Extrusion process for 6110A aluminum alloy automobile anti-collision beam
By homogenizing, cooling, heating and extruding and aging the 6110A aluminum alloy casting rod, the problem of 6110A aluminum alloy automobile anti-collision beam processing in the prior art is solved, and extrusion with high strength and good bending resistance is achieved The process significantly enhances the value of aluminum alloy in automotive applications.
Patent Information
- Application Number
- CN202411111075.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the extrusion process of 6110A aluminum alloy automobile anti-collision beam is still in its infancy, and there is a lack of effective processing methods to meet the requirements of high strength and good bending resistance.
By homogenizing, cooling, heating and extruding molding and aging treatment on the 6110A aluminum alloy casting rod, a high-strength aluminum alloy car anti-collision beam is prepared. The specific steps include homogenizing the casting rod and heating it after cooling. And extrusion molding is carried out, and then aging is carried out.
A high-strength extruded 6110A aluminum alloy automobile anti-collision beam was successfully prepared, and the three-point bending test showed good bending resistance, meeting the application needs of automobile products.
Smart Images

Figure CN118904956A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal structural material processing, and particularly relates to an extrusion process for a 6110A aluminum alloy automotive anti-collision beam. Background Art
[0002] The application of aluminum alloys in automobiles has received increasing attention. Many automotive components are produced from aluminum alloys, especially the 6000 series, because they possess excellent properties such as excellent corrosion resistance, reflectivity, high strength and stiffness-to-weight ratio, good formability, weldability, and recycling potential. The high-strength aluminum alloys of the 6000 series are developed by adding copper elements, such as AA6110, AA6111, or AA6013, etc., and are widely used in the automotive industry.
[0003] Extrusion refers to a pressure processing method in which pressure is applied to one end of an ingot blank placed in an extrusion cylinder, causing it to pass through an extrusion die to achieve plastic deformation. Compared with forging and rolling processes, extrusion has a more intense three-dimensional compressive stress state than forging and rolling, and metals can exhibit their maximum plasticity; the extrusion process has great flexibility and is easy to operate; the product has high dimensional accuracy and good surface quality. Currently, the research on the extrusion process of 6110A aluminum alloy is still in its infancy.
[0004] Therefore, there is an urgent need to propose an extrusion process for a 6110A aluminum alloy automotive anti-collision beam to meet the needs of research and use. Summary of the Invention
[0005] The purpose of the present invention is to provide an extrusion process for a 6110A aluminum alloy automotive anti-collision beam to solve the problems existing in the above-mentioned prior art.
[0006] To achieve the above purpose, the present invention provides an extrusion process for a 6110A aluminum alloy automotive anti-collision beam, including the following steps:
[0007] Homogenize the 6110A aluminum alloy ingot.
[0008] Cool the homogenized 6110A aluminum alloy ingot.
[0009] Reheat the cooled 6110A aluminum alloy ingot and perform extrusion molding to obtain a 6110A aluminum alloy automotive anti-collision beam.
[0010] Perform aging treatment on the 6110A aluminum alloy automotive anti-collision beam.
[0011] Preferably, the diameter of the 6110A aluminum alloy ingot is 178 mm.
[0012] Preferably, the cross-sectional shape of the 6110A aluminum alloy automotive anti-collision beam is a "day" - shaped structure.
[0013] Preferably, the homogenization treatment temperature is 580° C. and the temperature is kept for 10 hours.
[0014] Preferably, the reheating temperature of the 6110A aluminum alloy cast rod is 540°C.
[0015] Preferably, during the extrusion molding, the extrusion speed of the extrusion rod is 0.8 mm / s.
[0016] Preferably, the cooling method for cooling the 6110A aluminum alloy cast rod after homogenization treatment is water spray cooling.
[0017] Preferably, the aging treatment is carried out at a temperature of 175° C. for 12 hours.
[0018] Compared with the prior art, the present invention has the following advantages and technical effects:
[0019] By using the 6110A aluminum alloy automobile anti-collision beam extrusion process provided by the present invention, a high-strength extruded 6110A aluminum alloy automobile anti-collision beam can be successfully produced, and after a three-point bending test, it shows good anti-bending performance, which is of great value for the application of the alloy in automobile products. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 The macrostructure of the cross section of the extruded profile in Comparative Example 1 of the present invention;
[0022] Figure 2 The three-point bending result of the extruded profile in Comparative Example 1 of the present invention;
[0023] Figure 3 The macrostructure of the cross section of the extruded profile in Example 1 of the present invention;
[0024] Figure 4 This is the three-point bending result of the extruded profile in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The described embodiments are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The present invention will be described in detail below with reference to the drawings and in combination with the embodiments.
[0026] The present invention provides a 6110A aluminum alloy automobile anti-collision beam extrusion process, comprising the following steps:
[0027] Homogenization treatment of 6110A aluminum alloy casting rod;
[0028] Cooling the homogenized 6110A aluminum alloy casting rod;
[0029] The cooled 6110A aluminum alloy casting rod is reheated and extruded to obtain a 6110A aluminum alloy automobile anti-collision beam;
[0030] Aging treatment of 6110A aluminum alloy automotive anti-collision beam.
