Laser filler wire welding device and welding method of tube plate lap joint structure

By using a forward push-type laser welding torch and an adjustable wire feeding mechanism in the laser wire fill welding device, the problem of the gas outlet of the welding torch cannot float in time is solved, and welds without pore defects are achieved, and welding efficiency and surface quality are improved.

CN118905425APending Publication Date: 2024-11-08CRRC QINGDAO SIFANG CO LTD

Patent Information

Application Number
CN202411066104.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Handheld laser wire filler welding torch often has weld hole defects during the pretreatment and welding of bogie beams, mainly because the protective gas at the outlet of the welding torch is easily blown into the inside of the molten pool, resulting in the gas not floating out in time, resulting in condensation and internal air holes in the weld. question.

Method used

The front push-type laser welding torch is adopted. The welding wire extends from the front of the welding torch into the molten pool. The welding molten pool is in front of the handheld laser welding torch. The relative position of the wire feeding nozzle and the welding torch is adjusted through an adjustable mechanism to ensure that the protective gas energy floats out in time and achieve no Welds with air hole defects.

Benefits of technology

It effectively avoids pore defects inside the weld, and the surface of the weld is bright and clean after welding is completed, reducing manual cleaning time and cost and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905425A_ABST
    Figure CN118905425A_ABST
Patent Text Reader

Abstract

The invention firstly provides a laser wire filling welding device which comprises a forward pushing type laser welding gun and a wire feeding mechanism, the wire feeding mechanism comprises a wire feeding nozzle, and when the welding gun is pushed to advance for welding, a welding wire extends into a laser welding pool through the wire feeding nozzle on the front side of the welding direction. The invention further provides a welding method of the tube plate lap joint structure. According to the laser wire filling welding device and the welding method of the tube plate lap joint structure, the forward pushing type laser welding gun is adopted, the welding wire extends into the welding pool from the front side of the advancing direction of the welding gun, the welding pool is located in front of the handheld laser welding gun, and a welding seam generated by new condensation is located behind the handheld laser wire filling welding gun; the problems that protective gas at an outlet of a welding gun is easily obliquely blown into a laser welding pool and cannot emerge out of the surface in time when a welding seam is cooled are solved, the protective gas cannot appear in the welding seam generated by new condensation, and then the effect that no pore defect exists in the welding seam is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, in particular to a laser wire-filling welding device and a welding method for a tube-sheet overlap structure. Background Art

[0002] In the process of using hand-held laser wire-filling welding guns currently available on the market to perform pretreatment welding of bogie crossbeams, there is a problem of porosity defects in the weld. There is currently no good solution, mainly because the current hand-held laser wire-filling welding guns all have the welding wire behind the laser welding gun, with the laser on top and the welding wire at the bottom, and a back-pull welding method. The welding molten pool is in front of the hand-held laser wire-filling welding gun, and the shielding gas at the welding gun outlet can easily be blown obliquely into the laser welding molten pool; due to the concentrated laser welding energy and the large depth-to-width ratio of the molten pool; the hand-held laser wire-filling welding molten pool cools down quickly, and the shielding gas cannot float to the surface of the molten pool in time, so that the shielding gas remains inside the newly condensed weld in front of the laser welding gun, forming porosity defects inside the weld.

[0003] In the prior art, similar problems exist when using a handheld laser welding gun for back-pull welding for tube-sheet overlap structures such as bogie crossbeam pretreatment or other structures that require laser wire welding. Summary of the invention

[0004] The main purpose of the present invention is to solve the above-mentioned problems and shortcomings, and to provide a laser wire-filling welding device and a welding method for a tube-sheet overlap structure. A forward-push laser welding gun is adopted, and the welding wire extends into the welding molten pool from the front side of the welding gun in the forward direction. The welding molten pool is in front of the handheld laser welding gun, and the newly condensed weld is behind the handheld laser wire-filling welding gun. This solves the problem that the shielding gas at the welding gun outlet is easily blown obliquely into the laser welding molten pool, and the shielding gas cannot float to the surface in time when the weld is cooled, so that the shielding gas will not appear in the newly condensed weld, thereby achieving the effect of no pore defects inside the weld.

