Large steel ingot production device and method

By setting up a cladding core cylinder in the steel ingot pouring mold, it restrains the agitation of the steel water and casts in a vacuum environment, the surface defects caused by the upper pouring are solved, the surface and internal quality of the steel ingot is improved, and high efficiency and low cost are achieved High-quality steel ingot manufacturing.

CN118905165APending Publication Date: 2024-11-08TIANJIN HEAVY EQUIP ENG RES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995649.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing up-injection casting devices and methods can easily cause large steel ingots to scar and form surface defects such as subcutaneous bubbles, resulting in a large number of surface defects in the forged forgings.

Method used

A cladding core cylinder is installed in the steel ingot casting mold, and the steel water is injected into the cladding core cylinder, flows out from the lower end of the cladding core cylinder and enters the surrounding area, restraining the vigorously stirred steel to create a smoothly rising liquid level, combined with the pouring method, Achieve an effect similar to betting and pouring in a vacuum environment to protect the molten steel.

Benefits of technology

It effectively overcomes the surface defects of the upper pouring casting, improves the surface quality of the steel ingot, and ensures the internal quality of the steel ingot without changing the process flow and adding equipment, achieving efficient and low-cost manufacturing of high-quality large forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905165A_ABST
    Figure CN118905165A_ABST
Patent Text Reader

Abstract

The invention relates to a large steel ingot production device and method, belongs to the technical field of iron-based molten steel ingot casting, and solves the problems that in the prior art, an upper pouring device and method easily cause large steel ingots to scar, form subsurface bubbles and other surface defects. The device comprises a steel ingot casting mold and a wrapping core barrel arranged in the steel ingot casting mold, the wrapping core barrel is in a barrel shape with the upper end and the lower end being open, the wrapping core barrel extends in the steel ingot casting mold from top to bottom, the upper end of the wrapping core barrel directly faces a molten steel inlet, and the lower end of the wrapping core barrel directly faces a molten steel outlet. And the lower end of the cladding core cylinder is not in contact with the bottom of the steel ingot casting mold. According to the device and method, the surface quality of the steel ingot is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron-based molten steel ingot casting, and in particular to a large-scale steel ingot production device and method. Background Art

[0002] Large forgings are usually made by free forging large steel ingots, and the ingot casting methods include top pouring and bottom pouring.

[0003] The steel ingot is cast by top pouring. Usually the casting system is sealed in a vacuum chamber, and the molten steel is poured into the ingot mold from the top.

[0004] The existing top-pouring pouring device and method easily cause large steel ingots to have surface defects such as scarring and subcutaneous bubbles, thereby causing a large number of surface defects in the forged forgings. Summary of the invention

[0005] In view of the above analysis, an embodiment of the present invention aims to provide a large steel ingot production device and method to solve the problem that the existing top pouring casting device and method easily cause large steel ingots to scar, form subcutaneous bubbles and other surface defects, thereby causing a large number of surface defects in the forged forgings.

[0006] On the one hand, an embodiment of the present invention provides a large-scale steel ingot production device, which includes a steel ingot casting mold and a coating core barrel arranged in the steel ingot casting mold, wherein the coating core barrel is a cylinder with open upper and lower ends, and the coating core barrel extends from top to bottom in the steel ingot casting mold, and the upper end of the coating core barrel faces the molten steel inlet, and the lower end of the coating core barrel does not contact the bottom of the steel ingot casting mold.

[0007] Preferably, a fixed load-bearing frame is provided at the upper end of the steel ingot casting mold, and the fixed load-bearing frame is connected to the upper end of the coating core barrel through a hanging support, so that the coating core barrel is suspended in the steel ingot casting mold.

[0008] Preferably, the central axis of the coating core barrel coincides with the central axis of the steel ingot.

[0009] Preferably, the inner diameter of the coating core barrel is greater than or equal to 300 mm and less than or equal to 3 / 4 of the average diameter of the steel ingot.

