Multi-scale reinforced phase reinforced laser cladding gear steel and preparation method thereof

By introducing multi-scale enhanced phases into aircraft engine transmission gear steel, laser cladding technology is used to achieve uniform distribution of enhanced phases in grain boundaries and crystals, the problem of low hardness in the existing technology is solved, and the wear resistance of gear steel is improved and high temperature stability.

CN118905243APending Publication Date: 2024-11-08XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999824.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The microstructure of the repair area obtained by the laser energy deposition and repair technology of the existing aero engine transmission gear lacks enhanced phase pinning, resulting in low hardness. The existing DS alloys are all based on single-scale enhanced phase reinforcement designs, and lack multi-scale enhanced phase coupling reinforcement. technology.

Method used

The preparation method of multi-scale enhanced phase-strengthening laser clad gear steel is adopted. By fully mixing the gear steel prealloy powder with TiC, TiH2 and YH2 composite system of different particle sizes, the enhanced phase powder is directly used for direct use of laser. The energy deposition method produces multi-scale enhanced phase-enhanced laser cladding gear steel to achieve uniform distribution of the enhanced phases in the grain boundaries and within the crystal.

Benefits of technology

The wear resistance and high-temperature structure stability of gear steel are improved, and the hardness and wear resistance of gear steel are improved through the pinning of micron-scale TiC or WC at the grain boundary and nano-scale Y-Ti-O in the crystal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905243A_ABST
    Figure CN118905243A_ABST
Patent Text Reader

Abstract

The invention discloses multi-scale reinforced phase reinforced laser cladding gear steel and a preparation method thereof, and belongs to the technical field of composite material preparation. According to the invention, by introducing multi-scale reinforced phase particles into the alloy, a plurality of reinforced phase pinning grain boundary and intragranular optimal microstructures are obtained, and the wear resistance of the gear steel is improved. Laser cladding is selected as a preparation means, on one hand, step simplification and cost reduction are considered, and on the other hand, due to the fact that an additive manufacturing molten pool is extremely small and the cooling speed is ultra-high, a reinforced phase can be evenly distributed. According to the multi-scale reinforced phase reinforced laser cladding gear steel prepared through the method, in the high-temperature deformation process, grain boundary TiC (or WC) can generate a remarkable pinning effect on the grain boundary, intragranular Y-Ti-O particles can form a dragging effect on dislocation and solid solution atoms, and therefore alloy has good high-temperature structure stability, the method is an effective means for improving the wear resistance of the gear steel, and the service life of the gear steel is prolonged. Therefore, the method can be widely applied to the fields of aero-engines and the like and is also suitable for field gear repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite material preparation, and in particular relates to a multi-scale enhanced phase strengthened laser cladding gear steel and a preparation method thereof. Background Art

[0002] Wear is one of the main forms of gear steel damage. China consumes millions of tons of steel every year due to wear, causing huge economic losses. The appearance and performance of aircraft engine gears cannot meet the needs of continued service due to the loss of pieces or wear. If the failed high-value aircraft engine transmission gears are directly discarded, it will cause huge economic losses. Laser energy deposition technology is an emerging technology for repairing high-value damaged parts of aircraft and engines. It has attracted widespread attention because it can simultaneously restore all geometric features and some mechanical properties of damaged parts, and has the advantages of short cycle and low cost. However, if laser energy deposition is used alone to repair damaged parts with gear steel powder, the hardness is low due to the lack of reinforcing phase pinning such as carbide in the repair area, which cannot meet the needs.

[0003] Dispersion Strengthened (DS) is a strengthening method that uses high-density, high-temperature stable reinforcing phases to be evenly dispersed in the alloy matrix to significantly improve the high-temperature mechanical properties of the alloy. Compared with traditional alloys, the DS alloy microstructure has better high-temperature stability and has been successfully used in extreme service conditions such as aerospace and nuclear power. Although traditional processes have been successful in preparing DS alloys, they usually require mechanical alloying, thermoplastic forming (such as hot isostatic pressing, hot sintering, etc.), subtractive processing and other processes ( Figure 1 ) to get the final product, which is costly, cumbersome and has unstable performance. On the contrary, laser energy deposition, as a new forming technology, can directly obtain complex and near-net-shaped components from metal powder ( Figure 1 ), which makes it possible to prepare DS alloys at low cost. Moreover, the laser energy deposition process has an ultra-fast cooling rate, and the resulting alloy microstructure is finer and the composition is more uniform. Therefore, in theory, laser energy deposition can produce DS alloys with better hardness. In addition, the existing DS alloy hardness improvement mainly focuses on the introduction of a single-scale reinforcement phase, or the reinforcement phase pinning the grain boundary ( Figure 2 (a)) or the enhanced phase pinning in the crystal ( Figure 2 (b)), and for multiple reinforced phase coupling reinforced composite materials ( Figure 2 There are few reports on the research and development of (c)).

