] In many fields of modern industry, aluminum alloys have become indispensable materials due to their excellent properties, such as light weight, high strength, good processing performance and electrical conductivity. However, aluminum alloys face many challenges in practical applications, especially under complex and changeable environmental conditions. Their insufficient anti-corrosion and antibacterial properties seriously limit their wider application. For example, in the marine environment, aluminum alloys will be corroded by seawater, and substances such as chloride ions in it can easily cause corrosion of aluminum alloys, resulting in a decrease in structural strength, affecting the normal operation and service life of the equipment. The attachment of microorganisms in the ocean can also seriously affect the life of metal materials. Pseudomonas aeruginosa, the main bacteria in the ocean, is also highly corrosive and accelerates the corrosion of metal materials.

[0003] In order to meet these challenges, it is urgent to develop aluminum alloy coatings with super-amphiphobicity (super-hydrophobicity and super-oleophobicity), anti-corrosion and antibacterial multifunctionality. However, the existing preparation methods of aluminum alloy coatings have many shortcomings, such as it is difficult to achieve the level of super-amphiphobicity (both hydrophobic and super-oleophobicity), and the self-corrosion current density of the coating is not high, only reaching 10 -8 A / cm 2 About 100% of the total surface area is 20000 square meters, which cannot provide sufficient anti-corrosion protection for aluminum alloys. In terms of antibacterial properties, the main focus is on Escherichia coli and Staphylococcus aureus. In addition, the preparation process of some anti-corrosion coatings is complicated and costly, which is not conducive to large-scale production and wide application. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing a super-amphiphobic anticorrosive and antibacterial aluminum alloy coating. Micro-arc oxidation is performed on the surface of the aluminum alloy before spraying the coating. While improving the corrosion resistance, the hydrophobic and oleophobic properties of the coating are further improved. The contact angles of water and oil of the prepared coating are both >150°, and the rolling angles are both <10°. It has super-amphiphobic characteristics and obvious antibacterial properties.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] The present invention provides a method for preparing a super-amphiphobic anticorrosive and antibacterial aluminum alloy coating, comprising the following steps:

[0007] (1) Clean the aluminum alloy surface after grinding;

[0008] (2) performing micro-arc oxidation on the aluminum alloy treated in step (1), and washing and drying after the reaction is completed;

[0009] The micro-arc oxidation electrolyte contains: 12-16 g / L sodium silicate, 1.0-1.5 g / L KOH and 0.8-1.2 g / L disodium ethylenediaminetetraacetate;

[0010] The parameters of micro-arc oxidation treatment are: duty cycle 10% to 80%, frequency 100 to 400 Hz, current density 6 to 30 A / dm 2 , oxidation time 10~60min;

[0011] (3) spraying the super-amphiphobic cured coating onto the surface of the aluminum alloy treated in step (2), and obtaining a super-amphiphobic cured coating after curing;

[0012] The super-amphiphobic curing coating comprises modified metal oxide nanoparticles, epoxy resin and curing agent; the metal oxide nanoparticles comprise TiO2 nanoparticles;

[0013] The preparation process of the modified metal oxide nanoparticles comprises the following steps:

[0014] (3-1) adding perfluorosilane and tetraethyl orthosilicate into anhydrous ethanol and stirring to obtain a solution;

[0015] (3-2) adding metal oxide nanoparticles to the solution obtained in step (3-1), and continuing stirring to form an emulsion suspension;

[0016] (3-3) Adding an inducing agent to the emulsion suspension obtained in step (3-2) to form a coating layer on the surface of the metal oxide nanoparticles, thereby obtaining a dispersion containing modified metal oxide nanoparticles.

[0017] Preferably, the metal oxide nanoparticles further include a bactericide; the bactericide is at least one of ZnO nanoparticles or CuO nanoparticles.

[0018] Preferably, the mass percentage of TiO2 nanoparticles in the metal oxide nanoparticles is 83% to 90%.

[0019] Preferably, the ratio of the sum of the mass of the epoxy resin and the curing agent to the mass of the modified metal oxide nanoparticles is 0.1 to 0.8:1.