[0010] Preferably, the length of the coating core barrel is 0.9-1.4 times the height of the steel ingot body.

[0011] Preferably, the wall thickness of the coating core tube is 5-50 mm.

[0012] Preferably, the distance between the lower end of the coating core barrel and the bottom end surface of the steel ingot body is 50-800 mm.

[0013] Preferably, the steel ingot casting mold comprises a chassis, a steel ingot mold, and a heat preservation cap which are arranged in sequence from bottom to top.

[0014] On the other hand, the present invention also provides a method for producing a large steel ingot, using the above-mentioned large steel ingot production device, the method comprising:

[0015] A large ingot production device is placed in a vacuum chamber, and molten steel is injected into the coating core barrel from the molten steel inlet. The molten steel flows out from the lower end of the coating core barrel and enters around the coating core barrel until the pouring is completed and the molten steel level in the coating core barrel is flush with the molten steel level outside the coating core barrel.

[0016] Preferably, the injection speed of molten steel is 1-9t / min.

[0017] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0018] 1. The present invention provides a coating core barrel in the steel ingot casting mold. During casting, molten steel is injected into the coating core barrel, and the molten steel flows out from the lower end of the coating core barrel and enters the surrounding of the coating core barrel, thereby confining the violently agitated molten steel in the coating core barrel, and creating a flow field outside the coating core barrel that rises steadily to the liquid surface, so that the flow field of the molten steel for upper casting is equivalent to that of lower casting, thereby well overcoming the disadvantages of upper casting, and fully realizing a casting method similar to lower casting, thereby improving the surface quality of the steel ingot.

[0019] 2. Although the present invention combines the bottom pouring method, the device is still an upper pouring device. The upper pouring device is relatively small and can be placed in a vacuum chamber. The ingot pouring is carried out in a vacuum environment. The vacuum pouring can protect the molten steel from secondary oxidation, further remove harmful gases in the molten steel, and ensure the internal quality of the bottom pouring.

[0020] 3. The device of the present invention does not need to add special large-scale equipment, does not need to extend the time of each process, and does not change the basic process flow. Instead, a coated core barrel is set in the existing upper pouring mold to improve product quality, thereby realizing efficient and low-cost manufacturing of high-quality steel ingots for large forgings.

[0021] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0023] Figure 1 The invention relates to a large-scale steel nail production device.

[0024] Reference numerals:

[0025] 1-coated core barrel; 2-molten steel inlet; 3-fixed load-bearing frame; 4-hanging support; 5-chassis; 6-ingot mold; 7-insulation cap; 8-insulation brick. DETAILED DESCRIPTION

[0026] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0027] The inventors discovered during their research that when casting steel ingots using the top pouring method, molten steel is injected into the ingot mold from the top. The larger the ingot, the greater the drop of the molten steel in the ingot mold. The molten steel is stirred violently, which can easily cause splashing and air entrainment, thereby forming surface defects such as ingot scarring and subcutaneous bubbles.

[0028] When casting steel ingots by pouring, the pouring system is large and complicated, and it is usually carried out in an atmospheric environment. The molten steel is slowly poured into the ingot mold from the bottom of the ingot mold, and the liquid level of the molten steel rises steadily, which is conducive to the floating and discharge of inclusions in the steel. However, due to non-vacuum casting, the molten steel is easily secondary oxidized or air-absorbed, affecting the quality of the ingot.

[0029] Therefore, the inventors proposed a method of combining the bottom pouring method with the top pouring method, which can not only solve the surface defects such as ingot scarring and subcutaneous bubbles formed due to the violent stirring of molten steel during top pouring, but also ensure the internal quality of the ingot.

