Design method of large complex three-dimensional multi-parting-surface forge piece
By increasing the number of parting surfaces and using upsetting technology, the problem of large die forging presses being unable to provide horizontal forming force was solved, enabling efficient forming of complex three-dimensional forgings, reducing production costs and improving forging performance.
Patent Information
- Application Number
- CN202411150883.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
In the existing technology, large die forging presses with a capacity of 40,000 tons or more can only provide forming force in the vertical direction and cannot provide forming force in the horizontal direction at the same time. This results in limitations on the geometric design of large aerospace parts, especially when there are features such as high rims, branches, and ribs perpendicular to the parting surface. The forming difficulty is high, and the integrated design leads to a larger outer dimension of the forging and serious material waste.
By increasing the number of parting surfaces, designing vertically intersecting parting surfaces, and using upsetting to replace reverse extrusion forming, combined with draft angle design and transition fillet treatment, forging is carried out using a unidirectional large die forging press. The parting surface is designed to be multiple, reducing the thickness of the large cross-section and improving the feasibility of the forging process.
It enables the forming of complex three-dimensional multi-part forgings on existing equipment, reducing production costs, improving equipment utilization efficiency, avoiding material waste, and enhancing the structural strength and fatigue life of forgings.
Smart Images

Figure CN118905121A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of die forging, in particular to a design method for a large complex three-dimensional multi-partition die surface forging. Background Art
[0002] As the security situation around the country becomes increasingly severe, aviation equipment is accelerating its upgrading and replacement, and the demand for faster, lighter, longer-range, more reliable and longer-life aircraft is becoming increasingly strong. In order to meet the needs of iterative upgrades of aircraft, it is inevitable to comprehensively optimize the design of the aircraft's internal structure, part shape, etc. Due to the development and progress of basic theory, numerical simulation, and emerging technologies, the design ideas of aircraft structural designers are no longer limited to the conventional structures of the past. Through continuous innovation and transformation, some new complex structures have been designed, which solve the problems of only being able to rely on 3D printing manufacturing and insufficient fatigue life of 3D parts, and are more suitable for the optimization of aircraft force transmission and structure; through continuous innovation and transformation, some new complex structures have been designed, which are more suitable for the optimization of aircraft force transmission and structure. Large integral structural parts have force transmission continuity, which can improve structural strength, stiffness and fatigue life, while avoiding deformation caused by post-processing of welds and shortening the part manufacturing cycle. Due to the removal of a large number of fasteners such as rivets and screws, the weight reduction effect of large integral structural parts is obvious, and the number of aircraft parts assembly and tooling requirements are reduced, the interchangeability problem is simplified, and the assembly difficulty is greatly reduced.
[0003] Now that a novel design scheme for large integral parts has been proposed, the issue of engineering implementation needs to be considered; at present, the movable crossbeam of large-scale die forging presses above 40,000 tons in China can only move up and down in the vertical direction, providing downward forming pressure to drive the metal to flow from the center to the surroundings. There is currently no large-scale multi-directional die forging press that can provide forming forces in both the horizontal and vertical directions, resulting in limited geometric design of large aviation parts, that is, there are obvious differences between the length, width, and thickness dimensions of the parts. Usually there is only one maximum projection surface, and the parting surface is unique; if the forging has features such as high bulges, branches, and ribs that are perpendicular to the parting surface, the metal flow can be guided by transition fillets, conformal parting, process dressings, etc., and reverse extrusion can also be used to form the parting surface without affecting the uniqueness of the parting surface. Generally speaking, if the aspect ratio of the ribs is greater than 3.5, the forging will be more difficult to form, and if the aspect ratio is greater than 5, it cannot be formed by reverse extrusion.