[0020] Preferably, the perfluorosilane is 1H,1H,2H,2H-perfluorodecyltriethoxysilane.

[0021] Preferably, the mass ratio of perfluorosilane, tetraethyl orthosilicate and metal oxide nanoparticles is: (5-7): (2-4): (3-5).

[0022] Preferably, the inducer is ammonia water or sodium methyl silicate; the mass ratio of the inducer to tetraethyl orthosilicate is 0.2 to 2:1.

[0023] Preferably, the preparation process of the super amphiphobic cured coating is:

[0024] Add epoxy resin and curing agent to the dispersion containing metal oxide nanoparticles obtained in step (3-3), stir for 1.5 to 2.5 hours to obtain a mixed suspension; spray the mixed suspension onto the surface of the aluminum alloy after micro-arc oxidation, and cure at 60 to 150°C.

[0025] The present invention also provides a super-amphiphobic anticorrosive and antibacterial aluminum alloy coating, comprising a micro-arc oxidation layer located on the surface of the aluminum alloy and a super-amphiphobic cured coating located on the surface of the micro-arc oxidation layer;

[0026] The micro-arc oxidation layer is a film layer formed by micro-arc oxidation treatment using a micro-arc oxidation electrolyte; the micro-arc oxidation electrolyte contains: 12-16 g / L sodium silicate, 1.0-1.5 g / L KOH and 0.8-1.2 g / L disodium ethylenediaminetetraacetate;

[0027] The super-amphiphobic cured coating is a film layer formed by spraying the super-amphiphobic cured coating onto the surface of the micro-arc oxidation layer and curing; the super-amphiphobic cured coating includes modified metal oxide nanoparticles, epoxy resin and curing agent; the modified metal oxide nanoparticles are metal oxide nanoparticles coated with a silicon film on the surface; the silicon film surface contains hydroxyl groups and perfluorosilane grafts; the metal oxide nanoparticles include TiO2 nanoparticles.

[0028] Preferably, the electrical parameters of micro-arc oxidation are: duty cycle 18-22%, frequency 380-420 Hz, current density 10-16 A / dm 2 , oxidation time 20 to 30 minutes.

[0029] The present invention also provides an application of the super-amphiphobic anticorrosion and antibacterial aluminum alloy coating, which is used for the anti-corrosion and anti-fouling of aluminum alloys used in marine environments.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] (1) The preparation method of the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating of the present invention is to perform micro-arc oxidation on the aluminum alloy surface before spraying the coating. The super-amphiphobic surface first needs to construct a micro / nano structure and then be modified with a low surface energy substance. The present invention adjusts the composition of the micro-arc oxidation electrolyte and the electrical parameters of the micro-arc oxidation so that the film layer obtained by the micro-arc oxidation treatment has an appropriate roughness and has many micropores on the surface, providing the micro / nano structure necessary for the super-amphiphobic surface. Therefore, micro-arc oxidation of the aluminum alloy surface before spraying the coating further improves the hydrophobicity and oleophobicity of the coating. In addition, the micro-arc oxidation coating as an intermediate layer can not only provide good adhesion between the super-amphiphobic cured coating and the aluminum alloy, but also capture air in the gap to form an air layer, forming an air cushion, reducing the contact area between the corrosive liquid and the solid surface, while significantly increasing the liquid-gas contact area, further limiting the corrosive medium (Cl - ) transmission, reducing the self-corrosion current density of aluminum alloy, thereby improving the corrosion resistance.

[0032] (2) The preparation method of the super-amphiphobic anti-corrosion and antibacterial aluminum alloy coating of the present invention uses tetraethyl orthosilicate to coat metal oxide nanoparticles. The silicon film generated by hydrolysis contains hydroxyl groups and organic silane grafting, so that the coated nanoparticles have low surface energy, which is beneficial to improving the hydrophobic and oleophobic properties.

[0033] (3) The preparation method of the super-amphiphobic anti-corrosion and antibacterial aluminum alloy coating of the present invention is to compound metal oxide nanoparticles with antibacterial properties and add an appropriate amount of bactericide ZnO nanoparticles or CuO nanoparticles on the basis of TiO2 nanoparticles, which is beneficial to the improvement of antibacterial properties. The antibacterial rate against Pseudomonas aeruginosa reaches more than 99%.