[0005] To achieve the purpose of the invention, the present invention first provides a laser line filling welding device, which adopts the following technical solution:

[0006] A laser wire-filling welding device comprises a handheld forward-pushing laser welding gun and a wire feeding mechanism, wherein the wire feeding mechanism comprises a wire feeding nozzle and a wire feeding tube. When the welding gun is pushed forward for welding, the welding wire extends through the wire feeding nozzle into the laser welding molten pool at the front side of the welding direction.

[0007] Furthermore, the wire feeding mechanism is assembled and connected to the welding gun via an adjustable mechanism, and the adjustable mechanism can adjust the relative position of the wire feeding nozzle and the welding gun.

[0008] Furthermore, the adjustable mechanism includes an adjustment slideway provided on the welding gun and an angle adjustment block provided on the wire feeding mechanism, and the angle adjustment block is slidably connected to the adjustment slideway.

[0009] Furthermore, the adjustable mechanism also includes a length adjustment mechanism for adjusting the extension length of the welding wire.

[0010] Furthermore, it also includes a positioning device for maintaining the stability of the welding gun during the welding process.

[0011] Furthermore, the positioning device includes a positioning rod and a positioning wheel, one end of the positioning rod is fixed to the welding gun, and the other end is fixed to the positioning wheel.

[0012] The second invention object of the present invention is to provide a welding method for a tube sheet overlap structure, which adopts the following technical solution:

[0013] A welding method for a tube-sheet overlap structure uses the aforementioned laser wire-filling welding device to perform wire-filling primer pretreatment during the welding process, and then performs robot welding after the primer pretreatment.

[0014] Furthermore, the proportional relationship between wire feeding speed and welding speed is related to the wire diameter and weld size.

[0015] Furthermore, the angle between the laser emitted by the laser welding gun and the ground is 45°~70°; the angle between the welding wire and the laser is 20°~65°; the laser spot diameter is 0.8mm, the welding wire diameter is 1.2mm, and the defocus amount is -1mm~+1mm; the scanning width is in the range of 0~6mm, the peak power is 1800W, the wire feeding speed is 35cm / min, the welding speed is 5mm / s~6mm / s, the welding shielding gas is 80% Ar and 20% CO2, and the welding shielding gas flow rate is 16L / min~18L / min.

[0016] Furthermore, after the laser wire-filling welding device performs the wire-filling base pretreatment welding, before the robot welding, a small current robot rapid base welding is also performed.

[0017] In summary, the laser wire-filling welding device and the welding method of the tube-sheet structure provided by the present invention have the following technical advantages compared with the prior art:

[0018] Because the forward-push laser welding technology with the welding wire in front of the laser welding gun is adopted, the welding pool is in front of the handheld laser wire-filling welding gun, and the newly condensed weld is behind the handheld laser wire-filling welding gun. Therefore, the problem that the shielding gas at the welding gun outlet is easily blown obliquely into the laser welding pool and the shielding gas cannot float to the surface in time when the weld is cooled is solved, so that the shielding gas will not appear in the newly condensed weld, thereby achieving the effect of no porosity defects in the weld.

[0019] The handheld laser wire filling primer pretreatment welding + robot welding process replaces the manual MAG primer pretreatment welding + robot welding process, which can achieve smaller displacement deformation after the beam welding is completed, bright and clean weld surface, and no surface cleaning is required, reducing manual labor and weld cleaning time, saving manpower costs, and improving the production efficiency of the beam welding process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 : A laser wire-filling welding device provided by the present invention;

[0021] Figure 2 : A schematic diagram of a welding pool in a tube-sheet overlap structure welding method provided by the present invention;

[0022] Figure 3 : Figure 2 Enlarged view of section A.

[0023] Figure 4 : Macroscopic metallographic structure of the weld after welding in a tube-sheet overlap structure welding method provided by the present invention;

[0024] Among them, 1. wire feeding tube; 2. welding gun switch; 3. laser welding gun; 4. welding gun light outlet tube; 5. positioning wheel; 6. positioning rod; 7. welding wire; 8. wire feeding nozzle; 9. wire feeding nozzle length adjustment knob; 10. adjustment slide; 11. wire feeding nozzle angle adjustment block; 12. laser beam; 13. welding wire; 14. welding direction; 15. test plate; 16. welding molten pool; α-the angle between the laser and the ground; β-the angle between the welding wire and the laser.

