Aluminum alloy welding method and aluminum alloy workpiece

By laser remelting the welding heat-affected zone, the local hardening zone is formed, which solves the problem of the decrease in the strength of high-strength aluminum alloy welded joints, and significantly improves the mechanical properties and durability of the welded joints.

CN118905436APending Publication Date: 2024-11-08WEIQIAO LIGHTWEIGHT RESEARCH CENTER AT SOOCHOW +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411317255.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the welding process, high-strength aluminum alloys have poor high-temperature thermal stability, resulting in softening of the welding heat-affected zone, and the strength and toughness of the welded joints have significantly decreased, limiting their application in structural parts.

Method used

The laser heat source is used to laser remelve the heat-affected zone of the welded joint to form a supersaturated remelting zone, and a local hardening zone is formed through natural aging to form a hardness gradient structure to enhance the overall strength of the welded joint.

Benefits of technology

Through laser remelting treatment, the tensile strength and toughness of the welded joints are significantly improved, the mechanical properties of the welding heat-affected zone are improved, and the overall strength and durability of the welded joints are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905436A_ABST
    Figure CN118905436A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy welding method and an aluminum alloy workpiece, and the method comprises the following steps: welding an aluminum alloy part to form a welding joint; a laser heat source is adopted for conducting laser remelting on a target area with the peak temperature ranging from 400 DEG C to 500 DEG C in the heat affected area of the welded joint, a remelting area is formed, and elements in the remelting area are in a supersaturated state; and the remelting area is naturally aged to form a local hardening area, and the local hardening area and an area which is not affected by laser form a hardness gradient structure. According to the aluminum alloy welding method and the aluminum alloy workpiece, after welding, laser remelting treatment is conducted on the specific area of the heat affected zone, a supersaturated solid solution can be formed in the local area, the remelting area is subjected to natural aging, a fine strengthening phase can be separated out, and a local hardening area is formed; a welding heat affected zone is changed into a zone with hardness gradient from an original softening zone, and the strength of a welding joint is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal processing, and in particular relates to an aluminum alloy welding method and an aluminum alloy workpiece. Background Art

[0002] The automotive industry is moving towards lightweight and energy-efficient development, especially in the field of new energy vehicles. In order to achieve the goal of reducing carbon emissions, the application of lightweight materials is becoming increasingly important. Using high-strength, heat-treatable aluminum alloy materials instead of traditional steel materials has become an effective means of reducing the weight of the vehicle body. This lightweight design can not only effectively improve the fuel efficiency of the vehicle, but also reduce carbon dioxide emissions.

[0003] However, although high-strength heat-treatable aluminum alloys have excellent specific strength and good machinability, and can significantly reduce the weight of the vehicle body, they face some technical difficulties in the welding process. In particular, under the action of welding thermal cycles, the main nano-reinforced phase in high-strength aluminum alloys will lose its strengthening effect due to poor high-temperature thermal stability. This problem leads to a significant softening effect in the heat-affected zone (HAZ) of aluminum alloy welding, which significantly reduces the mechanical properties of the welded joint and significantly deteriorates the strength.

[0004] In the existing technology, the softening problem of the heat-affected zone of welding has seriously limited the application of high-strength aluminum alloys in structural parts, especially in the field of automobile manufacturing, where the strength and toughness of welded joints are crucial to the overall performance of the vehicle body. If the strength of welded joints decreases, the performance of the entire vehicle in terms of load-bearing performance, safety and durability will be seriously affected.

[0005] Therefore, it is necessary to provide a new solution to the above technical problems. Summary of the invention

[0006] The object of the present invention is to provide an aluminum alloy welding method and an aluminum alloy workpiece, which can improve the strength and toughness of the welded joint and solve the problem of decreased joint strength caused by softening of the heat affected zone.

[0007] To achieve the above purpose, the technical solution provided by the present invention is as follows:

[0008] In a first aspect, the present invention provides an aluminum alloy welding method, comprising: welding aluminum alloy parts to form a welded joint; using a laser heat source to laser remelt a target area in a heat affected zone of the welded joint, where the peak temperature is between 400°C and 500°C, to form a remelted zone, so that the remelted zone is in an oversaturated state; the remelted zone is subjected to natural aging to form a local hardened zone, which forms a hardness gradient structure with the area not affected by the laser.