[0030] Based on this, the present invention provides a large-scale steel ingot production device, such as Figure 1 As shown, the device includes a steel ingot casting mold and a coating core barrel 1 arranged in the steel ingot casting mold, the coating core barrel is a cylinder with open upper and lower ends, the coating core barrel 1 extends from top to bottom in the steel ingot casting mold, and the upper end of the coating core barrel 1 is opposite to the molten steel inlet 2, and the lower end of the coating core barrel 1 does not contact the bottom of the steel ingot casting mold.

[0031] During implementation, a large-scale steel ingot production device is placed in a vacuum chamber, molten steel is injected into the coating core barrel from the molten steel inlet, and the molten steel flows out from the lower end of the coating core barrel and enters the surrounding of the coating core barrel until the pouring is completed and the molten steel level in the coating core barrel is flush with the molten steel level outside the coating core barrel.

[0032] Compared with the prior art, the present invention sets a coating core barrel in the steel ingot casting mold. During casting, molten steel is injected into the coating core barrel, and the molten steel flows out from the lower end of the coating core barrel and enters the surrounding of the coating core barrel, constraining the violently agitated molten steel in the coating core barrel, and creating a steady rise to the liquid surface outside the coating core barrel, so that the flow field of the upper pouring molten steel is equivalent to the lower pouring, thereby well overcoming the shortcomings of the upper pouring, and fully realizing the casting method similar to the lower pouring, and improving the surface of the steel ingot; the device of the present invention is still an upper pouring device, so that the steel ingot casting can be carried out in a vacuum environment, and the vacuum pouring can protect the molten steel from secondary oxidation, and further remove harmful gases in the steel liquid. The device of the present invention does not need to add special large-scale equipment, does not need to extend the time of each process, and does not change the basic process flow, but sets a coating core barrel in the existing upper pouring casting mold to improve the quality of the steel ingot, and realizes the efficient and low-cost manufacturing of high-quality steel ingots for large forgings.

[0033] It should be noted that the “large steel ingot” refers to a steel ingot with a total weight of not less than 30t.

[0034] Exemplarily, a fixed load-bearing frame 3 is provided at the upper end of the steel ingot casting mold, and the fixed load-bearing frame 3 is connected to the upper end of the coating core barrel 1 through a hanging support 4, so that the coating core barrel 1 is suspended in the steel ingot casting mold.

[0035] It should be noted that the strength of the hanging support 4 ensures that the coated core tube 1 will not swing or sway due to the impact of molten steel during the pouring process.

[0036] Exemplarily, the central axis of the coating core barrel 1 coincides with the central axis of the steel ingot.

[0037] Exemplarily, the temperature of the coating core barrel 1 is -20 to 40°C.

[0038] For example, the inner diameter of the coating core barrel 1 is greater than or equal to 300 mm and less than or equal to 3 / 4 of the average diameter of the steel ingot. If the inner diameter of the coating core barrel 1 is too large, the coating core barrel 1 is easy to leak out during the forging process, and if the inner diameter of the coating core barrel 1 is too small, the casting cannot be completed smoothly.

[0039] Exemplarily, the length of the coating core barrel 1 is 0.9-1.4 times the height of the steel ingot body, such as 1.0 times, 1.1 times, 1.2 times, and 1.3 times. If the length of the coating core barrel 1 is too long, it cannot be completely coated in the steel ingot. If the length of the coating core barrel 1 is too short, the violently agitated molten steel cannot be confined in the coating core barrel.

[0040] It should be noted that, in order to ensure that the steel ingot completely wraps the coating core barrel 1, the length of the coating core barrel 1 cannot exceed the total height of the steel ingot (the sum of the heights of the ingot body, the nozzle, and the riser).

[0041] Exemplarily, the wall thickness of the coating core tube 1 is 5-50 mm. For example, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm. If the wall thickness of the coating core tube 1 is too thin, it is easy to melt or break during the pouring process, reducing the effect; if the wall thickness of the coating core tube 1 is too thick, it will increase the solidification rate, affecting the smooth pouring and the stability of the overall structure.