[0025] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.

[0027] In the description of the present invention, it should be noted that the directions or positional relationships indicated by terms such as “upper”, “lower”, “front”, “back”, “left”, “right”, “vertical”, “inside” and “outside” are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0028] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0029] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0030] The present invention first provides a laser wire-filling welding device, including a handheld forward-pushing laser welding gun and a wire feeding mechanism, wherein the wire feeding mechanism includes a wire feeding nozzle. When the welding gun is pushed forward for welding, the welding wire extends through the wire feeding nozzle to the laser welding molten pool 16 on the front side of the welding direction.

[0031] The laser wire welding device provided by the present invention comprises a handheld forward-pushing laser welding gun 3, which can emit a welding laser to form a welding molten pool 16 at the welding position. Figure 1 As shown, the welding gun 3 includes a welding gun handle and a welding gun light outlet tube 4. The welding gun handle is generally in the shape of "7", including a transverse ( Figure 1 The welding gun comprises a holding portion (in the direction shown) and a fixing portion arranged to be tilted downward, and a welding gun switch 2 is arranged at the holding portion. During the welding process, the operator holds the holding portion. Further, the welding gun tip 2 is arranged at the lower side of the holding portion. When holding, the state of the welding gun switch 2 can be controlled by fingers to control the output and shutdown of the laser.

[0032] The front end of the grip ( Figure 1 The left side in the figure is the front) and is fixed to the upper part or the top of the fixing part, so that the gripping part and the fixing part form a structure similar to a "7" shape. Figure 1 As shown, the front end of the gripping portion is fixed to the right end surface of the upper portion of the fixing portion. Preferably, the fixing position and the fixing angle are adjustable to adapt to different welding structures.

[0033] At the bottom of the fixed part, a welding gun light outlet tube 4 is provided, and the welding gun 3 can emit a laser beam 12 to form a welding molten pool at the part to be welded. Figure 1 As shown, a welding gun light emitting tube 4 is provided at the bottom of the fixed part, and a thread is provided at the lower part of the welding gun light emitting tube 4, so that the welding gun light emitting tube 4 is threadedly connected to the welding gun handle, and the vertical distance between the welding gun light emitting tube 4 and the holding part can be adjusted through the thread, that is, the fixed height of the welding gun light emitting tube 4 is adjusted.

[0034] A positioning device is provided at the side end of the lower part of the fixing part, which plays a role in positioning the welding height and welding position when the hand welding gun is performing welding operations. Figure 1As shown, the positioning device includes a positioning rod 6 and a positioning wheel 5. One end of the positioning rod 6 is assembled and fixed to the side of the welding light emitting tube 4 at an angle, so that the positioning rod 6 is arranged on the rear side of the forward direction of the welding light emitting tube 4, and the other end is connected to the positioning wheel through a bearing. The positioning wheel 5 can rotate around the bearing. When pushed forward, the positioning wheel plays a role in positioning the welding height and welding position of the handheld laser welding device.

[0035] The welding device further includes a wire feeding mechanism. In this embodiment, the wire feeding mechanism is fixed to the front side of the welding gun 3. Specifically, the wire feeding mechanism is fixed to the front side of the fixed part. The wire feeding mechanism includes a wire feeding nozzle 8 and a wire feeding tube 1. The wire feeding tube 1 extends from the top of the welding gun 3 to the front side. The wire feeding nozzle 8 is threadedly connected to the end of the wire feeding tube 1. When the welding gun 3 is pushed forward for welding, the welding wire extends from the front side of the welding direction through the welding wire tube 1 and the wire feeding nozzle 8 to the laser welding molten pool 16. The wire feeding nozzle 8 is located at the front side of the welding light output tube 4, and the welding wire extends backward from the front side of the laser beam 12 into the welding molten pool 16.

