Submerged-arc welding method for super-thick ocean engineering steel

By using submerged arc welding method and heat treatment technology with single-sided asymmetric K-shaped bevel on marine engineering steel, the problems of high welding difficulty and poor joint performance of super-thick marine steel are solved, and the high strength and high welded joints are achieved Toughness, suitable for 120~180mm thick 500MPa ultra-high strength offshore steel.

CN118905393APending Publication Date: 2024-11-08NANJING IRON & STEEL CO LTD

Patent Information

Application Number
CN202410804443.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art cannot effectively weld ultra-high strength marine engineering steel with a thickness of 120~180mm, resulting in poor mechanical properties of the welded joints and difficult to meet the requirements of marine steel.

Method used

The submerged arc welding method is adopted with a single-sided asymmetric K-shaped bevel. The welding speed is 29~39cm/min, the arc voltage is 27~35V, the welding current is 410~560A, and the welding heat input is 17~40kJ/cm. After welding, Perform heat treatment from 300℃~400℃, and use specific components of welding wire and steel plate materials to ensure the comprehensive mechanical properties of the welded joints.

Benefits of technology

The welded joints with 120~180mm thick 500MPa ultra-high strength marine steel have excellent comprehensive mechanical properties, including high tensile strength and low temperature impact work, filling the gap in the existing technology, and the performance of the welded joints is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a submerged-arc welding method of super-thick steel for ocean engineering, which comprises the following steps: welding a welding wire on an ultrahigh-strength steel plate by adopting a submerged-arc welding method, and the thickness of the steel plate is 120-180mm; the groove is a single-sided asymmetric K-shaped groove, the angle of an upper groove is 40-45 degrees, the angle of a lower groove is 45-50 degrees, and the size of a truncated edge is 5-6 mm; the welding position of submerged-arc welding is flat welding, the preheating temperature before welding is larger than or equal to 200 DEG C, the interlayer temperature is 130-200 DEG C, and back gouging treatment needs to be conducted before back face welding; the welding speed is 29-39 cm / min, the arc voltage is 27-35 V, the welding current is 410-560 A, and the welding heat input is 17-40 kJ / cm; and heat treatment is carried out at the temperature of 300-400 DEG C after welding, and the heating rate is 2.0-2.5 T / min. The welding method has the advantages that the comprehensive mechanical property of a welding joint is excellent, and the welding method is suitable for welding 500 MPa ultrahigh-strength maritime work steel with the thickness of 120-180mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel production, and in particular relates to a submerged arc welding method for ultra-thick marine engineering steel. Background Art

[0002] Ultra-high-strength marine engineering steel is usually used in key welded structural parts of large marine components such as marine platforms, offshore cryogenic structures, and large ships, including pile legs, pile shoes, cantilever beams, rack lifting mechanisms, etc. of self-elevating platforms. However, the development of ultra-thick steel plates is difficult, and ultra-high-strength ship plates bring a series of welding problems. Generally speaking, the higher the strength of the welded joint, the worse the toughness. The control level of each link in the production process determines the actual performance of welding. Especially for the thickness of 120~180mm, the welding is more difficult. The existing welding process cannot meet the welding requirements of ultra-thick marine steel, and the mechanical properties of the welded joint are poor. Summary of the invention

[0003] The purpose of the present invention is to solve the problems of limited welding thickness, great welding difficulty and poor performance of welded joints of existing marine engineering steel, and to provide a submerged arc welding method for ultra-thick marine engineering steel, so that the welded joint has excellent comprehensive mechanical properties, which is suitable for welding of 120~180mm thick 500MPa ultra-high strength marine engineering steel.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions: A submerged arc welding method for ultra-thick marine engineering steel, specifically comprising: (1) The welding wire is welded on the ultra-high strength steel plate by submerged arc welding, and the thickness of the steel plate is 120~180mm; (2) The groove form is a single-sided asymmetric K-type groove, the upper groove angle is 40-45°, the lower groove angle is 45-50°, and the blunt edge size is 5-6 mm; (3) The welding position of submerged arc welding is flat welding, the preheating temperature before welding is ≥200℃, the interlayer temperature is 130℃~200℃, and the root cleaning is required before welding on the reverse side; (4) The welding speed is 29~39cm / min, the arc voltage is 27~35V, the welding current is 410~560A, and the welding heat input is 17~40kJ / cm; (5) Heat treatment is performed after welding at a temperature of 300°C to 400°C with a heating rate of 2.0 to 2.5 T / min, where T is the thickness of the steel plate, to complete the welding process.