[0042] For example, the distance between the lower end of the coating core barrel 1 and the bottom end surface of the steel ingot body is 50-800 mm. If the distance is too small, it will affect the smooth pouring, and if the distance is too large, it will affect the quality of the steel ingot.

[0043] Exemplarily, the steel ingot casting mold comprises a bottom plate 5, a steel ingot mold 6, and a heat preservation cap 7 which are sequentially arranged from bottom to top. The coating core barrel 1 extends from the heat preservation cap 7 to the steel ingot mold 6.

[0044] Exemplarily, the inner wall of the thermal insulation cap 7 is provided with thermal insulation bricks 8 .

[0045] Exemplarily, the molten steel inlet 2 is arranged at the upper end of the thermal insulation cap 7 , and the fixed load-bearing frame 3 is arranged above the thermal insulation cap 7 .

[0046] The present invention has no limitation on the specific structure of the fixed load-bearing frame 3, as long as it does not affect the pouring of molten steel. For example, the fixed load-bearing frame 3 is in a well shape, and the four strip structures forming the well are supported by the upper end surface of the insulation cap 7. This arrangement will not block the molten steel inlet, and can stably hang the coated core tube 1.

[0047] Exemplarily, the hanging support 4 is a straight rod type or a spiral type. The hanging support 4 and the fixed load-bearing frame 3 ensure the stability of the hanging of the coating core tube 1.

[0048] On the other hand, the present invention also provides a method for producing a large steel ingot, using the above-mentioned large steel ingot production device, the method comprising:

[0049] A large-scale steel ingot production device is placed in a vacuum chamber, and molten steel is injected into the coating core barrel 1 from the molten steel inlet 2. The molten steel flows out from the lower end of the coating core barrel 1 and enters the surrounding of the coating core barrel 1 until the pouring is completed. The molten steel level in the coating core barrel 1 is flush with the molten steel level outside the coating core barrel 1.

[0050] Exemplarily, during pouring, the vacuum degree of the device is not higher than 133Pa.

[0051] Exemplarily, the superheat degree of the poured molten steel is 20-100° C. For example, 40° C., 60° C., 80° C., etc.

[0052] Exemplarily, the injection speed of molten steel is 1-9 t / min, such as 2 t / min, 3 t / min, 4 t / min, 5 t / min, 6 t / min, 7 t / min, 8 t / min.

[0053] Exemplarily, the method also includes: after the pouring is completed, when the molten steel on the outer wall of the coating core tube 1 begins to solidify, lifting the coating core tube 1 so that it is lifted out of the ingot casting mold as a whole; or, 1-2 hours before the molten steel is completely solidified into an ingot, lifting and pulling off the hanging support 4, so that the hanging support 4 is completely separated from the coating core tube 1, and the coating core tube 1 remains in the ingot.

[0054] In practical applications, the coated core tube 1 can be lifted or left in the ingot according to the purpose of use of the ingot. For solutions that require homogenization inside the ingot, the coated core tube 1 can be lifted; for solutions that require homogenization inside the ingot, the coated core tube 1 can be left in the ingot.

[0055] In order to ensure that the steel ingot is uniformly ductile as a whole during the subsequent forging process, the material of the coating core tube 1 has similar ductility to that of the steel ingot.

[0056] Since the solidification speeds of ingots of different sizes are different, the time for lifting the coated core barrel 1 can be determined according to the size of the ingot. For example, the time for lifting the coated core barrel 1 is 3-30 hours after the pouring of molten steel. If the tube is pulled out in advance, the surface quality of the ingot will be affected.

[0057] Exemplarily, the speed of lifting the covering core barrel 1 is 5 m / min.

[0058] Exemplarily, the method further includes: removing the heat preservation cap 7 1-2 hours before the molten steel is completely solidified into a steel ingot, and then lifting the completely solidified steel ingot out of the steel ingot mold 6 .

[0059] The large-scale steel ingot production device and method of the present invention are further described below through specific embodiments.