[0036] The wire feeding tube 1 can be directly fixed to the front side of the welding gun 3. In the present embodiment, the wire feeding mechanism is fixed to the front side of the fixed part of the welding gun 3 by an adjustable mechanism. The adjustable mechanism is used to adjust the relative position between the wire feeding nozzle 8 and the welding gun 3, including but not limited to the relative angle between the wire feeding nozzle 8 and the welding light output tube 4, the longitudinal relative height and / or the extension length of the welding wire.

[0037] The adjustment mechanism includes a wire feed nozzle angle adjustment slide 10, such as Figure 1 As shown, the adjustment slide 10 is an arc-shaped structure, extending from the fixed position with the fixing part in the forward direction, and bending downward in an arc shape toward the wire feeding nozzle 8. The wire feeding tube 8 is provided with a wire feeding nozzle angle adjustment block 11, and the wire feeding nozzle angle adjustment block 11 is slidably connected with the adjustment slide 10, so as to adjust the relative angle between the wire feeding nozzle 8 and the welding gun light outlet tube 4. The end of the wire feeding tube 1 is threadedly connected with the top of the wire feeding nozzle angle adjustment block 11.

[0038] Furthermore, the wire feeding nozzle angle adjustment block 11 is provided with a fastening structure. After being adjusted to the set angle, the fastening structure is used to fasten the relative position between the wire feeding nozzle angle adjustment block 11 and the adjustment slide 10 to prevent movement during welding and change the relative angle between the wire feeding nozzle 8 and the welding gun light output tube 4.

[0039] The adjustable mechanism also includes a length adjustment mechanism that can adjust the length of the welding wire extending out of the wire feeding nozzle. Figure 1As shown, a length adjustment mechanism is provided at the lower end of the wire feeding nozzle angle adjustment block 11, and the lower end of the length adjustment mechanism is assembled and connected to the wire feeding nozzle 8. A through hole is provided between the wire feeding nozzle angle adjustment block 11, the length adjustment mechanism and the wire feeding nozzle 8. The welding wire passes through the through hole and finally extends from the front end of the wire feeding nozzle 8, and the extension length of the welding wire is adjusted by the length adjustment mechanism. In this embodiment, the length adjustment mechanism includes a wire feeding nozzle length adjustment knob 9, and the extension length of the welding wire is adjusted by the wire feeding nozzle length adjustment knob 9, thereby adjusting the extension length of the welding wire relative to the welding gun 3, that is, by adjusting the extension length of the welding wire, the longitudinal relative height or relative position between the end of the welding wire and the front end of the welding gun light outlet tube 4 is adjusted.

[0040] like Figure 1 As shown, the wire feeding nozzle angle adjustment block 11 is connected to the wire feeding nozzle length adjustment knob 9 through bolt threaded contact, and the wire feeding nozzle 8 is assembled and connected below the wire feeding nozzle length adjustment knob 9. Preferably, the wire feeding nozzle 8 is threadedly connected to the lower end of the wire feeding nozzle length adjustment knob 9, and the wire feeding nozzle 8 and the wire feeding nozzle length adjustment knob 9 cooperate with each other to adjust the dry extension length of the welding wire.

[0041] The present invention further provides a method for welding a tube-sheet overlap structure using the welding device described above. The welding method for the tube-sheet overlap structure provided in this embodiment is applied in the base pretreatment welding process of the overlap welding of the beam steel pipe and the flat plate with a 30° to 50° V-shaped groove. At the same time, it is also applicable to structures such as flat plate butt welding and tube-sheet butt annular welding. There are no restrictions on the size and angle of the groove. In the discussion of this article, it is collectively referred to as the welding of the tube-sheet overlap structure, which cannot be regarded as a limitation on the welding method provided in this application.

[0042] Taking the crossbeam welding process of bogie assembly as an example, the welding device described above is used to perform base pretreatment welding on the crossbeam, and mechanical welding is performed after pretreatment welding. During the welding process, the positioning wheel 5 of the laser wire filling welding device described above is placed above the parts to be welded, the grip is held, and the welding gun switch 2 is pressed. The laser is emitted from the welding gun light outlet tube 4, hitting the surface of the parts to be welded and forming a molten pool; at the same time, the welding wire passes through the wire feeding tube 1, the wire feeding nozzle angle adjustment block 11, the wire feeding nozzle length adjustment knob 9, and the wire feeding nozzle 8 to extend into the laser welding molten pool 16, and at the same time, the laser welding gun 3 is pushed forward to form a new welding molten pool 16 in front of the welding gun 3, and a new weld is formed behind the welding gun.

