Method for controlling low-glossiness stability of surface of cold-rolled 5052 aluminum alloy strip
Through cold rolling production process and electric spark blistering treatment, the problem of unstable gloss on the surface of aluminum alloy strips is solved, the uniformity and stability of gloss is achieved, and the safety and environmental risks in production are reduced. An environmentally friendly and reliable control method.
Patent Information
- Application Number
- CN202411141601.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The prior art has difficulties in water treatment, safety and environmental risks of chemical agents, and production problems caused by gloss in the low gloss control of aluminum alloy strips, which affect welding and QR code identification.
The cold rolling production process is adopted, including cold rolling on the billet, intermediate annealing, cold rolling of finished products, degreasing agent cleaning, annealing and edge cutting. Through multi-pass rolling and electric spark blistering treatment, the surface roughness and gloss of the rolling rolls are controlled. , use environmentally friendly light white oil and alcohol additives to ensure that the rolling oil is tempered and oil pressure is within the appropriate range.
It effectively reduces the yield loss, improves the stability and uniformity of the surface gloss of the strip, reduces the surface gloss of the aluminum alloy, and provides an environmentally friendly, reliable, simple and easy to promote control method.
Smart Images

Figure CN118904920A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for controlling the low gloss stability of a cold-rolled 5052 aluminum alloy strip surface. Background Art
[0002] At present, the company's products are widely used in electronic products, such as Huawei mobile phone shells, Apple mobile phone shells, laptop computer shells, mobile phone mid-plates and other products. The color difference value B value is required to be ≤3.5, the glossiness of the upper and lower surfaces at 20° is required to be 60-180GU, and the surface roughness Ra≤0.6μm; its glossiness requirement mainly affects the positioning needs of the laser light source for welding after the downstream stamping and forming of electronic products. High glossiness reduces the positioning accuracy and makes it difficult to scan and recognize two-dimensional codes. The surface of the aluminum plate needs to obtain a glossiness of 60-200GU at 20° on the upper and lower surfaces in the longitudinal direction. At present, in order to obtain low-gloss products at home and abroad, strong acids or strong alkalis are generally added during cleaning to etch the surface of the strip, and chemical treatment is used. In industrial applications, it is difficult to treat water, and the chemical agents are highly corrosive, which poses certain safety and environmental risks to people and equipment. Therefore, the current strong alkali and strong acid chemicals for cleaning have been gradually replaced by neutral degreasing agents. When the etching is severe, the surface layer tissue is corroded and color differences and surface defects are easily produced.
[0003] In order to solve the above technical problems, the present invention proposes a method for controlling the low gloss stability of the surface of cold-rolled 5052 aluminum alloy strip, aiming to overcome the existing production process difficulties and provide an environmentally friendly, reliable, simple and easy-to-promote cold rolling control method. Summary of the invention
[0004] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for controlling the low gloss stability of the surface of a cold-rolled 5052 aluminum alloy strip.
[0005] In order to solve the above technical problems, the technical solution of the present invention is: a method for controlling the low gloss stability of the surface of a cold-rolled 5052 aluminum alloy strip, wherein the cold rolling production process is sequentially blanking cold rolling, intermediate annealing, finished product cold rolling, degreasing agent cleaning, finished product annealing, finished product trimming, and packaging; Cold rolling mills are used for cold rolling of slabs and finished products. The roll diameter range of cold rolling is 400-440mm, and the roll type is flat roll; the rolling oil temperature is 30±5℃, the rolling oil flow rate is 2500-3500L / min, and the rolling oil pressure is 8~10bar, among which: The slab is cold rolled through multiple passes to the intermediate annealing pass thickness, and the transverse roughness Ra of the first roller surface used in the rolling is 0.8~1.0μm; The total processing rate after intermediate annealing is 20-25%, and the finished product is cold rolled in two passes, with the inlet strip temperature controlled at ≤45°C: The first pass processing rate is 5%~7%, and the second roller is rolled by EDM texturing, and the transverse roughness of the second roller surface is Ra: 2.75~3.05μm; The second pass processing rate is 10%~20%, and the third roller with a surface lateral roughness Ra: 0.35~0.45μm is used.
[0006] Preferably, the grinding process parameters of the first rolling roller are: using a grinder, the grinding machine cutting fluid uses a mixture of coolant and water, the required concentration is: 3~6%, and the pH value is 8~10; the grinding wheel uses 60 mesh and the grinding wheel hardness is F grade, so that the lateral roughness of the surface of the first rolling roller is Ra: 0.8~1.0μm, and there is no visible color difference or scratch defects on the surface after grinding.