[0004] Integration will inevitably lead to larger outer dimensions of forgings. Not only does the forming tonnage far exceed 40,000 tons, but the size differences of some forgings in three dimensions gradually decrease, and the maximum projected cross-section does not exist. In traditional design ideas, if the size of the fillet and the process dressing are simply increased, not only will materials be wasted, but the performance of thick and large cross-sections will also be difficult to guarantee. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a design method for large complex three-dimensional multi-partition surface forgings, by increasing the number of parting surfaces, reducing the thick cross-section size of the forgings, and transforming the reverse extrusion forming into upsetting forming, thereby improving the feasibility of the forging process.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A design method for a large complex three-dimensional multi-partition surface forging comprises the following steps:
[0008] 1. Forging design
[0009] S1. Parting surface design: according to the shape of the forging, a parting surface 1 and a parting surface 2 are divided, and the parting surface 1 and the parting surface 2 intersect and are perpendicular to each other;
[0010] S2. Forging allowance design: According to the size of the forging parts, the single-side allowance of the forging is designed to be 5-30mm;
[0011] S3. Draft angle design: The vertical edges on the forgings are designed with the same small draft angle or the variable draft angle. The same small draft angle is designed to expand toward the root along the stepped arrangement, and the slope is designed to be 1-10°; the variable draft angle is designed to gradually increase from the rib top to the root, and the slope is designed to be 1-10°;
[0012] S4. Transition fillet design: The radius of the concave fillet on the forging is 0.5-3 times the height of the vertical edge, and the radius of the convex fillet is equal to the single-side allowance at that position;
[0013] 2. Molding process
[0014] K1. Blank making: First, put the forging material into the heating furnace for preheating, then put the preheated forging into the one-way fast forging machine for upsetting, gather the head metal, press the metal on both sides of the forging parting surface 1 through the head forming tool A, then take out the forging and return it to the furnace for heat preservation for 30 to 120 minutes, then press the metal on both sides of the forging parting surface 2 through the head forming tool B, and place it on a special material rack for cooling after forging to form a blank, and control the underpressure to 5-10mm;
[0015] K2, pre-forging: spray lubricant evenly on the surface of the blank, place the blank in a heating furnace for preheating, connect the pre-forging die to the press, spray lubricating medium in the pre-forging die cavity, then place the heated blank in the die cavity, and press the metal on both sides of the parting surface 1 through the pre-forging die;
[0016] K3. Final forging: Spray lubricant evenly on the surface of the blank, then place it in a heating furnace for preheating, connect the final forging die to the press, spray lubricating medium in the final forging die cavity, then place the heated blank in the die cavity, and press the metal on both sides of the parting surface 2 through the final forging die. After forming, cool it on a special cooling rack.
[0017] In step S1, the forging has a three-dimensional shape, with a cross-shaped structure when projected from the side and a sun-shaped structure when projected from the top. The forging is designed with a parting surface 1 and a parting surface 2 in two spatial dimensions.
[0018] In step S2, the size of the forging part is ≥1200×1200×1000 mm, and the projected area of the forging is greater than 1.2 m2.
[0019] In step S3, the same small draft angle is a gradient draft with at least two steps, and the height difference between the steps is evenly divided; the variable draft angle is at least two slopes, and the bevel edge connection points are equally divided according to the width.
[0020] The beneficial effects of the present invention are:
[0021] 1. The use of unidirectional large-scale die forging presses to form multi-partition surface structural forgings provides a new idea, which can avoid enterprises from investing in new equipment such as multi-directional large-scale die forging presses again, reduce production costs, improve equipment utilization efficiency, and strongly support the production of new complex large-scale integral structural forgings, contributing to improving aircraft performance.
[0022] 2. By increasing the number of parting surfaces, reducing the size of the thick section of the forging, and transforming the reverse extrusion forming into upsetting forming, the feasibility of the forging process is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the dimensions of the forging;
[0024] Figure 2 The schematic diagram of the design of the parting surface;
[0025] Figure 3 It is a schematic diagram of the forging's allowance;
[0026] Figure 4 This is a schematic diagram of the design of the draft angle;
[0027] Figure 5 This is a schematic diagram of the design of the fillet of the forging;
[0028] Figure 6 It is a schematic diagram of metal forming on both sides of the parting surface 1;
[0029] Figure 7It is a schematic diagram of metal forming on both sides of the parting surface 2;
[0030] Figure 8 Cooling schematic diagram. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0032] Example 1
[0033] A design method for a large complex three-dimensional multi-partition surface forging comprises the following steps:
[0034] 1. Forging design (such as Figures 1 to 5 (shown)
[0035] S1. Parting surface design: Parting surface 1 and parting surface 2 are divided according to the shape of the forging. Parting surface 1 and parting surface 2 intersect and are perpendicular to each other. This type of forging has no maximum projection surface. The spatial dimensions of the forging are approximately 1200mm×1200mm×1000mm and above. The ratio of the projection area of the vertical length and width is close to 1. After finding two or more larger projection surfaces of the same area according to the shape characteristics of the part, the design principle to be followed is that one of the parting surfaces is perpendicular to the die base to ensure that the forging dressing is minimized.