[0009] In one or more embodiments, the laser heat source is divided into two laser beams by a beam splitter, which act on the heat affected zones on both sides of the weld joint respectively.

[0010] In one or more embodiments, the parameters of the laser remelting include a laser power of 1.6-1.8 kW and a laser beam moving speed of 60-80 mm / s.

[0011] In one or more embodiments, the oscillation trajectory of the laser beam is close to a circle, the oscillation amplitude is 0.6 to 0.8 mm, and the frequency is 120 to 180 Hz.

[0012] In one or more embodiments, the remelting zone has a depth of 30-50% of the thickness of the aluminum alloy component and a width of 1-2 mm.

[0013] In one or more embodiments, the aluminum alloy component is made of a heat-treatable aluminum alloy having a yield strength greater than 300 MPa.

[0014] In one or more embodiments, the heat-treatable aluminum alloy includes a 2xxx series aluminum alloy, a 6xxx series aluminum alloy, or a 7xxx series aluminum alloy.

[0015] In one or more embodiments, the aluminum alloy component has a thickness of 2 to 4 mm.

[0016] In one or more embodiments, the method further comprises: during the welding process, using an infrared temperature measurement system to measure the peak temperature distribution of the heat affected zone of the weld joint.

[0017] In a second aspect, the present invention provides an aluminum alloy workpiece, which is welded by the aluminum alloy welding method as described in the preceding item.

[0018] Compared with the prior art, the aluminum alloy welding method and aluminum alloy workpiece provided by the present invention can form a supersaturated solid solution in the local area by performing laser remelting treatment on a specific area of ​​the heat affected zone after welding. The remelted area can precipitate fine strengthening phases through natural aging to form a local hardened zone, so that the welding heat affected zone is transformed from the original softening zone to a zone with a hardness gradient, thereby enhancing the overall strength of the weld joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0020] Figure 1 A flowchart of an aluminum alloy welding method according to an embodiment of the present invention;

[0021] Figure 2 This is a hardness distribution diagram of the heat-affected zone of a CMT welded joint in Example 1 of the present invention;

[0022] Figure 3 This is a morphology diagram of the remelting zone of the weld joint after laser treatment in Example 1 of the present invention;

[0023] Figure 4 This is a hardness distribution diagram of the heat-affected zone of the weld joint after laser treatment in Example 1 of the present invention;

[0024] Figure 5 is an engineering stress-strain curve diagram of the weld joint before and after laser treatment in Example 2 of the present invention;

[0025] Figure 6 This is a hardness surface distribution diagram of the heat-affected zone of the weld joint after laser treatment in Example 2 of the present invention;

[0026] Figure 7 This is the engineering stress-strain curve of the welded joint after laser treatment in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] It should be noted that, unless otherwise indicated, all numbers used in the specification and claims to represent feature sizes, quantities and physical properties should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.2, 1.4, 1.55, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0029] In the modern automotive industry, especially in the field of new energy vehicles, lightweighting has become one of the key means to improve vehicle performance, reduce energy consumption and reduce carbon emissions. High-strength, heat-treatable aluminum alloys are widely considered to be an ideal choice to replace traditional steel materials due to their excellent specific strength and specific stiffness. However, in practical applications, such aluminum alloys face significant technical challenges during welding.

[0030] Specifically, the strengthening of high-strength aluminum alloys mainly relies on nanoscale strengthening phases, which are formed during the heat treatment of the material and give the material high mechanical properties. However, these nano-strengthening phases are extremely sensitive to high temperatures and are easily dissolved or coarsened under the action of welding thermal cycles, resulting in loss of strengthening effects. As a result, the heat-affected zone of the weld shows significant softening, and the strength and toughness of the joint are significantly reduced. This phenomenon limits the application of high-strength aluminum alloys in structural parts that require high reliability and high performance.

[0031] In view of the above problems, the technical implementation idea of ​​the present invention is to find a method that can effectively improve the performance of the heat affected zone of welding without overall heat treatment. To this end, the inventors have conducted in-depth research on the organizational evolution and performance change mechanism of high-strength aluminum alloys during the welding process, and found that by making local and precise microstructural adjustments to the heat affected zone of welding, the softening problem can be improved and the mechanical properties of the joint can be improved.