[0004] In summary, the microstructure of the repaired area obtained by the existing laser energy deposition repair technology of aircraft engine transmission gears lacks reinforcement phase pinning and has low hardness; DS technology is an effective means to improve the hardness of alloys, but the existing DS alloys are all based on single-scale reinforcement phase strengthening design, and multi-scale reinforcement phase coupling strengthening technology has not been developed. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a multi-scale enhanced phase strengthened laser cladding gear steel and a preparation method thereof, so as to solve the technical problem that the existing method cannot ensure the microstructure stability of the gear steel and thus leads to lower hardness.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preparing a multi-scale enhanced phase strengthened laser cladding gear steel, comprising: fully and uniformly mixing gear steel pre-alloy powder and enhanced phase powder, and preparing a gear steel block by laser direct energy deposition, namely, multi-scale enhanced phase strengthened laser cladding gear steel; wherein,

[0008] The reinforcing phase powder is a composite system of TiC, TiH2 and YH2 with different particle sizes or a composite system of WC, TiH2 and YH2.

[0009] Preferably, the D50 particle size of TiC powder and WC powder is less than 5 μm, and the D50 particle size of TiH2 and YH2 particles is less than 10 μm.

[0010] Preferably, TiC powder and WC powder account for 10% to 30% of the bulk volume of the gear steel pre-alloyed powder; TiH2 and YH2 particles account for 0.2% to 1.0% of the mass of the gear steel pre-alloyed powder respectively.

[0011] Preferably, the gear steel pre-alloyed powder comprises, by mass percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe; the particle size of the gear steel pre-alloyed powder is 50-180μm.

[0012] Preferably, the mixing is carried out uniformly by using an acoustic resonance method or a mechanical alloying method.

[0013] Among them, acoustic resonance mixing is a technology that uses the principle of sound wave resonance to achieve uniform mixing of materials. It usually uses an exciter to generate a vibration frequency that is close to or the same as the resonance frequency of the mixed material system, thereby inducing a resonance effect in the material and achieving uniform mixing of the material.

[0014] Therefore, it is further preferred that the process parameters of the acoustic resonance method used in the present invention are a vibration frequency of 40-80 Hz, an acceleration of 60-80 G, a vibration time of not less than 10 min, and drying after mixing to form a composite powder.

[0015] Mechanical alloy mixing is a method of uniformly mixing alloy powders or raw materials by mechanical means. This method mainly relies on mechanical mixing equipment, such as high-energy ball mills, blenders, stirrers, etc., which mix alloy powders or raw materials inside the equipment through mechanical friction, collision, extrusion, etc.

[0016] Therefore, it is further preferred that the process parameters of the mechanical alloying method used in the present invention are a ball-to-material ratio of 10:1, a main disk speed of 200-400rpm, a revolution-to-rotation ratio of 1:2, and a ball milling time of 15-40 hours under the protection of high-purity argon.

[0017] Preferably, the process parameters of the laser direct energy deposition method are laser power 500-1800 W, scanning speed 5-12 mm / s, and feed rate 0.3-0.8 r / min.

[0018] The present invention also discloses a multi-scale reinforced phase strengthened laser cladding gear steel prepared by the above-mentioned preparation method. When the reinforced phase powder is a composite system of TiC, TiH2 and YH2, TiC particles are evenly distributed on the grain boundaries of the prepared multi-scale reinforced phase strengthened laser cladding gear steel, with an average size of less than 1.5 μm, and the nano-Ti-YO reinforced phase formed by the in-situ reaction of TiH2 particles and YH2 particles during the preparation process is distributed inside the grains.