[0034] (4) The super-amphiphobic anti-corrosion and antibacterial aluminum alloy coating of the present invention has the characteristics of super-amphiphobic, anti-corrosion, anti-fouling, antibacterial, and self-cleaning. It can not only be used for marine anti-corrosion, but also can be used in fields such as construction, photovoltaics, and furniture that require anti-corrosion and antibacterial. It is also suitable for complex environments such as acid, alkali, and high temperature. DETAILED DESCRIPTION

[0035] The present invention will be further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0036] Example 1

[0037] The super-amphiphobic anti-corrosion and antibacterial aluminum alloy coating of this embodiment is prepared as follows:

[0038] 1. Aluminum alloy surface pretreatment

[0039] 1.1 Pretreatment of aluminum alloy: Use 400#, 800#, and 1200# sandpaper to polish the surface of the aluminum alloy until the surface of the sample is smooth and has no obvious scratches. Use 50g / L NaOH, ethyl acetate, anhydrous ethanol, and deionized water to ultrasonically clean the sample and dry it.

[0040] 1.2 Micro-arc oxidation: Prepare micro-arc oxidation electrolyte (electrolyte composition: 12g / L sodium silicate, 1g / L KOH and 0.8g / L disodium ethylenediaminetetraacetate), and pour it into the micro-arc oxidation electrolytic cell. Fix the aluminum alloy as the anode in the micro-arc oxidation electrolytic cell, and set the micro-arc oxidation electrical parameters (duty cycle 30%, frequency 350Hz, current density 12A / dm 2 , oxidation time 20min), and micro-arc oxidation treatment was carried out.

[0041] 1.3 Post-treatment: After the micro-arc oxidation, the aluminum alloy samples were washed with anhydrous ethanol and deionized water, respectively, and finally dried to obtain an aluminum alloy covered with a micro-arc oxidation layer.

[0042] 2. Preparation of Modified Composite Particles

[0043] 2.1 Add 6 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and 5 mL of tetraethyl orthosilicate into anhydrous ethanol and stir.

[0044] 2.2 Add 4g TiO2 (particle size D≤100nm) and 0.3g ZnO (particle size D≤100nm) to the above solution and continue stirring to form an emulsion suspension.

[0045] 2 mL of ammonia water was added to the suspension as an inducing agent to induce the hydrolysis and polycondensation of silane. Stirring was continued, and after reacting for 7 h, the suspension was centrifuged at 4000 rpm and dried to obtain modified composite particles.

[0046] 3. Coating curing

[0047] 3.1 Add 1.5 g of the modified composite particles into anhydrous ethanol and disperse them by ultrasonic for 25 min.

[0048] 3.2 Add 0.6g of epoxy resin E-44 and 0.6g of curing agent (methyltetrahydrophthalic anhydride, C9H 10 O3), stirred for 2h to obtain a mixed suspension.

[0049] 3.3 The mixed suspension is sprayed onto the surface of the aluminum alloy after micro-arc oxidation, and heated to 80°C for curing, so as to prepare a super-amphiphobic cured coating on the surface of the micro-arc oxidation layer of the aluminum alloy, thereby obtaining a super-amphiphobic and anti-corrosion and antibacterial multifunctional aluminum alloy coating.

[0050] Example 2

[0051] The super-amphiphobic anti-corrosion and antibacterial aluminum alloy coating of this embodiment is prepared as follows:

[0052] 1. Aluminum alloy surface pretreatment

[0053] 1.1 Pretreatment of aluminum alloy: Use 400#, 800#, and 1200# sandpaper to polish the surface of the aluminum alloy until the surface of the sample is smooth and has no obvious scratches. Use 50g / L NaOH, ethyl acetate, anhydrous ethanol, and deionized water to ultrasonically clean the sample and dry it.