[0043] After the handheld laser wire filling primer pretreatment welding is completed, the beam is transferred to the robot welding station for robot welding. In the welding method provided in this embodiment, a new small current fast primer welding is added in front of the original robot welding process, so that the size of the laser wire filling pretreatment weld plus the new robot primer weld is equal to the size of the manual MAG primer pretreatment weld, thereby completing the robot welding process of the beam without changing the subsequent original robot welding process parameters.

[0044] When the laser wire-filling root welding is performed using the welding device described above, the process parameters used in the welding process include but are not limited to: Figure 2 and Figure 3 As shown, the angle α between the laser beam 12 emitted by the laser welding gun 3 and the ground is 45°~70°; the angle β between the welding wire 13 and the laser beam 12 is 20°~65°, and the handheld welder advances the welding along the welding direction 14; the laser spot diameter is 0.8mm, the welding wire diameter is 1.2mm, and the defocus amount is -1mm~+1mm; the scanning width is within the range of 0~6mm, such as 5mm, the peak power is 1800W, the wire feeding speed is 35cm / min, the welding speed is 5mm / s~6mm / s, and the proportional relationship between the wire feeding speed and the welding speed is related to the wire diameter and the weld size; the welding shielding gas is 80% Ar and 20% CO2, and the welding shielding gas flow rate is 16L / min~18L / min.

[0045] This technology is also applicable to structures such as flat plate butt welding and tube-sheet butt ring welding, and there are no restrictions on the size and angle of the groove. The welding parameters described above are applicable to the parameter control of the bottom welding of the bogie crossbeam. For parts with different welding groove forms, the method of changing the size of the welding parameters can be adopted to achieve laser wire welding. By changing the size of the laser peak power, adjusting the scanning width of the laser, and changing the depth and width of the welding pool 16. Increasing the laser power, reducing the welding speed, and increasing the scanning width can achieve increasing the cladding metal at the groove and increasing the size of the weld.

[0046] During the welding process, the laser beam 12 is irradiated on the surface of the parts to be welded. Figure 2 The material of the test plate 15 reaches the melting point instantly, and the material to be welded will evaporate rapidly. The metal vapor pressure and vapor reaction force can overcome the surface tension of the molten metal and the static pressure of the liquid metal to form a small hole. The small hole is similar to a black body, which helps to absorb the energy of the beam. At the same time, the welding wire is melted into the molten pool after contacting the laser beam. The laser beam pushes forward relative to the parts to be welded, and the small hole near the surface molten pool forms a Figure 2 The vortex shown in the figure, the gas inside the small hole floats to the surface of the molten pool along with the vortex, the temperature of the liquid metal behind the small hole decreases, and it cools quickly to form Figure 4Weld shown.

[0047] Compared with the currently used MAG welding, the laser wire-filling welding device and the welding method of the tube-sheet overlap structure provided by the present invention have a large molten pool depth-to-width ratio, low line energy, no porosity defects in the weld, and small displacement deformation of the parts after welding. The welding deformation of the parts can be better controlled, and the cost of later adjustment and repair of the parts can be reduced. The weld surface of the handheld laser wire-filling welding is bright and clean after completion, and no surface cleaning is required, saving man-hour costs. The handheld laser wire-filling welding is simple to operate and easy to master, which reduces the difficulty for welding personnel to get started.

[0048] By adding a new low-current rapid rooting weld in front of the original robot welding process, the size of the laser wire pretreatment weld plus the robot's new rooting weld is equal to the size of the manual MAG rooting pretreatment weld, and the robot welding process is completed without changing the subsequent original robot welding process parameters. The welding process parameters of the new robot low-current rapid rooting weld are welding voltage 24±2V, welding current 190±2A, wire diameter 1.2mm, and welding speed 8±0.5mm / s.