[0019] The present invention also discloses a multi-scale enhanced phase strengthened laser cladding gear steel prepared by the above-mentioned preparation method. When the reinforcing phase powder selects a composite system of WC, TiH2 and YH2, WC particles are uniformly distributed on the grain boundaries of the prepared multi-scale enhanced phase strengthened laser cladding gear steel, with an average size of less than 1.5 μm, and the nano-Ti-YO reinforcing phase formed by the in-situ reaction of TiH2 particles and YH2 particles during the preparation process is distributed inside the grains.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention adopts laser cladding technology for gear steel, and obtains multiple reinforcing phases pinning grain boundaries and optimal microstructures within the grains by introducing multi-scale reinforcing phase particles into the alloy, thereby improving the wear resistance of the gear steel. The present invention selects laser cladding as the preparation method, on the one hand to simplify the steps and reduce costs, and on the other hand, because the additive manufacturing molten pool is extremely small and the cooling rate is ultra-fast, the reinforcing phase can be evenly distributed during the preparation process; TiC (or WC) is selected as the reinforcing phase because of its high melting point (TiC melting point is 3160°C, WC melting point is 2780°C), which is much higher than the melting point of iron 1538°C, so during the laser cladding process, TiC (or WC) is still a solid particle, which can be used as a non-uniform nucleating agent during alloy solidification to refine the grains. , pinning the grain boundaries and improving the stability of the alloy structure; TiH2 and YH2 particles are selected as the reinforcing phase because of their low melting points (TiH2 melting point is 350°C, YH2 melting point is 300°C), so during the laser cladding process, TiH2 and YH2 particles can be supersaturated and dissolved in the molten pool, and in the subsequent intrinsic cycle heat treatment of laser cladding, the Ti and Y dissolved in the matrix and the O element introduced in the additive manufacturing react in situ to precipitate the nano Y-Ti-O precipitated phase with the best size and density, thereby pinning the crystal. Therefore, it can be seen that the preparation method of the present invention has simple process steps and low cost, can effectively regulate the microstructure of gear steel, make a variety of reinforcing phases evenly distributed in the alloy, and simultaneously improve the stability of the microstructures at the grain boundaries and within the crystal, thereby improving the hardness of the gear steel.

[0022] The multi-scale enhanced phase strengthened laser cladding gear steel prepared by the method of the present invention has its grain boundaries pinned by micron-level TiC (or WC) and the crystals pinned by nano-level Y-Ti-O precipitation phases. During high-temperature deformation, the grain boundary TiC (or WC) can produce a significant pinning effect on the grain boundaries, and the Y-Ti-O particles in the crystals can form a dragging effect on dislocations and solid solution atoms, so that the alloy has good high-temperature structural stability, which is an effective means to improve the wear resistance of gear steel. Therefore, it can be widely used in the fields of aircraft engines and is also suitable for field gear repair. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Comparison of the steps for preparing DS alloy using traditional technology and additive manufacturing;

[0024] Figure 2 Design diagrams for different DS alloy microstructures;

[0025] Figure 3 The micrograph of the metallographic structure of the gear steel in Example 1 of the present invention, in which the volume content of TiC is 20%, the weight content of TiH2 and YH2 is 0.3% and 0.5% respectively, indicates that the grain boundary is pinned by spherical TiC;

[0026] Figure 4This is a microscopic photograph of the metallographic structure of the gear steel in Example 1 of the present invention, in which the volume content of TiC is 20%, and the weight contents of TiH2 and YH2 are 0.3% and 0.5% respectively, indicating that the crystal is pinned by high-density Ti-YO particles. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0029] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0030] The preparation method of multi-scale enhanced phase strengthened laser cladding gear steel disclosed in the present invention comprises:

[0031] First, a gear steel pre-alloyed powder with a particle size range of 50μm-180μm is configured by mass percentage, 10-30% of TiC (or WC) (D50 particle size less than 5μm) particles are configured according to the loose volume of the gear steel powder, and 0.2-1.0% of TiH2 and YH2 particles (D50 particle size less than 10μm) are configured according to the weight of the gear steel powder; then, the above powders are fully mixed by mechanical alloying or acoustic resonance process; finally, a gear steel block is obtained by laser direct energy deposition process, and multi-scale enhanced phase reinforced gear steel can be obtained.