[0036] S2. Forging allowance design: According to the size of forging parts, the single-side allowance of forgings is designed to be 5-30mm. The single-parting die web allowance can be selected as a smaller value, and the difficult-to-fill part can be selected as a larger value;
[0037] S3. Draft angle design: The vertical edges on the forgings are designed with the same small draft angle design or the variable draft angle design. The same small draft angle design is designed to expand toward the root along the stepped arrangement, and the slope is designed to be 1-10°; the variable draft angle design is designed to gradually increase from the rib top to the root, and the slope is designed to be 1-10°. Both the same small draft angle design and the variable draft angle design should ensure smooth transitions and reduce metal flow resistance. The gradient draft should be designed with at least two steps, and the height difference should be evenly divided. The variable draft should be designed with at least two slopes, and the bevel edge connection points should be equally divided according to the width;
[0038] S4. Transition fillet design: The radius of the concave fillet on the forging is 0.5-3 times the height of the vertical edge, and the radius of the convex fillet is equal to the single-side allowance at that position;
[0039] 2. Molding process (such as Figures 6 to 8 (shown)
[0040] K1. Billet making: The billet making process is completed on a one-way fast forging machine. First, the forging material is placed in a heating furnace for preheating (the preheating temperature of metals of different materials is different, and the preheating temperature of forgings made of titanium alloy is 800-985℃). Then the preheated forging is placed in a one-way fast forging machine for upsetting, and the head metal is gathered. The metal on both sides of the forging parting surface 1 is pressed by the head forming tool A, and then the forging is taken out and returned to the furnace for insulation for 30-120 minutes, and then the metal on both sides of the forging parting surface 2 is pressed by the head forming tool B. After forging, it is placed on a special material rack for cooling to form a blank. The underpressure is controlled to be 5-10mm. The specific forging times should be reasonably allocated according to the actual material requirements for deformation. Steel forgings have fewer times, and titanium alloy forgings can be carried out in multiple times. The tooling cavity needs to be sprayed with a lubricating medium. The blanking process is characterized by using a one-way fast forging machine and a blanking tooling to press the two parting surfaces of a forging, preliminarily distribute the metal, and use a special material rack for cooling to avoid deformation during the cooling process;
[0041] K2. Pre-forging: The pre-forging process is carried out on a large unidirectional die forging press. Lubricant (glass powder lubricant) is evenly sprayed on the surface of the blank. The blank is placed in a heating furnace for preheating (preheating temperature is 800-985°C). The pre-forging die is connected to the press, and the lubricating medium (graphite lubricant) is sprayed in the cavity of the pre-forging die. Then the heated blank is placed in the die cavity. The press presses the metal on both sides of the parting surface 1 through the pre-forging die. At this time, pay attention to control underpressure to prevent the forging from squeezing out burrs, and then return to the furnace immediately. If burrs are squeezed out, it is necessary to place it on a special cooling rack for cooling, and then remove the burrs and return to the furnace for heating. The process described in step two is characterized by using a large unidirectional die forging press and a die to simplify the forgings with multiple parting surface structures into a single parting surface structure for pressing in one fire;
[0042] K3. Final forging: The final forging process is carried out on a unidirectional large-scale die forging press. The surface of the blank is evenly sprayed with lubricant, and then placed in a heating furnace for preheating (preheating temperature is 800-985℃). The final forging die is connected to the press, and the lubricating medium is sprayed in the final forging die cavity. Then the heated blank is placed in the die cavity. The press presses the metal on both sides of the parting surface 2 through the final forging die, and after forming, it is cooled on a special cooling rack.
[0043] If the forging design and forming process on the market are not adopted, firstly, the forging of this cross-shaped three-dimensional structure needs to be invested in a large multi-directional die forging press, which increases the equipment cost; secondly, if new equipment is not invested, a large amount of material can only be applied to reduce the aspect ratio, which will lead to material waste, and the performance of the thick and large cross-section is lower than that of the thin cross-section, as shown in Table 1.
[0044] Material Thick section forging strength properties Strength properties of forgings at thin sections Ti-55531 1192MPa 1213MPa TA15 987MPa 1024MPa
[0045] Table 1
[0046] In step S1, the forging has a three-dimensional shape, with a cross-shaped structure when projected from the side and a sun-shaped structure when projected from the top. The forging is designed with a parting surface 1 and a parting surface 2 in two spatial dimensions.
[0047] In step S2, the size of the forging part is ≥1200×1200×1000 mm, and the projected area of the forging is greater than 1.2 m2.
[0048] In step S3, the same small draft angle is a gradient draft with at least two steps, and the height difference between the steps is evenly divided; the variable draft angle is at least two slopes, and the bevel edge connection points are equally divided according to the width.
[0049] The advantage of designing two steps is to reduce dressing and save raw materials. If a draft angle is conventionally designed for this type of cross-shaped forging, a large amount of dressing will accumulate at the root, which will lead to waste of raw materials, increase the cross section, and affect the final performance of the forging.
[0050] Example 2
[0051] 1. According to the shape of the part, design the position of the double parting surface according to step 1, then design the forging allowance, then design the forging draft angle, and finally design the forging fillet.