[0005] Furthermore, the ultra-high strength steel plate includes the following components in weight percentage: C: 0.07%~0.17%, Si≤0.50%, Mn≤1.60%, Ni≤2.70%, Mo≤0.60%, Cu≤0.50%, P≤0.010%, S≤0.002%, B≤0.0030%, and the balance is Fe and unavoidable impurities.

[0006] Furthermore, the yield strength of the ultra-high strength steel plate is ≥500MPa, the tensile strength is ≥590MPa, the elongation is ≥17%, and the -60°C impact energy KV2 is ≥33J.

[0007] Furthermore, the welding wire comprises the following components in weight percentage: C: 0.02%~0.15%, Mn: 2.8%~5.0%, Si: 0.22%~0.45%, S≤0.01%, P≤0.02%, Ni: 3.2%~5.8%, Cr: 0.30%~0.60%, Mo: 0.48%~0.79%, V≤0.01%, and the balance is Fe and unavoidable impurities.

[0008] Furthermore, the diameter of the welding wire is 3.2 mm, and the tensile strength of the welding wire is ≥590 MPa.

[0009] Furthermore, when selecting welding materials, we must first ensure that the weld and heat-affected zone of the welding joint have a -60°C low-temperature impact energy KV2≥33J at the 1 / 4 and 1 / 2 positions in the thickness direction, the side bending of the welding joint is d=4a, 180°, there is no crack, and the strength of the weld metal matches that of the parent material, and select appropriate welding wire.

[0010] Furthermore, in step (4), the welding speed is 38 cm / min, the arc voltage is 28 V, the welding current is 420 A, and the welding heat input is 18 kJ / cm.

[0011] Furthermore, in step (4), the welding speed is 34 cm / min, the arc voltage is 31 V, the welding current is 480 A, and the welding heat input is 26 kJ / cm.

[0012] Furthermore, in step (4), the welding speed is 30 cm / min, the arc voltage is 34 V, the welding current is 550 A, and the welding heat input is 37 kJ / cm.

[0013] In the technical solution of the present invention, by adopting the gas shielded welding process, the operation is simple, and the low-temperature impact energy KV2 of the weld seam and the heat-affected zone of the welding joint can be guaranteed to be ≥33J at the 1 / 4 and 1 / 2 positions in the thickness direction at -60°C, the tensile strength of the welding joint is ≥590MPa, the side bending d=4a, 180°, and there is no crack in the welding joint. The welding joint formed by this welding process has excellent comprehensive mechanical properties and is suitable for welding of 120~180mm thick 500MPa ultra-high strength marine steel, filling the gap in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram of the welding groove of the present invention. DETAILED DESCRIPTION Example 1

[0015] To make the present invention more clear, the submerged arc welding method of an ultra-thick marine engineering steel of the present invention is further described below in conjunction with the accompanying drawings. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0016] This embodiment is applicable to the submerged arc welding method of 120~180mm thick 500MPa ultra-high strength marine steel, and specifically includes the following steps: The steel plate properties are yield strength ≥ 500MPa, tensile strength ≥ 590MPa, elongation ≥ 17%, -60℃ impact energy KV2 ≥ 33J. It is an excellent 120mm thick 500MPa grade ultra-high strength steel. The welding test plate combination is 120mm+120mm, and the test plate size is thickness*width*length, which is 120mm*250mm*700mm.

[0017] Matching welding material composition: C: 0.02%~0.15%, Mn: 2.8%~5.0%, Si: 0.22%~0.45%, S≤0.01%, P≤0.02%, Ni: 3.2%~5.8%, Cr: 0.30%~0.60%, Mo: 0.48%~0.79%, V≤0.01%, the balance is Fe and unavoidable impurities.

[0018] The diameter of the welding wire is Φ3.2mm.

[0019] The groove form is a single-sided asymmetric K-type groove, the upper groove angle is 40-45°, the lower groove angle is 45-50°, and the blunt edge size is 5-6mm. Figure 1 As shown, a is the blunt edge size and T is the thickness of the steel plate.