[0032] Specifically, the steps include:

[0033] Step 1, the gear steel pre-alloyed powder, the powder components by weight percentage are: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe; the powder particle size is 50-180μm;

[0034] Step 2, reinforcement phase: the reinforcement phase includes TiC (or WC), TiH2, and YH2 particles, the D50 particle size of TiC powder (or WC powder) is less than 5 μm, and the D50 particle size of TiH2 and YH2 particles is less than 10 μm;

[0035] Step 3, powder mixing: the gear steel pre-alloyed powder and the reinforcement phase are uniformly mixed by acoustic resonance or mechanical alloying process;

[0036] Step 4, alloy preparation: obtaining a gear steel block by laser direct energy deposition process;

[0037] The multi-scale reinforced phase strengthened laser cladding gear steel prepared by the above method has TiC particles (or WC particles) evenly distributed at the grain boundaries, with an average size of less than 1.5 μm, and the nano-reinforced phase formed by the in-situ reaction of TiH2 and YH2 particles during the preparation process is distributed inside the grains.

[0038] Example 1

[0039] Step 1: Take gear steel pre-alloyed powder and reinforcement phase particles, wherein the gear steel pre-alloyed powder is as follows by weight percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe, and the powder particle size is 50-180μm;

[0040] Step 2: According to the loose volume of the gear steel powder in step 1, 20% TiC particles (D50 particle size is less than 5 μm) are configured, and according to the weight of the gear steel powder, 0.3% TiH2 and 0.6% YH2 particles (both D50 particle sizes are less than 10 μm) are configured;

[0041] Step 3: The gear steel pre-alloyed powder and the reinforcement phase particles in the above steps 1 and 2 are fully mixed by an acoustic resonance process, wherein the acoustic resonance parameters are a vibration frequency of 60 Hz, an acceleration of 80 G, and a vibration time of not less than 30 min;

[0042] Step 4: The gear steel block is obtained by laser direct energy deposition process, and the laser direct energy deposition process parameters used are laser power 1200W, scanning speed 9mm / s, and feeding weight 0.7r / min;

[0043] Step 5: Prepare the block obtained in step 4 as a metallographic sample, and observe the pinning phase near its grain boundary using a metallographic microscope, such as Figure 3 As shown, it can be seen that submicron TiC particles are evenly distributed near the grain boundaries;

[0044] Step 6: The block obtained in step 4 is prepared as a transmission sample, and the in-situ nano-precipitated phase in the crystal is observed using a transmission electron microscope, such as Figure 4 As shown, it can be seen that the nanoscale reinforcement phase is evenly distributed in the crystal;

[0045] Step 7: The block obtained in step 4 was prepared as a metallographic sample, and the hardness was measured under a load of 1000 g and full load of 15 s. The results are listed in Table 1.

[0046] Example 2

[0047] Step 1: Take gear steel pre-alloyed powder and reinforcement phase particles, wherein the gear steel pre-alloyed powder is as follows by weight percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe, and the powder particle size is 50-180μm;

[0048] Step 2: According to the loose volume of the gear steel powder, 20% of WC particles (D50 particle size is less than 5μm) are configured, and according to the weight of the gear steel powder, 0.3% of TiH2 and 0.6% of YH2 particles (both D50 particle size is less than 10μm) are configured:;

[0049] Step 3: The gear steel pre-alloyed powder and the reinforcement phase particles in the above steps 1 and 2 are fully mixed by an acoustic resonance process, wherein the acoustic resonance parameters are a vibration frequency of 60 Hz, an acceleration of 80 G, and a vibration time of not less than 30 min;

[0050] Step 4: The gear steel block is obtained by laser direct energy deposition process, and the laser direct energy deposition process parameters used are laser power 1200W, scanning speed 8mm / s, and feeding weight 0.6r / min;

[0051] Step 5: The block obtained in step 4 was prepared as a metallographic sample, and the hardness was measured under a load of 1000 g and full load of 15 s. The results are listed in Table 1.