[0032] Based on this idea, the present invention proposes a method for controlled treatment of the heat affected zone of welding using a laser heat source. By laser remelting specific areas of the heat affected zone after welding, a supersaturated solid solution can be formed in the local area. Then, these areas are subjected to natural aging treatment to precipitate fine strengthening phases and form local hardening zones, so that the heat affected zone of welding is transformed from the original softening area to an area with a hardness gradient, thereby enhancing the overall strength of the welded joint.

[0033] Please refer to Figure 1 FIG. 1 is a flow chart of an aluminum alloy welding method in an embodiment of the present invention. The aluminum alloy welding method specifically comprises the following steps:

[0034] S101: Welding aluminum alloy components to form welded joints.

[0035] It should be noted that the specific welding method may vary depending on the type of aluminum alloy, the geometry of the component, and the application scenario. Welding processes include MIG (metal inert gas arc welding), TIG (tungsten inert gas welding), and CMT (cold metal transfer) welding.

[0036] In an exemplary embodiment, the material of the aluminum alloy component is preferably a heat-treatable aluminum alloy with a yield strength greater than 300 MPa. For example, the heat-treatable aluminum alloy includes 2××× aluminum alloy, 6××× aluminum alloy or 7××× aluminum alloy. The thickness of the aluminum alloy component is preferably 2 to 4 mm.

[0037] Yield strength refers to the maximum stress that a material can withstand before plastic deformation. For the aluminum alloy parts in the present invention, the yield strength is preferably greater than 300 MPa, so that the material can maintain its shape and avoid permanent deformation when subjected to high loads. For example, in the structure of an automobile body, an aluminum alloy with a yield strength greater than 300 MPa can effectively withstand the impact, vibration and various mechanical stresses when the vehicle is running, thereby improving the safety and durability of the vehicle.

[0038] 2××× series, 6××× series and 7××× series aluminum alloys are common high-strength aluminum alloys. The difference between these series of aluminum alloys lies in their alloy composition and performance characteristics. 2××× series aluminum alloys (mainly containing copper) are usually used in the aerospace field because of their high strength and heat resistance. 6××× series aluminum alloys (mainly containing magnesium and silicon) are often used in the automotive industry because of their good machinability, corrosion resistance and weldability. 7××× series aluminum alloys (mainly containing zinc) are widely used in high-stress structural parts such as aircraft frames or high-performance racing cars due to their extremely high strength. By selecting these heat-treatable aluminum alloys, it is possible to achieve lightweight design while ensuring the strength and safety performance of structural parts.

[0039] The design choice of aluminum alloy parts with a thickness of 2 to 4 mm is suitable for structural applications that require a balance between strength and lightness. For automotive bodies and aviation components, a thickness of 2 to 4 mm can not only ensure that the parts have sufficient strength and rigidity, but also effectively reduce the total weight of the body or structure, thereby improving energy efficiency. For example, the panels of automobile bodies are usually in the range of 2 to 4 mm in thickness to reduce the weight of the vehicle as much as possible while meeting collision safety, improving fuel efficiency and reducing carbon dioxide emissions.

[0040] S102: Using a laser heat source to laser remelt a target area in a heat-affected zone of the weld joint, where the peak temperature is between 400° C. and 500° C., to form a remelting zone, and making the remelting zone in an oversaturated state.

[0041] In step S102, the mechanical properties of the welded joint are improved by utilizing the local heating and rapid cooling characteristics of the laser heat source.

[0042] During the welding process, the heat affected zone of the weld joint experiences high temperature, which will cause the nano-reinforced phase inside the material to fail, thereby weakening the strength of the weld joint. The role of step S102 is that the laser remelting process uses the high energy density of the laser to quickly heat the target area to a predetermined temperature, causing the material in the area to melt locally, and through subsequent rapid cooling, the area is in an oversaturated state. This oversaturated state provides favorable conditions for subsequent aging treatment, helps to form a reinforcement phase in the area, and improves the strength and hardness of the joint. At the same time, the process also has high precision and controllability, and can be flexibly adjusted according to different material and process requirements, thereby meeting the diverse needs of industrial applications, such as automotive, aerospace, and shipbuilding, which require high-strength connectors.