[0049] In summary, the laser wire-filling welding device and the welding method of the tube-sheet structure provided by the present invention have the following technical advantages compared with the prior art:

[0050] Because the forward-push laser welding technology with the welding wire in front of the laser welding gun is adopted, the welding pool is in front of the handheld laser wire-filling welding gun, and the newly condensed weld is behind the handheld laser wire-filling welding gun. Therefore, the problem that the shielding gas at the welding gun outlet is easily blown obliquely into the laser welding pool and the shielding gas cannot float to the surface in time when the weld is cooled is solved, so that the shielding gas will not appear in the newly condensed weld, thereby achieving the effect of no porosity defects in the weld.

[0051] The handheld laser wire filling primer pretreatment welding + robot welding process replaces the manual MAG primer pretreatment welding + robot welding process, which can achieve smaller displacement deformation after the beam welding is completed, bright and clean weld surface, and no surface cleaning is required, reducing manual labor and weld cleaning time, saving manpower costs, and improving the production efficiency of the beam welding process.

[0052] As described above, similar technical solutions can be derived from the given solution content. However, any simple modification, equivalent changes and modifications made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A laser wire welding device, characterized in that: It comprises a handheld forward-pushing laser welding gun and a wire feeding mechanism, wherein the wire feeding mechanism comprises a wire feeding nozzle and a wire feeding tube. When the welding gun is pushed forward for welding, the welding wire extends through the wire feeding nozzle to the laser welding molten pool at the front side of the welding direction.

2. A laser wire welding device as claimed in claim 1, characterized in that: The wire feeding mechanism is assembled and connected with the welding gun through an adjustable mechanism, and the adjustable mechanism can adjust the relative position of the wire feeding nozzle and the welding gun.

3. A laser wire welding device as claimed in claim 2, characterized in that: The adjustable mechanism comprises an adjusting slideway arranged on the welding gun and an angle adjusting block arranged on the wire feeding mechanism, and the angle adjusting block is slidably connected to the adjusting slideway.

4. A laser wire welding device as claimed in claim 2, characterized in that: The adjustable mechanism also includes a length adjustment mechanism for adjusting the extension length of the welding wire.

5. A laser welding device with filler wire according to any one of claims 1 to 4, characterized in that: It also includes a positioning device to maintain the welding gun stable during the welding process.

6. A laser wire welding device as claimed in claim 5, characterized in that: The positioning device comprises a positioning rod and a positioning wheel. One end of the positioning rod is fixed to the welding gun, and the other end is fixed to the positioning wheel.

7. A welding method for a tube sheet overlap structure, characterized in that: During the welding process, a laser wire-filling welding device as described in any one of claims 1 to 6 is used to perform wire-filling primer pretreatment, and robot welding is performed after the primer pretreatment.

8. A method for welding a tube-sheet overlap structure according to claim 7, characterized in that: The proportional relationship between wire feeding speed and welding speed is related to the wire diameter and weld size.

9. A method for welding a tube-sheet overlap structure according to claim 7, characterized in that: The angle between the laser emitted by the laser welding gun and the ground is 45°~70°; the angle between the welding wire and the laser is 20°~65°; the laser spot diameter is 0.8mm, the welding wire diameter is 1.2mm, and the defocus amount is -1mm~+1mm; the scanning width is in the range of 0~6mm, the peak power is 1800W, the wire feeding speed is 35cm / min, the welding speed is 5mm / s~6mm / s, the welding shielding gas is 80% Ar and 20% CO2, and the welding shielding gas flow rate is 16L / min~18L / min.

10. A method for welding a tube-sheet overlap structure according to any one of claims 7 to 9, characterized in that: After the laser wire-filling welding device performs the wire-filling base pretreatment welding, a small current robot rapid base welding is also performed before the robot welding.

Citation Information

Patent Citations

  • Narrow gap multi-pass laser welding method for thick plate

    CN103008895A

  • Laser-TOPTIG hybrid welding method

    CN104014933A

  • Horizontal-8-shaped mould laser welding method

    CN104308364A

  • Laser wire filing welding device and method

    CN108581201A

  • Handheld laser welding gas protection device and method

    CN116851912A

Cited By

  • Backweld method for handheld laser welding

    CN121315433A