[0060] Example 1

[0061] This embodiment provides a large-scale steel ingot production device, the corresponding steel ingot weight of the device is 74t, the average diameter of the steel ingot is 1830mm, and the height of the steel ingot body is 2950mm; the device includes a steel ingot casting mold and a coating core barrel 1 arranged in the steel ingot casting mold, the coating core barrel is a cylindrical shape with open upper and lower ends, the coating core barrel 1 extends from top to bottom in the steel ingot casting mold, and the upper end of the coating core barrel 1 is directly opposite to the molten steel inlet 2, and the lower end of the coating core barrel 1 does not contact the bottom of the steel ingot casting mold; a fixed load-bearing frame 3 is arranged at the upper end of the steel ingot casting mold, and the fixed load-bearing frame 3 is connected to the upper end of the coating core barrel 1 through a hanging support 4, so that the coating core barrel 1 is suspended in the steel ingot casting mold; the hanging support 4 is a straight rod type. The central axis of the coating core barrel 1 coincides with the central axis of the steel ingot, and the temperature is 30°C. The inner diameter of the coating core barrel 1 is 500 mm, the length is 2730 mm, and the wall thickness is 20 mm. The distance between the lower end of the coating core barrel 1 and the bottom end surface of the steel ingot body is 200 mm. The steel ingot casting mold includes a bottom plate 5, a steel ingot mold 6, and a heat preservation cap 7 arranged in sequence from bottom to top. The coating core barrel 1 extends from the heat preservation cap 7 to the steel ingot mold 6. The inner wall of the heat preservation cap 7 is provided with heat preservation bricks 8.

[0062] Example 2

[0063] This embodiment provides a method for producing a large steel ingot, using the device of embodiment 1, the method comprising:

[0064] Step (1): placing a large-scale steel ingot production device in a vacuum chamber with a vacuum degree not higher than 133Pa; injecting molten steel into the coating core barrel 1 from the molten steel inlet 2, and the molten steel passes through the coating core barrel 1 into the steel ingot mold, with an injection rate of 6t / min and a superheat degree of the poured molten steel of 80°C; the molten steel flows out from the lower end of the coating core barrel 1 and enters the surrounding of the coating core barrel 1 until the pouring is completed and the molten steel liquid level in the coating core barrel 1 is flush with the molten steel liquid level outside the coating core barrel 1.

[0065] Step (2): After the pouring is completed, wait for 6 hours after the molten steel is poured, and then lift out the coated core tube 1 by lifting the fixed load-bearing frame 3, so that it can be lifted out of the steel ingot casting mold as a whole.

[0066] Step (3): The complete solidification time of the 74t steel ingot is 22h. The insulation cap 7 is removed 20h after the steel ingot is poured, and then the steel ingot is lifted out of the ingot mold 6.

[0067] Example 3

[0068] This embodiment provides a large-scale steel ingot production method similar to that of Embodiment 2, except that, in step 4, after the molten steel is completely solidified into a steel ingot, the hanging support 4 is lifted and pulled off, so that the hanging support 4 is completely separated from the steel ingot.

[0069] Example 4

[0070] This embodiment provides a large steel ingot production method similar to that of Embodiment 3, except that the central axis of the coating core barrel 1 does not coincide with the central axis of the steel ingot.

[0071] Example 5

[0072] This embodiment provides a large-scale steel ingot production method similar to that of Embodiment 3, except that the inner diameter of the coating core barrel 1 is greater than 3 / 4 of the average diameter of the steel ingot, which is 1400 mm.

[0073] Example 6

[0074] This embodiment provides a large-scale steel ingot production method similar to that of Embodiment 2, except that the distance between the lower end of the coating core barrel 1 and the bottom end surface of the steel ingot body is 900 mm.

[0075] Example 7

[0076] This embodiment provides a large-scale steel ingot production method similar to that of Embodiment 2, except that in step (2), after the pouring is completed, the coated core tube 1 is hoisted out after 2 hours of molten steel pouring.