[0043] In an exemplary embodiment, the laser heat source is divided into two laser beams by a beam splitter, which act on the heat-affected zones on both sides of the weld joint respectively, so as to more evenly treat the heat-affected zones of the weld joint and ensure that both sides of the joint are acted upon by the laser at the same time, thereby effectively avoiding structural defects and degradation of mechanical properties caused by uneven heating on one side.

[0044] The application of laser heat source in welding is highly controllable, with high energy density and fast heating speed, which can achieve precise local processing. In the traditional welding process, due to the uneven heating of the heat-affected zone, the mechanical properties of one side of the weld joint are often better than the other side, which in turn affects the overall performance of the joint. By dividing the laser heat source into two beams and acting on both sides of the weld joint respectively, symmetrical and uniform heating can be achieved, which effectively improves this problem.

[0045] For example, in automobile manufacturing, the aluminum alloy structural parts of the car body often need to withstand extremely high stress. When using traditional welding methods, due to the asymmetry of the welding thermal cycle, the welded joint may form a large stress concentration on one side, which may easily cause cracks or breakage during use. By using the beam splitting technology of the beam splitter, the laser is evenly distributed to both sides of the joint, which can significantly reduce stress concentration and enhance the uniformity and reliability of the welded joint.

[0046] Specifically, the laser remelting parameters include a laser power of preferably 1.6-1.8 kW, a laser beam moving speed of preferably 60-80 mm / s, a laser beam swing trajectory close to a circle, a swing amplitude of preferably 0.6-0.8 mm, and a frequency of preferably 120-180 Hz.

[0047] Aluminum alloy has a low melting point, so too high laser power may cause over-melting or surface ablation, forming welding defects such as pores or cracks; while too low power may lead to insufficient remelting and fail to achieve the expected strengthening effect. Therefore, the power range of 1.6-1.8kW can ensure that the laser has enough energy to control the depth of the local remelting zone.

[0048] The moving speed of the laser beam is set to 60-80 mm / s, which is to control the speed of the laser moving on the surface of the material, thereby affecting the laser dwell time and heat input. Too fast moving speed may lead to insufficient depth of the remelting zone and aggravate the cracking tendency of the remelting zone; while too slow speed will lead to a decrease in the cooling speed of the remelting zone, affect the degree of solid solution of elements, and may cause excessive melting of the material or expansion of the heat affected zone. The speed of 60-80 mm / s can ensure that the remelting zone has a faster cooling speed and depth while maintaining welding efficiency, so as to achieve the best remelting effect.

[0049] The oscillation trajectory of the laser beam approaches a circle, the oscillation amplitude is preferably 0.6-0.8mm, and the frequency is preferably 120-180Hz. These oscillation parameters are set to optimize the energy distribution of the laser on the surface of the weld joint. The circular oscillation trajectory can ensure that the laser energy evenly covers the remelting area and avoids the concentration of energy at a certain point causing overheating problems. The amplitude range is set to 0.6-0.8mm to ensure that the oscillation range is large enough to effectively cover the width of the weld joint without dispersing the energy too much. The frequency is set to 120-180Hz to ensure that the oscillation speed of the laser beam is fast enough to ensure the stability of the keyhole in the remelting area, inhibit the formation of pores, and eliminate the pore problem caused by remelting.

[0050] In the welding of high-strength aluminum alloys, grain refinement in the remelting zone is one of the key factors in improving mechanical properties. By controlling the laser power movement speed, the heating and cooling rates of the material can be effectively adjusted to achieve grain refinement. The design of the oscillation trajectory and frequency ensures uniform temperature distribution in the entire remelting zone, so that the microstructure of the material is optimized. This uniform heat input method can not only enhance the tensile strength and toughness of the material, but also reduce the residual stress that may occur during welding and improve the fatigue resistance of the welded joint.

[0051] Specifically, the depth of the remelting zone is preferably 30-50% of the thickness of the aluminum alloy component, and the width is preferably 1-2 mm.