[0054] 1.2 Micro-arc oxidation: Prepare micro-arc oxidation electrolyte (electrolyte composition: 16g / L sodium silicate, 1.5g / L KOH and 1.2g / L disodium ethylenediaminetetraacetate), and pour it into the micro-arc oxidation electrolytic cell. Fix the aluminum alloy as the anode in the micro-arc oxidation electrolytic cell, and set the micro-arc oxidation electrical parameters (duty cycle 20%, frequency 400Hz, current density 14A / dm 2 , oxidation time 25min), and micro-arc oxidation treatment was carried out.

[0055] 1.3 Post-treatment: After the micro-arc oxidation, the aluminum alloy samples were washed with anhydrous ethanol and deionized water, respectively, and finally dried to obtain an aluminum alloy covered with a micro-arc oxidation layer.

[0056] 2. Preparation of Modified Composite Particles

[0057] 2.1 Add 6 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and 6 mL of tetraethyl orthosilicate into anhydrous ethanol and stir.

[0058] 2.2 Add 4g TiO2 (particle size D≤100nm) and 0.3g ZnO (particle size D≤100nm) to the above solution and continue stirring to form an emulsion suspension.

[0059] 2.3 Add 0.5 mL of ammonia water as an inducing agent to the suspension to induce the hydrolysis and polycondensation of silane. Continue stirring, react for 7 hours, centrifuge at 4000 rpm, and dry to obtain modified composite particles.

[0060] 3. Coating curing

[0061] 3.1 Add 1.5 g of the modified composite particles into anhydrous ethanol and disperse them by ultrasonic for 25 min.

[0062] 3.2 Add 0.3g of epoxy resin E-44 and 0.6g of curing agent (methyltetrahydrophthalic anhydride, C9H 10 O3), stirred for 2h to obtain a mixed suspension.

[0063] The mixed suspension is sprayed onto the surface of the aluminum alloy after micro-arc oxidation, and heated and cured at 100°C to obtain a multifunctional aluminum alloy coating with super amphiphobic properties and anti-corrosion and antibacterial properties.

[0064] Example 3

[0065] In the modified composite particle preparation stage, ZnO (particle size D≤100 nm) is replaced by CuO (particle size D≤100 nm). The remaining conditions are the same as those in Example 2.

[0066] Example 4

[0067] In the preparation stage of the modified composite particles, the inducer was changed from ammonia water to sodium methyl silicate. The other conditions were the same as those in Example 2.

[0068] Example 5

[0069] During the preparation of the modified composite particles, no bactericide was added. The remaining conditions were the same as in Example 1.

[0070] Comparative Example 1

[0071] This comparative example is an untreated aluminum alloy.

[0072] Comparative Example 2

[0073] This comparative example is an aluminum alloy treated by micro-arc oxidation, and the treatment steps are the same as the aluminum alloy surface pretreatment steps in Example 1.

[0074] Comparative Example 3

[0075] This comparative example is a coating that has not been treated with micro-arc oxidation. The treatment steps are: after adopting the same aluminum alloy pretreatment as in Example 1, directly adopt the same coating curing steps as in Example 1, wherein the preparation of the modified composite particles is also the same as in Example 1.

[0076] Hydrophobic and oleophobic properties:

[0077] The hydrophobic and oleophobic properties of the coating are evaluated by the water contact angle, water rolling angle, oil contact angle and oil rolling angle. The higher the water contact angle, the better the hydrophobic property, that is, the material surface has a low affinity for water and is non-wettable. The higher the oil contact angle, the better the oleophobic property, that is, the material surface has a low affinity for oil and is non-wettable. Rolling angle: When the angle of the inclined plane increases to a certain extent, the droplets will roll on the surface without sticking to the surface. This angle is the rolling angle. Therefore, the smaller the rolling angle, the better the hydrophobic and oleophobic properties.