[0031] After further optimization, the diameter of the 6110A aluminum alloy casting rod is 178 mm.
[0032] According to the further optimization plan, the cross-sectional shape of the 6110A aluminum alloy automobile anti-collision beam is a "sun" shaped structure.
[0033] The scheme was further optimized, and the homogenization temperature was 580°C and kept warm for 10 hours.
[0034] The solution was further optimized, and the reheating temperature of the 6110A aluminum alloy casting was 540°C.
[0035] The scheme is further optimized, and during extrusion molding, the extrusion speed of the extrusion rod is 0.8 mm / s.
[0036] The scheme is further optimized, and the cooling method for cooling the 6110A aluminum alloy cast rods after homogenization is water spray cooling.
[0037] The scheme was further optimized, with the aging treatment temperature at 175°C and insulation for 12 hours.
[0038] Comparative Example 1
[0039] The composition of the 6110A aluminum alloy casting rod used is as follows: Mg1.05%, Si0.93%, Cu0.75%, Mn0.33%, and Al is the balance. The diameter of the casting rod used is 178mm. The casting rod is heated to 580℃ and kept warm for 10 hours for homogenization. The homogenized casting rod is sawn into short rods with a length of 500mm for heating. The heating temperature is set to 520℃, the mold heating temperature is 510℃, and the extrusion barrel temperature is 510℃. The extrusion rod speed is set to 1.3mm / s, and the cooling method is water cooling. The cooled extruded profile is placed in an aging furnace, heated to 175℃, and kept warm for 12 hours. The aged sample is subjected to a three-point bending test, which is carried out on a universal testing machine with a compression stroke of 150mm.
[0040] In the anti-collision beam produced by the above extrusion process, in the macrostructure of the cross-section of the extruded profile, the center of the thin wall of the profile is fibrous crystal, and the edge is coarse recrystallized grains, such as Figure 1 In addition, in the three-point bending test, obvious cracks appeared on the edge of the profile, which could not meet the requirements of automotive parts. Figure 2 shown.
[0041] Example 1
[0042] The 6110A aluminum alloy automobile anti-collision beam extrusion process provided by the present invention is used. The composition of the 6110A aluminum alloy cast rod used is as follows: Mg1.05%, Si0.93%, Cu0.75%, Mn0.33%, and Al is the balance by weight content percentage. The diameter of the cast rod used is 178mm, and the cast rod is heated to 580°C and kept warm for 10 hours for homogenization. The homogenized cast rod is sawn into a short rod with a length of 500mm for heating, and the heating temperature is set to 540°C, the mold heating temperature is 510°C, and the extrusion barrel temperature is 510°C. The extrusion rod speed is set to 0.8mm / s, and the cooling method is water cooling. The cooled extruded profile is placed in an aging furnace, heated to 175°C, and kept warm for 12 hours. The sample after aging treatment is subjected to a three-point bending test, which is carried out on a universal testing machine with a compression stroke of 150mm.
[0043] The anti-collision beam manufactured by the extrusion process provided by the present invention has no obvious coarse recrystallized structure in the low-magnification structure section of the extruded profile, such as Figure 3 In addition, it performs well in the three-point bending test without any cracks. Figure 4 shown.
[0044] By using the 6110A aluminum alloy automobile anti-collision beam extrusion process provided by the present invention, a high-strength extruded 6110A aluminum alloy automobile anti-collision beam can be successfully produced, and after a three-point bending test, it shows good anti-bending performance, which is of great value for the application of the alloy in automobile products.
[0045] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be covered within the protection scope of the present application.
Claims
1. A 6110A aluminum alloy automobile anti-collision beam extrusion process, characterized in that: It includes the following steps: Homogenize the 6110A aluminum alloy casting rod; Cool the homogenized 6110A aluminum alloy casting rod; Reheat the cooled 6110A aluminum alloy casting rod and perform extrusion molding to obtain a 6110A aluminum alloy automotive anti-collision beam; Perform aging treatment on the 6110A aluminum alloy automotive anti-collision beam.
2. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: The diameter of the 6110A aluminum alloy casting rod is 178 mm.
3. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: The cross-sectional shape of the 6110A aluminum alloy automotive anti-collision beam is a "day" shaped structure.
4. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: The temperature of the homogenization treatment is 580 °C, and the holding time is 10 h.
5. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: The temperature for reheating the 6110A aluminum alloy casting rod is 540 °C.
6. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: During the extrusion molding, the extrusion speed of the extrusion rod is 0.8 mm / s.
7. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: The cooling method for cooling the homogenized 6110A aluminum alloy casting rod is spray cooling.
8. The 6110A aluminum alloy automobile anti-collision beam extrusion process according to claim 1 is characterized in that: The temperature of the aging treatment is 175 °C, and the holding time is 12 h.
Citation Information
Patent Citations
Extrusion process of 6063 aluminum alloy sections
CN107983792A
Production process of aluminum alloy anti-collision cross beam with high strength and high plasticity
CN112359254A
Preparation method of 6-series aluminum alloy for automobile anti-collision beam
CN117144163A
High-strength aluminum alloy and preparation method thereof
CN117867341A