[0052] 2. Design the pre-forgings and blanks in sequence according to the cross-sectional dimensions of the forgings, and design tooling A and the pre-forging die according to the structures on both sides of the parting surface 1, design tooling B and the final forging die according to the structures on both sides of the parting surface 2, and design the inner diameter of the upsetting cylinder according to the size of the bar.
[0053] 3. After assembling the upsetting tooling, spray the release agent on the surface of the inner cavity of the tooling, then put the bar material in for upsetting. After the upsetting is completed, immediately pull out the bar material and then return it to the furnace for heating.
[0054] 4. Spray graphite lubricant in tooling A, then place the heated blank into tooling A, press the metal on both sides of the parting surface 1, and then immediately return it to the furnace for heating.
[0055] 5. Spray graphite lubricant in tooling B, then place the heated blank into tooling B, press the metal on both sides of the parting surface 2, and then cool it using a special material rack.
[0056] 6. Spray the lubricating medium evenly on the surface of the blank obtained in step 5, then place it in a heating furnace for preheating, then connect the pre-forging die and the press, and spray the lubricating medium in the die cavity, then place the heated blank in the die cavity to press the metal on both sides of the parting surface 1, and choose to return to the furnace or cool according to the burr situation.
[0057] 7. Spray the lubricating medium evenly on the surface of the blank obtained in step 6, then place it in a heating furnace for preheating, then connect the final forging die and the press, and spray the lubricating medium in the die cavity, then place the heated blank in the die cavity to press the metal on both sides of the parting surface 2, and cool it on a special cooling rack after forming.
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A design method for a large, complex, three-dimensional, multi-partition surface forging, characterized in that: The following steps are involved:
1. Forging design S1. Parting surface design: according to the shape of the forging, a parting surface 1 and a parting surface 2 are divided, and the parting surface 1 and the parting surface 2 intersect and are perpendicular to each other; S2. Forging allowance design: According to the size of the forging parts, the single-side allowance of the forging is designed to be 5-30mm; S3. Draft angle design: The vertical edges on the forgings are designed with the same small draft angle or the variable draft angle. The same small draft angle is designed to expand toward the root along the stepped arrangement, and the slope is designed to be 1-10°; the variable draft angle is designed to gradually increase from the rib top to the root, and the slope is designed to be 1-10°; S4. Transition fillet design: The radius of the concave fillet on the forging is 0.5-3 times the height of the vertical edge, and the radius of the convex fillet is equal to the single-side allowance at that position; 2. Molding process K1. Blank making: First, put the forging material into the heating furnace for preheating, then put the preheated forging into the one-way fast forging machine for upsetting, gather the head metal, press the metal on both sides of the forging parting surface 1 through the head forming tool A, then take out the forging and return it to the furnace for heat preservation for 30 to 120 minutes, then press the metal on both sides of the forging parting surface 2 through the head forming tool B, and place it on a special material rack for cooling after forging to form a blank, and control the underpressure to 5-10mm; K2, pre-forging: spray lubricant evenly on the surface of the blank, place the blank in a heating furnace for preheating, connect the pre-forging die to the press, spray lubricating medium (glass powder lubricant) in the pre-forging die cavity, then place the heated blank in the die cavity, and press the metal on both sides of the parting surface 1 through the pre-forging die; K3. Final forging: Spray lubricant evenly on the surface of the blank, then place it in a heating furnace for preheating, connect the final forging die to the press, spray lubricating medium in the final forging die cavity, then place the heated blank in the die cavity, and press the metal on both sides of the parting surface 2 through the final forging die. After forming, cool it on a special cooling rack.
2. A design method for a large complex three-dimensional multi-partition surface forging according to claim 1, characterized in that: In step S1, the forging has a three-dimensional shape, with a side projection of a "cross" structure and a top projection of a "sun" structure. The forging is designed with a parting surface 1 and a parting surface 2 in two spatial dimensions.
3. The design method of a large complex three-dimensional multi-partition surface forging according to claim 1, characterized in that: In step S2, the size of the forging part is ≥1200×1200×1000mm.
4. A design method for a large complex three-dimensional multi-partition surface forging according to claim 1, characterized in that: In step S3, the same small draft angle is a gradient draft with at least two steps, and the height difference between the steps is evenly divided; the variable draft angle is at least two slopes, and the bevel edge connection points are equally divided according to the width.
Citation Information
Patent Citations
Large-scale engine casing forging mold and forging method
CN109093048A
Forging method of large-scale TC18 titanium alloy die forging for landing gear
CN110814251A
Forging method of high-boss TC18 titanium alloy die forging
CN114160732A
Forked flange forging process
CN116809832A
Novel finish forging die for transmission shaft disc flange yoke forgings
CN210676798U
Cited By
Forging method of cross-shaped forge piece