[0020] The preheating temperature is 200℃, the interlayer temperature is 130℃~200℃, and the back side needs to be root cleaned before welding.

[0021] The welding speed was 38 cm / min, the arc voltage was 28 V, the welding current was 420 A, and the welding heat input was 18 kJ / cm.

[0022] Immediately after welding, heat treatment at 330℃*2*120 min is performed to complete the welding. Example 2

[0023] This embodiment is applicable to the submerged arc welding method of 120-180 mm thick 500 MPa ultra-high strength marine steel, and specifically includes the following steps: The steel plate properties are yield strength ≥500MPa, tensile strength ≥590MPa, elongation ≥17%, -60℃ impact energy KV2 ≥33J. It is an excellent 160mm thick 500MPa grade ultra-high strength steel. The welding test plate combination is 160mm+160mm, and the test plate size is thickness*width*length, which is 160mm*250mm*700mm.

[0024] Matching welding material composition: C: 0.02%~0.15%, Mn: 2.8%~5.0%, Si: 0.22%~0.45%, S≤0.01%, P≤0.02%, Ni: 3.2%~5.8%, Cr: 0.30%~0.60%, Mo: 0.48%~0.79%, V≤0.01%, the balance is Fe and unavoidable impurities.

[0025] The diameter of the welding wire is Φ3.2mm.

[0026] The groove form is a single-sided asymmetric K-type groove, the upper groove angle is 40-45°, the lower groove angle is 45-50°, and the blunt edge size is 5-6mm.

[0027] The preheating temperature before welding is 200℃, the interlayer temperature is 130℃-200℃, and the back side needs to be root cleaned before welding.

[0028] The welding speed was 34 cm / min, the arc voltage was 31 V, the welding current was 480 A, and the welding heat input was 26 kJ / cm.

[0029] Immediately after welding, heat treatment at 330℃*2.2*160 min is performed to complete the welding. Example 3

[0030] This embodiment is applicable to the submerged arc welding method of 120-180 mm thick 500 MPa ultra-high strength marine steel, and specifically includes the following steps: The steel plate properties are yield strength ≥500MPa, tensile strength ≥590MPa, elongation ≥17%, -60℃ impact energy KV2 ≥33J. It is an excellent 180mm thick 500MPa grade ultra-high strength steel. The welding test plate combination is 180mm+180mm, and the test plate size is thickness*width*length, which is 180mm*250mm*700mm.

[0031] Matching welding material composition: C: 0.02%~0.15%, Mn: 2.8%~5.0%, Si: 0.22%~0.45%, S≤0.01%, P≤0.02%, Ni: 3.2%~5.8%, Cr: 0.30%~0.60%, Mo: 0.48%~0.79%, V≤0.01%, the balance is Fe and unavoidable impurities.

[0032] The diameter of the welding wire is Φ3.2mm.

[0033] The groove form is a single-sided asymmetric K-type groove, the upper groove angle is 40-45°, the lower groove angle is 45-50°, and the blunt edge size is 5-6mm.

[0034] The preheating temperature before welding is 200℃, the interlayer temperature is 130℃-200℃, and the back side needs to be root cleaned before welding.

[0035] The welding speed was 30 cm / min, the arc voltage was 34 V, the welding current was 550 A, and the welding heat input was 37 kJ / cm.

[0036] Immediately after welding, heat treatment at 330℃*2.5*200 min is performed to complete the welding.

[0037] After the 120-180 mm thick 500 MPa ultra-high strength marine steel was welded by gas shielded welding using the welding methods of the above-mentioned Examples 1-3, the mechanical properties of the welded joints are shown in the following table. The impact, tensile and bending properties of the welded joints are shown in Table 1:

[0038] It can be seen that the comprehensive mechanical properties of the welded joints obtained in Examples 1 to 3 are excellent. The impact energy KV2 at -60°C at 1 / 4 and 1 / 2 positions in the thickness direction of the weld and heat-affected zone is ≥33J, the tensile strength Rm is ≥590MPa, and the side bending d=4a of the welded joint is qualified at 180°. In addition, the process implementation method provided by this patent is simple and has strong applicability.