[0078] The hydrophobic and oleophobic properties of the untreated aluminum alloy, the aluminum alloy treated with micro-arc oxidation, the coating not treated with micro-arc oxidation, and the super-amphiphobic anticorrosive and antibacterial multifunctional aluminum alloy coating prepared by the present invention are shown in Table 1. The test water is deionized water, and the test oil is n-hexadecane. As can be seen from Table 1, compared with the coating not treated with micro-arc oxidation, the micro-arc oxidation treatment is added before spray curing in Examples 1 to 5, and the oleophobic and hydrophobic properties of the prepared coating are greatly improved, and the water contact angle and the oil contact angle are not less than 150°, indicating that the prepared coating has the characteristics of super-amphiphobic.

[0079] Table 1 Hydrophobic and oleophobic properties

[0080]

[0081] Anti-corrosion properties:

[0082] Through the electrochemical corrosion test, the dynamic potential polarization curve of the material is obtained, and the self-corrosion current density of the material is obtained after fitting the dynamic potential polarization curve. The smaller the self-corrosion current density, the better the anti-corrosion performance of the material. The self-corrosion current density detection data is shown in Table 2. It can be seen from the table that, relative to the untreated aluminum alloy of Comparative Example 1, the self-corrosion current density of the aluminum alloy of Comparative Example 2 is reduced by 2 orders of magnitude after micro-arc oxidation treatment, and the self-corrosion current density of the aluminum alloy of Comparative Example 3 is reduced by 3 orders of magnitude after direct coating without micro-arc oxidation treatment. Compared with Comparative Example 2, the self-corrosion current density of the coating prepared in Examples 1 to 5 of the present invention is further reduced by 3 orders of magnitude, indicating that the aluminum alloy coating of the present invention has a very obvious improvement effect on the corrosion resistance of the aluminum alloy.

[0083] Table 2 Anticorrosion performance

[0084] sample <![CDATA[Self-corrosion current density (A·cm -2 )]]> Aluminum alloy of Comparative Example 1 <![CDATA[2.52×10 -6 ]]> Aluminum alloy of comparative example 2 <![CDATA[7.05×10 -8 <!-- 5 -->]]> Coating of Comparative Example 3 <![CDATA[9.05×10 -9 ]]> Coating of Example 1 <![CDATA[1.86×10 -11 ]]> Coating of Example 2 <![CDATA[1.98×10 -11 ]]> Coating of Example 3 <![CDATA[2.01×10 -11 ]]> Coating of Example 4 <![CDATA[1.89×10 -11 ]]> Coating of Example 5 <![CDATA[1.92×10 -11 ]]>

[0085] Antimicrobial properties:

[0086] Pseudomonas aeruginosa, a major bacterium in the ocean, was used as a strain, and untreated aluminum alloy was used as a blank control to evaluate the antibacterial properties of the coating, and the antibacterial rate is shown in Table 3. As can be seen from the table, the coating prepared without adding a bactericide (Example 5) has a certain antibacterial effect on Pseudomonas aeruginosa, but the coating prepared with the addition of a bactericide (Examples 1 to 4) has an antibacterial rate of more than 99% against Pseudomonas aeruginosa. Compared with the coating prepared without adding a bactericide in Example 5, the antibacterial properties of the coatings prepared with the addition of a bactericide in Examples 1 to 4 have been greatly improved, and have excellent antibacterial properties.

[0087] Table 3 Antibacterial properties

[0088] sample Antibacterial rate Untreated aluminum alloy / Coating of Example 1 99.58% Coating of Example 2 99.42% Coating of Example 3 99.67% Coating of Example 4 99.47% Coating of Example 5 69.25%

[0089] Acid and alkali resistance:

[0090] The coatings of Examples 1 to 5 were immersed in a solution of pH 1 to pH 14 for 1 hour, and then the contact angle and rolling angle tests were performed. The contact angles were all greater than 150°, and the rolling angles were all less than 10°. There was no obvious change on the coating surface, indicating that the prepared coatings have good acid and alkali resistance.

[0091] Heat resistance:

[0092] The coatings of Examples 1 to 5 were placed in a drying oven at 80°C and heated for 2 hours, and then the contact angle and rolling angle tests were performed. The contact angles were all greater than 150°, and the rolling angles were all less than 10°. There was no obvious change on the coating surface, indicating that the prepared coatings have good heat resistance.