[0052] Example 3

[0053] Step 1: Take gear steel pre-alloyed powder and reinforcement phase particles, wherein the gear steel pre-alloyed powder is as follows by weight percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe, and the powder particle size is 50-180μm;

[0054] Step 2: According to the loose volume of the gear steel powder, 20% TiC particles (D50 particle size is less than 5 μm) are configured, and according to the weight of the gear steel powder, 0.3% TiH2 and 0.6% YH2 particles (both D50 particle size is less than 10 μm) are configured:;

[0055] Step 3: The gear steel pre-alloyed powder and the reinforcement phase particles in the above steps 1 and 2 are fully mixed by a mechanical alloying process, and the mechanical alloying parameters are a ball-to-material ratio of 10:1, a main plate speed of 300 rpm, a revolution-to-autonomous ratio of 1:2, high-purity argon (99.9999%) protection, and a ball milling time of 30 hours;

[0056] Step 4: The gear steel block is obtained by laser direct energy deposition process, and the laser direct energy deposition process parameters used are laser power 900W, scanning speed 7mm / s, and feeding weight 0.6r / min;

[0057] Step 5: The block obtained in step 4 was prepared as a metallographic sample, and the hardness was measured under a load of 1000 g and full load of 15 s. The results are listed in Table 1.

[0058] Example 4

[0059] Step 1: Take gear steel pre-alloyed powder and reinforcement phase particles, wherein the gear steel pre-alloyed powder is as follows by weight percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe, and the powder particle size is 50-180μm;

[0060] Step 2: According to the loose volume of the gear steel powder, 20% WC particles (D50 particle size is less than 5μm) are configured, and according to the weight of the gear steel powder, 0.3% TiH2 and 0.5% YH2 particles (both D50 particle size is less than 10μm) are configured:;

[0061] Step 3: The gear steel pre-alloyed powder and the reinforcement phase particles in the above steps 1 and 2 are fully mixed by a mechanical alloying process, and the mechanical alloying parameters are a ball-to-material ratio of 10:1, a main plate speed of 250 rpm, a revolution-to-autorotation ratio of 1:2, high-purity argon (99.9999%) protection, and a ball milling time of 35 hours;

[0062] Step 4: The gear steel block is obtained by laser direct energy deposition process, and the laser direct energy deposition process parameters used are laser power 700W, scanning speed 6mm / s, and feeding weight 0.6r / min;

[0063] Step 5: The block obtained in step 4 was prepared as a metallographic sample, and the hardness was measured under a load of 1000 g and full load of 15 s. The results are listed in Table 1.

[0064] Comparative Example 1

[0065] Step 1: Take gear steel pre-alloy powder, according to the weight percentage: 0.09% ≤ C ≤ 0.20%, 0.3% ≤ Mn ≤ 1.0%, 0.1% ≤ Si ≤ 1.0%, 0.05% ≤ Mo ≤ 0.35%, 0.5% ≤ Cr ≤ 2.0%, 1.0% ≤ Ni ≤ 5.0%, 0.03% ≤ Cu ≤ 0.5%, 0.1% ≤ Ti ≤ 0.5%, and the rest is Fe, and the powder particle size is 50-180 μm.

[0066] Step 2: Mix the gear steel pre-alloyed powder in an acoustic resonance device, wherein the acoustic resonance parameters are a vibration frequency of 60 Hz, an acceleration of 60 G, and a vibration time of not less than 60 min;

[0067] Step 3: The gear steel block is obtained by laser direct energy deposition process, and the laser direct energy deposition process parameters used are laser power 900W, scanning speed 7mm / s, and feeding weight 0.6r / min;

[0068] Step 4: The block obtained in step 3 was prepared as a metallographic sample, and the hardness was measured under a load of 1000 g and full load of 15 s. The results are listed in Table 1.

[0069] Comparative Example 2

[0070] Step 1: Take gear steel pre-alloyed powder and reinforcement phase particles, wherein the gear steel pre-alloyed powder is as follows by weight percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe, and the powder particle size is 50-180μm;

[0071] Step 2: Add 20% WC particles (D50 particle size less than 5 μm) according to the loose volume of gear steel powder;

[0072] Step 3: The gear steel pre-alloyed powder and the reinforcement phase particles in the above steps 1 and 2 are fully mixed by a mechanical alloying process, and the mechanical alloying parameters are a ball-to-material ratio of 10:1, a main disk speed of 250 rpm, a revolution-to-autorotation ratio of 1:2, high-purity argon (99.9999%) protection, and a ball milling time of 30 hours;

[0073] Step 4: The gear steel block is obtained by laser direct energy deposition process, and the laser direct energy deposition process parameters used are laser power 700W, scanning speed 6mm / s, and feeding weight 0.6r / min;

[0074] Step 5: The block obtained in step 4 was prepared as a metallographic sample, and the hardness was measured under a load of 1000 g and full load of 15 s. The results are listed in Table 1.