[0007] Preferably, the grinding process parameters of the second rolling roller are: using a 12-electrode electric spark texturing machine for surface treatment; using a grinding wheel type original roller with a roughness Ra≤0.2μm, and roughening after grinding; using a roughness meter to detect, so that the lateral roughness of the second rolling roller surface Ra: 2.75~3.05μm.
[0008] Preferably, the cold rolling mill is produced using a six-roll 1850mm cold rolling mill.
[0009] Preferably, the cold rolling mill uses light white oil 100# base oil, the additive is an alcohol additive, and the weight ratio of the alcohol additive to the base oil is 8.5-9.5%; 5052 aluminum alloy is used for production, and the mass fraction of chemical components is: Si: 0.06-0.2%; Fe: 0.2-0.4%; Cu: 0.01-0.05%; Mn: 0.01-0.05%; Mg: 2.4-2.8%; Ti: 0.014-0.02%; the hot-rolled billet thickness is 2.5~5.1mm, and the final rolling temperature is 310~330℃.
[0010] Preferably, the blank is cold rolled through 3 to 5 passes to the intermediate annealing pass thickness.
[0011] Preferably, the grinding process parameters of the third rolling roller are: using a grinder, the cutting fluid uses a mixture of coolant and water, the required concentration is 3-6%, and the pH value is 8-10; the grinding wheel uses 100 mesh and the grinding wheel hardness is F grade; the lateral roughness of the surface of the third rolling roller is Ra: 0.35-0.45μm, and there is no visible color difference or scratch defects on the surface after grinding.
[0012] Compared with the prior art, the present invention has the following beneficial effects: The rolling control method of the present invention can effectively reduce the loss of finished product rate; solve the scrap loss caused by unqualified glossiness due to production operation and rolling conditions; the method can also improve the color uniformity of the strip surface, effectively reduce the glossiness of the aluminum alloy surface and improve the glossiness stability during the production process. It is an environmentally friendly, reliable, simple and easy to promote control method.
[0013] The present invention is further described in detail below in conjunction with specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a schematic diagram of the changes in the speed-up length and glossiness during the ordinary roll-up rolling process in Scheme 2.
[0015] Figure 2 It is a schematic diagram of the change of the speed-up length and the glossiness during the rolling process in an embodiment of the present invention. DETAILED DESCRIPTION
[0016] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0017] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0018] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0019] This embodiment provides a method for controlling the low gloss stability of a cold-rolled 5052 aluminum alloy strip surface, wherein the cold rolling production process is sequentially blanking cold rolling, intermediate annealing, finished product cold rolling (the total processing rate after intermediate annealing is controlled at 20-25%), degreasing agent cleaning (conductivity 18-22ms / cm), finished product annealing, finished product trimming, and packaging; Cold rolling mills are used for cold rolling of slabs and finished products. The roller diameter range of cold rolling is 400-440mm, and the roller type is flat roller. The rolling oil temperature is 30±5℃, the rolling oil flow rate is 2500-3500L / min, the rolling oil pressure is 8~10bar, and the finished product thickness range is: 0.2~0.5mm, including: The slab is cold rolled through multiple passes to the intermediate annealing pass thickness, and the transverse roughness Ra of the first roller surface used in the rolling is 0.8~1.0μm; The total processing rate after intermediate annealing is 20-25%, and the finished product is cold rolled in two passes, with the inlet strip temperature controlled at ≤45°C: The first pass processing rate is 5%~7%, and the second roller treated with electric spark roughening is used for rolling. The transverse roughness of the second roller surface Ra is 2.75~3.05μm, and the strip surface roughness Ra is 0.9-1.3μm; The processing rate of the second pass (final rolling thickness pass) is 10%~20%. The third roller with a surface transverse roughness Ra: 0.35~0.45μm is used to obtain a qualified strip surface with a surface roughness Ra≤0.6μm, uniform surface roughness and low gloss.
[0020] In the embodiment of the present invention, the grinding process parameters of the first rolling roller are as follows: a German Waldrich grinder is used, and the grinding fluid is a mixture of Castrol syntilo66 coolant and water, with the required concentration of 3-6% and a pH value of 8-10; an Atlantic brand 60-mesh grinding wheel is used for grinding, and the grinding wheel hardness is grade F, so that the lateral roughness of the surface of the first rolling roller Ra is 0.8-1.0 μm, and there is no visible color difference or scratch defect on the surface after grinding.
[0021] The larger the grinding wheel particle size or the higher the roughness, the deeper and wider the cutting texture. Therefore, a 60-mesh grinding wheel is used to grind the required roller surface roughness Ra: 0.8~1.0μm for the first roller; thereby ensuring the depth of the roller cutting texture. As the number of rolling passes increases and the material hardening increases, the oil pits on the strip surface continue to decrease. The use of a 60-mesh grinding wheel to grind the first roller makes the strip surface cutting texture obvious, which can effectively slow down the increase in glossiness. Using the grinding process in Table 1, the transverse roughness of the first roller surface is Ra: 0.8~1.0μm, and there are no visible color differences, scratches and other defects on the surface after grinding.