[0052] The depth of the remelting zone is 30% to 50% of the thickness of the aluminum alloy part. This setting is mainly to ensure that the remelting can penetrate into the key areas of the material without causing too much impact on the overall structure. If the remelting depth is too shallow, a sufficiently large hardening zone may not be formed, resulting in limited reinforcement of the remelting zone on the weld joint. If the remelting depth is too deep, the original fine structure of the material may be completely destroyed, destroying its original mechanical properties, especially plasticity. A depth of 30% to 50% can ensure the overall strength and structural integrity of the welded parts while strengthening the weld joint.

[0053] The width of the remelting zone is set to 1-2 mm. This design is to ensure that the laser remelting can accurately act on specific parts of the heat-affected zone and will not extend to areas that do not need to be treated. A width that is too narrow may not fully cover the key parts of the weld joint, resulting in a strengthening area that is too small and difficult to provide significant mechanical property improvements. A width that is too large may cause excessive heating of the surface area of ​​the material, excessive melting or uneven material structure. The 1-2 mm width setting ensures that the remelting zone is wide enough to meet the strengthening requirements of the heat-affected zone while avoiding melting of excess areas.

[0054] In an exemplary embodiment, during the welding process, an infrared temperature measurement system is used to measure the peak temperature distribution of the heat-affected zone of the weld joint, so as to accurately grasp the temperature change of the heat-affected zone in real time during the welding process.

[0055] The main advantage of the infrared temperature measurement system is its non-contact measurement method, which can quickly and accurately detect the temperature changes of the welded joint without interfering with the welding process. Traditional contact temperature measurement methods often have problems such as slow response speed and discontinuous measurement, which are difficult to meet the dynamic needs of high-temperature welding. The infrared temperature measurement system can monitor the temperature distribution of the welded joint in real time by detecting the infrared radiation of the object, especially the peak temperature of the heat-affected zone.

[0056] S103: The remelted area forms a local hardened area through natural aging, and forms a hardness gradient structure with the area not affected by the laser.

[0057] In the present invention, through the previous laser remelting treatment, the rapid heating and cooling characteristics of laser remelting are utilized to make the elements in the local remelting zone in a supersaturated state, so as to promote natural aging in the region and promote precipitation hardening of the strengthening phase in the region to form a local hardened zone. Through this process, the grain structure of the remelting zone is refined, and the strengthening phase is fully precipitated, so that the remelting zone has higher hardness and strength.

[0058] By locally hardening to form a hardness gradient structure, a hard-soft mechanical structure is constructed in the key area of ​​the welded joint. Such a hardness gradient structure helps to relieve stress concentration and enhance the tensile properties of the joint, especially when subjected to impact and fatigue loads, the strength and durability of the joint are significantly improved.

[0059] The present invention also provides an aluminum alloy workpiece, which is welded by the above-mentioned aluminum alloy welding method.

[0060] The present invention will be further described below in conjunction with specific embodiments.

[0061] Example 1

[0062] A 3.0 mm thick high-strength 6××× aluminum alloy plate was selected, with a yield strength of 370 MPa. The oxide scale in the welding area was removed mechanically, and the surface oil was removed with acetone and dried for later use.

[0063] The aluminum alloy plates are placed on the workbench in a spliced ​​manner and fixed with welding fixtures to prevent displacement during welding.

[0064] The CMT TPS 400i arc welding machine was used to perform CMT welding on the test plate to obtain a CMT welded joint. During the welding process, the wire feeding speed was 6.6m / min, the welding speed was 10mm / s; the shielding gas was argon with a purity of 99.99%, and the gas flow rate was 20L / min; and the infrared temperature measurement system was used to record the peak temperature experienced by the heat-affected zone during the welding process.

[0065] Wilson VH1102 fully automatic Vickers hardness tester was used to test the heat affected zone of the welded joint according to the national standard "GB / T4340.1-2009". The test results are as follows: Figure 2 As shown, the hardness of the over-aging area is the lowest, less than 70HV. According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the welded joint were tested on the Shimadzu AGS-X universal material testing machine, and the tensile strength was 245MPa.