[0077] Comparative Example 1

[0078] This comparative example adopts an existing large-scale steel ingot production device, that is, it is similar to the device of Example 1, except that the coating core barrel 1, the fixed load-bearing frame 3 and the hanging support 4 are not provided.

[0079] Results

[0080] The steel ingots of Examples 2-7 and Comparative Example 1 were subjected to forging, post-forging heat treatment, rough machining, and then to quenching and tempering, differential temperature and other heat treatment processes. The forgings obtained after fine machining were subjected to UT flaw detection (internal defects) and surface wave inspection (surface defects). The characterization results are shown in Table 1:

[0081] Table 1

[0082]

[0083] As can be seen from Table 1, the surface quality of Example 2-7 is better than that of Comparative Example 1. This is because Example 2-7 is provided with a coating core barrel in the steel ingot casting mold. During casting, molten steel is injected into the coating core barrel, and the molten steel flows out from the lower end of the coating core barrel and enters the surrounding of the coating core barrel, constraining the violently agitated molten steel in the coating core barrel, and creating a stable rise to the liquid surface outside the coating core barrel, so that the flow field of the upper pouring molten steel is equivalent to the lower pouring, thereby well overcoming the disadvantages of the upper pouring, and fully realizing the casting method similar to the lower pouring, and improving the surface quality of the steel ingot. Although Example 2-7 combines the lower pouring method, the device is still an upper pouring device, which is relatively small and can be placed in a vacuum chamber. The steel ingot is cast in a vacuum environment. The vacuum casting can protect the molten steel from secondary oxidation, further remove harmful gases in the molten steel, and ensure the internal quality of the steel nail. The internal quality of the steel ingot will not be affected by combining the lower pouring method with the upper pouring method.

[0084] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A large-scale steel ingot production device, characterized in that: The device includes a steel ingot casting mold and a coating core barrel arranged in the steel ingot casting mold. The coating core barrel is a cylinder with open upper and lower ends. The coating core barrel extends from top to bottom in the steel ingot casting mold, and the upper end of the coating core barrel faces the molten steel inlet, and the lower end of the coating core barrel does not contact the bottom of the steel ingot casting mold.

2. The device according to claim 1, characterized in that A fixed load-bearing frame is arranged at the upper end of the steel ingot casting mold, and the fixed load-bearing frame is connected to the upper end of the coating core barrel through a hanging support, so that the coating core barrel is suspended in the steel ingot casting mold.

3. The device according to claim 1, characterized in that The central axis of the cladding core barrel coincides with the central axis of the steel ingot.

4. The device according to claim 1, characterized in that The inner diameter of the coating core barrel is greater than or equal to 300 mm and less than or equal to 3 / 4 of the average diameter of the steel ingot.

5. The device according to claim 1, characterized in that The length of the coating core barrel is 0.9-1.4 times the height of the steel ingot body.

6. The device according to claim 1, characterized in that The wall thickness of the coating core tube is 5-50 mm.

7. The device according to claim 1, characterized in that The distance between the lower end of the coating core barrel and the bottom end surface of the steel ingot body is 50-800 mm.

8. The device according to claim 1, characterized in that The steel ingot casting mold comprises a chassis, a steel ingot mold and a heat preservation cap which are arranged in sequence from bottom to top.

9. A method for producing large steel ingots, characterized in that: Using the large-scale steel ingot production device according to any one of claims 1 to 8, the method comprises: A large ingot production device is placed in a vacuum chamber, and molten steel is injected into the coating core barrel from the molten steel inlet. The molten steel flows out from the lower end of the coating core barrel and enters around the coating core barrel until the pouring is completed and the molten steel level in the coating core barrel is flush with the molten steel level outside the coating core barrel.

10. The method according to claim 9, characterized in that The injection speed of molten steel is 1-9t / min.