[0022] Table 1 Grinding process parameters of the first roll In the embodiment of the present invention, the grinding process parameters of the second rolling roller are as follows: using a British Sarclad 12 electrode electric spark texturing machine tool for surface treatment (i.e., EDT: Electro-Disharge Textured); using a grinding wheel type original roller with a roughness of Ra≤0.2μm, and roughening according to the process in Table 2 after grinding; using a German Taylor Hobson Surtronic S128 roughness meter for testing, so that the lateral roughness of the second rolling roller surface Ra: 2.75~3.05μm.
[0023] Table 2 Deburring process parameters The principle of roller EDM texturing is: by applying high voltage between the electrode and the roller to form a conductive spark, the heat generated by the spark will melt the electrode and the roller surface, and form bubbles in the insulating oil. When the power is turned off, the bubbles burst and leave a pit on the roller surface. Through pulse discharge, the operation is repeated millions of times to form a controllable roller surface roughness and peak value. Through millions of physical and chemical reactions, a truly disordered EDM surface is formed; the EDM texturing surface conducts the surface morphology during the rolling of the rolling mill. EDM texturing can obtain a completely disordered strip surface with good repeatability. After EDM texturing, pits are generated on the strip surface, which can quickly reduce the glossiness of the strip surface and obtain a surface with uniform roughness.
[0024] In the embodiment of the present invention, the cold rolling mill is produced by a six-roll 1850mm cold rolling mill.
[0025] In an embodiment of the present invention, the cold rolling mill adopts light white oil 100# base oil, and the additive is an alcohol additive, and the weight ratio of the alcohol additive to the base oil is 8.5-9.5%; 5052 aluminum alloy is used for production, and the mass fraction of chemical components is %: Si: 0.06-0.2%; Fe: 0.2-0.4%; Cu: 0.01-0.05%; Mn: 0.01-0.05%; Mg: 2.4-2.8%; Ti: 0.014-0.02%; the hot-rolled billet thickness is 2.5~5.1mm, and the final rolling temperature is 310~330℃.
[0026] In the embodiment of the present invention, the blank is cold rolled through 3 to 5 passes to the intermediate annealing pass thickness.
[0027] In the embodiment of the present invention, in order to ensure that the surface quality of the product is improved and the cutting marks are improved to avoid pits or color differences in the finished product due to too deep cutting marks, the grinding process parameters of the third roller are as follows: a German Waldrich grinder is used, and the cutting fluid uses a mixture of Castrol syntilo66 coolant and water, with the required concentration of 3~6%, and a pH value of 8~10; the grinding wheel uses an Atlantic brand 100-mesh grinding wheel for grinding, and the grinding wheel hardness is grade F; the grinding process in Table 3 is used to make the lateral roughness of the third roller surface Ra: 0.35~0.45μm, and there are no visible color differences, scratches and other defects on the surface after grinding.
[0028] Table 3. Grinding process parameters of the third roll In the embodiments of the present invention, in order to better illustrate the creativity of the present invention, the comparative scheme is listed as follows: Since the customer did not require glossiness at first, we used Scheme 1 for production. Scheme 1 was produced using ordinary rollers, and the glossiness of the strip surface fluctuated significantly and had poor stability.
[0029] Customers' requirements for glossiness gradually increase to 60-200GU, and some customers require ≤180GU; therefore, Scheme 2 is used for production. Scheme 2 reduces fluctuations by improving roughness, grinding wheel model and process parameters, and improves the glossiness of the strip surface; at the same time, ordinary grinding wheel production is affected by rolling lubrication conditions, which affects both rolling speed and lubrication conditions. Scheme 2 shows the schematic diagram of the speed increase length and glossiness change during ordinary roller lifting rolling. Figure 1 shown.
[0030] Scheme 3 adopts the patented control method to control the surface roughness of the strip, improve the stability of the surface gloss of the strip, and use EDT rolling to obtain low gloss; After production in Scheme 3, the schematic diagram of the change in speed increase length and gloss during the rolling process is as follows Figure 2 shown.
[0031] The glossiness of the rolling surface of the roller ground by ordinary grinding wheels is greatly affected by the rolling lubrication state. The surface glossiness of the strip rolled by the patented control method can obtain a more stable product with glossiness requirements by controlling the roughness of the EDT roller and the roughness of the finished pass roller.