[0066] For the aforementioned CMT welded joints, the surface oxide film and oil stains in the heat-affected zone (target area) with a peak temperature between 400 and 500°C were removed based on the infrared temperature measurement record results.

[0067] The two laser beams after splitting are used with an adjustable structure to locally remelt the above target area, and a local hardening area is formed after natural aging, which forms a hardness gradient structure with the area not affected by the laser. Among them, the laser power is 1.6kW, the moving speed is 80mm / s, the swing trajectory is "O" shaped, and the swing laser amplitude and frequency are 0.6mm and 150Hz respectively.

[0068] The depth and width of the laser remelting zone were measured using an Olympus optical microscope. The measurement results are shown in Figure 3 As shown in the figure, the depth and width of the remelting zone are approximately 1.2 mm and 1.8 mm respectively. Wilson VH1102 fully automatic Vickers hardness tester was used to test the heat affected zone of the laser treated welded joint according to the national standard GB / T4340.1-2009. The test results are shown in the figure below. Figure 4 As shown, the heat affected zone is not remelted ( Figure 4 The minimum hardness of the medium softening zone is 67HV, and the remelting zone ( Figure 4 The average hardness of the medium hardening zone is 80HV. According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the laser-treated welded joints were tested on the Shimadzu AGS-X universal material testing machine, and the tensile strength was 270MPa.

[0069] Example 2

[0070] A 3.0 mm thick high-strength 6××× aluminum alloy plate was selected, with a yield strength of 370 MPa. The oxide scale in the welding area was removed mechanically, and the surface oil was removed with acetone and dried for later use.

[0071] The aluminum alloy plates are placed on the workbench in a spliced ​​manner and fixed with welding fixtures to prevent displacement during welding.

[0072] The CMT TPS 400i arc welding machine was used to perform CMT welding on the test plate to obtain a CMT welded joint. During the welding process, the wire feeding speed was 6.6m / min, the welding speed was 10mm / s; the shielding gas was argon with a purity of 99.99%, and the gas flow rate was 20L / min; and the infrared temperature measurement system was used to record the peak temperature experienced by the heat-affected zone during the welding process.

[0073] According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the welded joint were tested on the Shimadzu AGS-X universal material testing machine. The test results are as follows: Figure 5 As shown, the tensile strength is 242MPa ( Figure 5 (corresponding curve without laser treatment).

[0074] For the aforementioned CMT welded joints, the surface oxide film and oil stains in the heat-affected zone (target area) with a peak temperature between 400 and 500°C were removed based on the infrared temperature measurement record results.

[0075] The two laser beams after splitting are used with an adjustable structure to locally remelt the above target area, and a local hardening area is formed after natural aging, which forms a hardness gradient structure with the area not affected by the laser. Among them, the laser power is 1.8kW, the moving speed is 60mm / s, the swing trajectory is "O" shaped, and the swing laser amplitude and frequency are 0.6mm and 150Hz respectively.

[0076] Wilson VH1102 fully automatic Vickers hardness tester was used to test the heat affected zone of the laser treated welded joint according to the national standard "GB / T4340.1-2009". The test results are as follows: Figure 6 As shown in the figure, the results show that the hardness of the local remelting zone is significantly higher than that of the over-aging zone, forming a circular arc-shaped local hardening zone. According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the laser-treated welded joints were tested on the Shimadzu AGS-X universal material testing machine, and the tensile strength was 262MPa ( Figure 5 (corresponding curve of laser treatment in the middle).

[0077] Comparative Example 1

[0078] A 3.0 mm thick high-strength 6××× aluminum alloy plate was selected, with a yield strength of 370 MPa. The oxide scale in the welding area was removed mechanically, and the surface oil was removed with acetone and dried for later use.

[0079] The aluminum alloy plates are placed on the workbench in a spliced ​​manner and fixed with welding fixtures to prevent displacement during welding.

[0080] The CMT TPS 400i arc welding machine was used to perform CMT welding on the test plate to obtain a CMT welded joint. During the welding process, the wire feeding speed was 6.6m / min, the welding speed was 10mm / s; the shielding gas was argon with a purity of 99.99%, and the gas flow rate was 20L / min; and the infrared temperature measurement system was used to record the peak temperature experienced by the heat-affected zone during the welding process.