[0039] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A submerged arc welding method for ultra-thick marine engineering steel, characterized in that: (1) The welding wire is welded on the ultra-high strength steel plate by submerged arc welding, and the thickness of the steel plate is 120~180mm; (2) The groove form is a single-sided asymmetric K-type groove, the upper groove angle is 40-45°, the lower groove angle is 45-50°, and the blunt edge size is 5-6 mm; (3) The welding position of submerged arc welding is flat welding, the preheating temperature before welding is ≥200℃, the interlayer temperature is 130℃~200℃, and the root cleaning is required before welding on the reverse side; (4) The welding speed is 29~39cm / min, the arc voltage is 27~35V, the welding current is 410~560A, and the welding heat input is 17~40kJ / cm; (5) Heat treatment is performed after welding at a temperature of 300°C to 400°C with a heating rate of 2.0 to 2.5 T / min, where T is the thickness of the steel plate, to complete the welding process.

2. The submerged arc welding method for ultra-thick marine engineering steel according to claim 1, characterized in that: The ultra-high strength steel plate includes the following components in weight percentage: C: 0.07%~0.17%, Si≤0.50%, Mn≤1.60%, Ni≤2.70%, Mo≤0.60%, Cu≤0.50%, P≤0.010%, S≤0.002%, B≤0.0030%, and the balance is Fe and unavoidable impurities.

3. The submerged arc welding method for ultra-thick marine engineering steel according to claim 2, characterized in that: The yield strength of the ultra-high strength steel plate is ≥500MPa, the tensile strength is ≥590MPa, the elongation is ≥17%, and the impact energy KV2 at -60°C is ≥33J.

4. The submerged arc welding method for ultra-thick marine engineering steel according to any one of claims 1 to 3, characterized in that: The welding wire comprises the following components in weight percentage: C: 0.02%~0.15%, Mn: 2.8%~5.0%, Si: 0.22%~0.45%, S≤0.01%, P≤0.02%, Ni: 3.2%~5.8%, Cr: 0.30%~0.60%, Mo: 0.48%~0.79%, V≤0.01%, and the balance is Fe and unavoidable impurities.

5. The submerged arc welding method for ultra-thick marine engineering steel according to claim 4, characterized in that: The diameter of the welding wire is 3.2 mm, and the tensile strength of the welding wire is ≥590 MPa.

6. The submerged arc welding method for ultra-thick marine engineering steel according to claim 4, characterized in that: When selecting welding materials, we must first ensure that the weld and heat-affected zone of the welding joint, the -60℃ low-temperature impact energy KV2≥33J at the 1 / 4 and 1 / 2 positions in the thickness direction, the side bending d=4a, 180°, no cracks, and the strength of the weld metal matches the parent material, and select suitable welding wire.

7. The submerged arc welding method for ultra-thick marine engineering steel according to any one of claims 1 to 3, characterized in that: In the step (4), the welding speed is 38 cm / min, the arc voltage is 28 V, the welding current is 420 A, and the welding heat input is 18 kJ / cm.

8. The submerged arc welding method for ultra-thick marine engineering steel according to any one of claims 1 to 3, characterized in that: In the step (4), the welding speed is 34 cm / min, the arc voltage is 31 V, the welding current is 480 A, and the welding heat input is 26 kJ / cm.

9. The submerged arc welding method for ultra-thick marine engineering steel according to any one of claims 1 to 3, characterized in that: In the step (4), the welding speed is 30 cm / min, the arc voltage is 34 V, the welding current is 550 A, and the welding heat input is 37 kJ / cm.

Citation Information

Patent Citations

  • A submerged arc welding method of 5ni steel for shipbuilding

    CA3189684A1

  • Submerged arc welding process for E36 oceaneering steel with thickness being 80mm

    CN102873439A

  • Submerged arc welding method for K-shaped groove of 80mm extra-thick steel plate with excellent plate shape after welding

    CN102922103A

  • Submerged-arc welding process for ocean engineering steel plate in low-temperature environment

    CN117381111A

  • Submerged-arc welding process for 980MPa-grade ultrahigh-strength steel with thickness of 80-130mm

    CN117444363A

Cited By

  • Welding process for large and thick ultrahigh-strength steel plate of offshore wind power pipe pile

    CN122164982A