[0032] The cold rolling mill's rolling acceleration and deceleration length generally reaches 500-1000 meters and the rolling speed is controlled at ≥700m / min, which has very strict requirements on production operation and rolling conditions; the acceleration and deceleration section loss is ≥1000 meters per roll; therefore, this patented rolling control method can effectively reduce the loss of finished product rate; solve the scrap loss caused by unqualified gloss due to production operation and rolling conditions; this method can also improve the uniformity of strip surface color, effectively reduce the surface gloss of aluminum alloy and improve the gloss stability during production. It is an environmentally friendly, reliable, simple and easy to promote control method.
[0033] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A method for controlling the low gloss stability of a cold-rolled 5052 aluminum alloy strip surface, wherein the cold rolling production process is followed in sequence: blank cold rolling, intermediate annealing, finished product cold rolling, degreasing agent cleaning, finished product annealing, finished product trimming, and packaging. Features: Cold rolling mills are used for cold rolling of slabs and finished products. The roll diameter range of cold rolling is 400-440mm, and the roll type is flat roll; the rolling oil temperature is 30±5℃, the rolling oil flow rate is 2500-3500L / min, and the rolling oil pressure is 8~10bar, among which: The slab is cold rolled through multiple passes to the intermediate annealing pass thickness, and the transverse roughness Ra of the first roller surface used in the rolling is 0.8~1.0μm; The total processing rate after intermediate annealing is 20-25%, and the finished product is cold rolled in two passes, with the inlet strip temperature controlled at ≤45°C: The first pass processing rate is 5%~7%, and the second roller is rolled by EDM texturing, and the transverse roughness of the second roller surface is Ra: 2.75~3.05μm; The second pass processing rate is 10%~20%, and the third roller with a surface lateral roughness Ra: 0.35~0.45μm is used.
2. The method for controlling the low gloss stability of the surface of the cold-rolled 5052 aluminum alloy strip according to claim 1, Features: The grinding process parameters of the first rolling roller are as follows: a grinder is used, and the cutting fluid of the grinder uses a mixture of coolant and water, with the required concentration of 3-6% and a pH value of 8-10; a 60-mesh grinding wheel with a grinding wheel hardness of grade F is used, so that the lateral roughness of the surface of the first rolling roller Ra is 0.8-1.0 μm, and there is no visible color difference or scratch defect on the surface after grinding.
3. The method for controlling the low gloss stability of the cold-rolled 5052 aluminum alloy strip surface according to claim 1, Features: The grinding process parameters of the second roller are as follows: using a 12-electrode electric spark texturing machine for surface treatment; using a grinding wheel type original roller with a roughness of Ra≤0.2μm, and roughening after grinding; using a roughness meter to detect, so that the lateral roughness of the second roller surface Ra: 2.75~3.05μm.
4. The method for controlling the low gloss stability of the surface of the cold-rolled 5052 aluminum alloy strip according to claim 1, Features: The cold rolling mill is produced by a six-roller 1850mm cold rolling mill.
5. The method for controlling the low gloss stability of the cold-rolled 5052 aluminum alloy strip surface according to claim 1, Features: The cold rolling mill uses light white oil 100# base oil, and the additive is an alcohol additive, and the weight ratio of the alcohol additive to the base oil is 8.5-9.5%; it is produced using 5052 aluminum alloy, and the mass fraction of chemical components is %: Si: 0.06-0.2%; Fe: 0.2-0.4%; Cu: 0.01-0.05%; Mn: 0.01-0.05%; Mg :2.4-2.8%; Ti: 0.014-0.02%; hot rolled billet thickness 2.5~5.1mm, final rolling temperature 310~330℃.
6. The method for controlling the low gloss stability of the cold-rolled 5052 aluminum alloy strip surface according to claim 1, Features: The slab is cold rolled through 3 to 5 passes to the intermediate annealing pass thickness.
7. The method for controlling the low gloss stability of the cold-rolled 5052 aluminum alloy strip surface according to claim 1, Features: The grinding process parameters of the third rolling roller are as follows: a grinding machine is used, a mixture of coolant and water is used as the cutting fluid, the required concentration is 3-6%, and the pH value is 8-10; a 100-mesh grinding wheel is used, and the grinding wheel hardness is grade F; the lateral roughness Ra of the surface of the third rolling roller is 0.35-0.45 μm, and there is no visible color difference or scratch defect on the surface after grinding.
Citation Information
Patent Citations
Stabilizing processing method of 5052 aluminium alloy
CN101935786A
Formulating method for 5052 aluminum alloy strip cold rolling process
CN104128371A
Preparation process of 5754 aluminum alloy plate with high formability
CN112553485A
Mirror surface aluminum plate strip with low surface roughness and preparation method thereof
CN117427999A
Manufacture of pure al plate for name plate
JP1982051246A