[0081] According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the welded joint were tested on a Shimadzu AGS-X universal material testing machine, and the tensile strength was 242MPa.

[0082] For the aforementioned CMT welded joints, the surface oxide film and oil stains in the heat-affected zone (target area) with a peak temperature between 300 and 400°C were removed based on the infrared temperature measurement record results.

[0083] The two laser beams after splitting are used with an adjustable structure to locally remelt the above target area, and a local hardening area is formed after natural aging, which forms a hardness gradient structure with the area not affected by the laser. Among them, the laser power is 1.8kW, the moving speed is 60mm / s, the swing trajectory is "O" shaped, and the swing laser amplitude and frequency are 0.6mm and 150Hz respectively.

[0084] According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the laser-treated welded joints were tested on the Shimadzu AGS-X universal material testing machine. The test results are as follows: Figure 7 As shown, the tensile strength is 250MPa.

[0085] Comparative Example 2

[0086] A 3.0 mm thick high-strength 6××× aluminum alloy plate was selected, with a yield strength of 370 MPa. The oxide scale in the welding area was removed mechanically, and the surface oil was removed with acetone and dried for later use.

[0087] The aluminum alloy plates are placed on the workbench in a spliced ​​manner and fixed with welding fixtures to prevent displacement during welding.

[0088] The CMT TPS 400i arc welding machine was used to perform CMT welding on the test plate to obtain a CMT welded joint. During the welding process, the wire feeding speed was 6.6m / min, the welding speed was 10mm / s; the shielding gas was argon with a purity of 99.99%, and the gas flow rate was 20L / min; and the infrared temperature measurement system was used to record the peak temperature experienced by the heat-affected zone during the welding process.

[0089] According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the welded joint were tested on a Shimadzu AGS-X universal material testing machine, and the tensile strength was 242MPa.

[0090] For the aforementioned CMT welded joints, the surface oxide film and oil stains in the heat-affected zone (target area) with a peak temperature between 300 and 400°C were removed based on the infrared temperature measurement record results.

[0091] The two laser beams after splitting are used with an adjustable structure to locally remelt the above target area, and a local hardening area is formed after natural aging, which forms a hardness gradient structure with the area not affected by the laser. Among them, the laser power is 1.8kW, the moving speed is 60mm / s, the swing trajectory is "O" shaped, and the swing laser amplitude and frequency are 0.6mm and 150Hz respectively.

[0092] According to GB / T2651-2010 Metal Room Temperature Tensile Test Method, the mechanical properties of the laser-treated welded joint were tested on a Shimadzu AGS-X universal material testing machine, and the tensile strength was 242 MPa.

[0093] Combining the performance test results of Example 2, Comparative Example 1 and Comparative Example 2, it can be seen that laser remelting the target area with a peak temperature between 400°C and 500°C in the heat affected zone of the weld joint can significantly improve the mechanical properties of the weld joint. However, laser remelting the target area with a peak temperature between 300°C and 400°C and 500°C to 560°C does not improve the mechanical properties of the weld joint or improves it insignificantly.

[0094] The reason for the above results is that high-strength heat-treatable aluminum alloys (such as 2×××, 6×××, and 7××× series) mainly rely on precipitation strengthening phases (such as Mg2Si, Al2Cu, etc.) to improve mechanical properties. The size, morphology, and distribution of these strengthening phases have a direct impact on the strength and hardness of the alloy. During the welding process, the heat-affected zone will experience different temperatures, resulting in changes in the microstructure.

[0095] For the area with a peak temperature of 300°C to 400°C, the material is in the over-aging stage, and the strengthening phase begins to coarsen or partially dissolve, but still exists in the matrix. The role of laser remelting in this area is mainly to dissolve the existing coarsened strengthening phase, but because the initial strengthening phase has not been completely dissolved, laser remelting cannot further increase the solubility of the alloying elements. The concentration of the supersaturated solid solution formed after remelting is low, and the amount of strengthening phase precipitated during the subsequent aging process is limited, making it difficult to significantly improve the hardness and strength.