[0075] Table 1 shows the micro-Vickers hardness of the samples of the embodiments of the present invention and the comparative examples.

[0076] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 360HV 347HV 373HV 368HV 278HV 323HV

[0077] It can be seen that the hardness of the multi-scale reinforcement phase strengthened gear steels prepared in Examples 1 to 4 of the present invention is higher than that of Comparative Example 1 without reinforcement phase and Comparative Example 2 with single-scale reinforcement phase. This further illustrates that the use of multi-scale reinforcement phases in the present invention can stably improve the hardness of gear steels.

[0078] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A preparation method for multi-scale enhanced phase laser cladding gear steel, It is characterized in that include: The gear steel pre-alloy powder and the reinforcement phase powder are fully mixed and uniformly, and the gear steel block is prepared by laser direct energy deposition method, that is, multi-scale reinforcement phase strengthened laser cladding gear steel; wherein, The reinforcing phase powder is selected from TiC, TiH 2 and YH 2 Composite system or WC, TiH 2 and YH 2 Composite system.

2. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 1, It is characterized in that The D50 particle size of TiC powder and WC powder is less than 5μm, and the D50 particle size of TiH 2 and YH 2 The particle size D50 is less than 10 μm.

3. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 1, It is characterized in that TiC powder and WC powder account for 10% to 30% of the loose volume of gear steel pre-alloyed powder; TiH 2 and YH 2 The particles account for 0.2%-1.0% of the mass of the gear steel pre-alloyed powder.

4. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 1, It is characterized in that The gear steel pre-alloyed powder comprises, by mass percentage: 0.09%≤C≤0.20%, 0.3%≤Mn≤1.0%, 0.1%≤Si≤1.0%, 0.05%≤Mo≤0.35%, 0.5%≤Cr≤2.0%, 1.0%≤Ni≤5.0%, 0.03%≤Cu≤0.5%, 0.1%≤Ti≤0.5%, and the rest is Fe; the particle size of the gear steel pre-alloyed powder is 50-180μm.

5. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 1, It is characterized in that The mixing is carried out uniformly by using an acoustic resonance method or a mechanical alloying method.

6. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 5, It is characterized in that The process parameters of the acoustic resonance method are a vibration frequency of 40-80 Hz, an acceleration of 60-80 G, a vibration time of not less than 10 min, and drying after mixing to form a composite powder.

7. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 5, It is characterized in that The process parameters of the mechanical alloying method are a ball-to-material ratio of 10:1, a main disk speed of 200-400rpm, a revolution-to-rotation ratio of 1:2, and a ball milling time of 15-40 hours under the protection of high-purity argon.

8. The method for preparing multi-scale enhanced phase strengthened laser cladding gear steel according to claim 1, It is characterized in that The process parameters of the laser direct energy deposition method are laser power 500-1800W, scanning speed 5-12mm / s, and feed rate 0.3-0.8r / min.

9. Multi-scale enhanced phase strengthened laser cladding gear steel prepared by any one of the preparation methods of claims 1 to 8, It is characterized in that When the reinforcing phase powder is TiC, TiH 2 and YH 2 When the composite system is prepared, TiC particles are evenly distributed on the grain boundaries of the prepared multi-scale enhanced phase strengthened laser cladding gear steel, with an average size of less than 1.5 μm, and TiH 2 Particles, YH 2 The nano-Ti-YO reinforcement phase formed by in-situ reaction during the preparation process is distributed inside the grains.

10. Multi-scale enhanced phase strengthened laser cladding gear steel prepared by the preparation method of any one of claims 1 to 8, It is characterized in that When the reinforcing phase powder is selected as WC, TiH 2 and YH 2 When the composite system is prepared, the WC particles are evenly distributed on the grain boundaries of the multi-scale enhanced phase strengthened laser cladding gear steel, with an average size of less than 1.5 μm, and the TiH 2 Particles, YH 2 The nano-Ti-YO reinforcement phase formed by in-situ reaction during the preparation process is distributed inside the grains.