[0093] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a super-amphiphobic anticorrosive and antibacterial aluminum alloy coating, characterized in that: The following steps are involved: (1) Clean the aluminum alloy surface after grinding; (2) performing micro-arc oxidation treatment on the aluminum alloy treated in step (1), and washing and drying after the reaction is completed; The micro-arc oxidation electrolyte contains: 12-16 g / L sodium silicate, 1.0-1.5 g / L KOH and 0.8-1.2 g / L disodium ethylenediaminetetraacetate; The parameters of micro-arc oxidation treatment are: duty cycle 10% to 80%, frequency 100 to 400 Hz, current density 6 to 30 A / dm 2 , oxidation time 10~60min; (3) spraying the super-amphiphobic cured coating onto the surface of the aluminum alloy treated in step (2), and obtaining a super-amphiphobic cured coating after curing; The super-amphiphobic curing coating comprises modified metal oxide nanoparticles, epoxy resin and curing agent; the metal oxide nanoparticles comprise TiO2 nanoparticles; The preparation process of the modified metal oxide nanoparticles comprises the following steps: (3-1) adding perfluorosilane and tetraethyl orthosilicate into anhydrous ethanol and stirring to obtain a solution; (3-2) adding metal oxide nanoparticles to the solution obtained in step (3-1), and continuing stirring to form an emulsion suspension; (3-3) Adding an inducing agent to the emulsion suspension obtained in step (3-2) to form a coating layer on the surface of the metal oxide nanoparticles, thereby obtaining a dispersion containing modified metal oxide nanoparticles.

2. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 1, characterized in that: The metal oxide nanoparticles also include a bactericide; the bactericide is at least one of ZnO nanoparticles or CuO nanoparticles.

3. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 2, characterized in that: The mass percentage of TiO2 nanoparticles in the metal oxide nanoparticles is 83% to 90%.

4. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 3, characterized in that: The ratio of the sum of the mass of the epoxy resin and the curing agent to the mass of the modified metal oxide nanoparticles is 0.1 to 0.8:

1.

5. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 1, characterized in that: The perfluorosilane is 1H,1H,2H,2H-perfluorodecyltriethoxysilane.

6. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 5, characterized in that: The mass ratio of the perfluorosilane, tetraethyl orthosilicate and metal oxide nanoparticles is: (5-7): (2-4): (3-5).

7. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 1, characterized in that: The inducer is ammonia water or sodium methyl silicate; the mass ratio of the inducer to tetraethyl orthosilicate is 0.2-2:

1.

8. The method for preparing the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 1, characterized in that: The preparation process of the super amphiphobic cured coating is as follows: Add epoxy resin and curing agent to the dispersion containing metal oxide nanoparticles obtained in step (3-3), stir for 1.5 to 2.5 hours to obtain a mixed suspension; spray the mixed suspension onto the surface of the aluminum alloy after micro-arc oxidation, and cure at 60 to 150°C.

9. A super-amphiphobic anti-corrosion and antibacterial aluminum alloy coating, characterized in that: It includes a micro-arc oxidation layer located on the surface of the aluminum alloy and a super-amphiphobic cured coating located on the surface of the micro-arc oxidation layer; The micro-arc oxidation layer is a film layer formed by micro-arc oxidation treatment using a micro-arc oxidation electrolyte; the micro-arc oxidation electrolyte contains: 12-16 g / L sodium silicate, 1.0-1.5 g / L KOH and 0.8-1.2 g / L disodium ethylenediaminetetraacetate; The super-amphiphobic cured coating is a film layer formed by spraying the super-amphiphobic cured coating onto the surface of the micro-arc oxidation layer and curing; the super-amphiphobic cured coating includes modified metal oxide nanoparticles, epoxy resin and curing agent; the modified metal oxide nanoparticles are metal oxide nanoparticles coated with a silicon film on the surface; the silicon film surface contains hydroxyl groups and perfluorosilane grafting; the metal oxide nanoparticles include TiO2 nanoparticles.

10. The use of the super-amphiphobic anticorrosive and antibacterial aluminum alloy coating according to claim 9, characterized in that: For corrosion and antifouling of aluminum alloys used in marine environments.