[0096] For the area with a peak temperature of 400°C to 500°C, the strengthening phase in the heat-affected zone has been mostly dissolved, but serious grain growth has not yet occurred. The material is in a solid solution state and has the potential to form a supersaturated solid solution. Laser remelting can completely dissolve the alloying elements in this area to form a uniform liquid phase. Due to the rapid heating and cooling characteristics of laser remelting, a supersaturated solid solution with fine grains is formed in the remelting zone during the cooling process. In the subsequent natural aging process, the alloying elements in the supersaturated solid solution gradually precipitate to form a fine and dispersed strengthening phase, thereby significantly improving the hardness and strength of the remelting zone. The hardened zone after remelting forms a hard-soft gradient structure with the area not affected by the laser, which effectively relieves stress concentration and improves the overall mechanical properties of the welded joint.

[0097] For the area with peak temperature of 500℃ to 560℃, the material may have been burned, the grains have grown severely, and even local melting has occurred. High temperature causes grain growth, the plasticity and toughness of the material decrease, and the strength decreases. Although laser remelting can dissolve alloy elements again, it is difficult to refine the grains again after remelting because the grains are already coarse, and it is difficult to improve the microstructure. Even if the alloy elements are dissolved again, the subsequent aging process will hardly make up for the performance loss caused by the coarse grains.

[0098] In summary, the aluminum alloy welding method and aluminum alloy workpiece provided by the present invention can form a supersaturated solid solution in the local area by performing laser remelting treatment on a specific area of ​​the heat affected zone after welding. The remelted area can precipitate fine strengthening phases through natural aging to form a local hardened zone, so that the welding heat affected zone is transformed from the original softening zone to a zone with a hardness gradient, thereby enhancing the overall strength of the weld joint.

[0099] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0100] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for welding aluminum alloy, characterized in that: include: Welding aluminum alloy parts to form welded joints; Using a laser heat source to laser remelt a target area in a heat-affected zone of the weld joint, where the peak temperature is between 400° C. and 500° C., to form a remelting zone, so that the remelting zone is in a supersaturated state; The remelted area forms a local hardened area through natural aging, and forms a hardness gradient structure with the area not acted by the laser.

2. The aluminum alloy welding method according to claim 1, characterized in that: The laser heat source is divided into two laser beams by a beam splitter, which act on the heat affected zones on both sides of the welding joint respectively.

3. The aluminum alloy welding method according to claim 2, characterized in that: The parameters of the laser remelting include a laser power of 1.6-1.8 kW and a laser beam moving speed of 60-80 mm / s.

4. The aluminum alloy welding method according to claim 3, characterized in that: The oscillation trajectory of the laser beam is close to a circle, the oscillation amplitude is 0.6-0.8 mm, and the frequency is 120-180 Hz.

5. The aluminum alloy welding method according to claim 1, characterized in that: The depth of the remelting zone is 30-50% of the thickness of the aluminum alloy component, and the width is 1-2 mm.

6. The aluminum alloy welding method according to claim 1, characterized in that: The aluminum alloy component is made of a heat-treatable aluminum alloy with a yield strength greater than 300 MPa.

7. The aluminum alloy welding method according to claim 6, characterized in that: The heat-treatable aluminum alloy includes a 2××× series aluminum alloy, a 6××× series aluminum alloy or a 7××× series aluminum alloy.

8. The aluminum alloy welding method according to claim 6, characterized in that: The thickness of the aluminum alloy component is 2-4 mm.

9. The aluminum alloy welding method according to claim 1, characterized in that: The method further comprises: During the welding process, an infrared temperature measurement system is used to measure the peak temperature distribution of the heat affected zone of the welding joint.

10. An aluminum alloy workpiece, characterized in that: The aluminum alloy is welded by the aluminum alloy welding method according to any one of claims 1 to 9.

Citation Information

Cited By

  • In-situ strengthening method for improving fracture toughness of aluminum alloy in additive manufacturing

    CN120249715A

  • An in-situ strengthening method to improve fracture toughness of aluminum alloys in additive manufacturing

    CN120249715B

  • Method for improving service performance of welded joint, welding method and device

    CN120734533A

  • Method for rapidly improving surface organization structure and roughness of cast aluminum alloy part

    CN120791159A