Low-silver vacuum brazing filler metal and preparation method thereof
By optimizing the solder formula, reducing the silver content and introducing Ge, Yb, Ni, Co, In and strengthening particles, the problems of high cost and poor performance of eutectic silver copper brazing are solved, and low-cost and high-performance low-silver is achieved Vacuum solder improves oxidation resistance and mechanical properties.
Patent Information
- Application Number
- CN202411404472.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-08
AI Technical Summary
The high silver content of existing eutectic silver copper brazing materials leads to an increase in production costs and poor processing and oxidation resistance. It is necessary to optimize the composition of the brazing materials to reduce costs and improve performance.
The low-silver vacuum solder formula is adopted, including Ag 58%-65%, Cu 32%-41%, Yb 0.05%-0.1%, Ge 0.1%-1%, and optionally added Ni, Co, In and strengthening particles. For example, zirconia, graphene, etc., the antioxidant properties and mechanical strength of the solder are improved through reasonable proportioning and treatment methods of these elements.
It effectively reduces the production cost of solder, improves the oxidation resistance and mechanical strength, ensures appropriate melting point and fluidity, and extends the service life of solder.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solder, and more specifically, to a low-silver vacuum solder and a preparation method thereof. Background Art
[0002] In a vacuum environment, the welding process requires materials to have high stability and reliability. In the fields of ceramic discharge tubes, relays, vacuum interrupters, and thyristors, eutectic silver-copper is mostly used as solder. Eutectic silver-copper (AgCu28) solder has low resistivity, excellent thermal conductivity and vacuum sealing performance. The working performance of the electric vacuum device using the above eutectic silver-copper is stable.
[0003] However, silver is a precious metal, and the amount of silver in eutectic silver-copper solder is very large, up to 72%. In addition, the price of industrial silver has continued to rise in recent years, leading to increasing production costs. Reducing the silver content in the solder is more likely to lead to problems such as poor solder processing performance and poor antioxidant performance, so the composition of the solder needs to be optimized. Summary of the invention
[0004] In order to improve the defects of high cost, poor processing performance and anti-oxidation performance of solder, the present application provides a low-silver vacuum solder and a preparation method thereof.
[0005] The present application provides a low-silver vacuum solder, which adopts the following technical solution: In a first aspect, the present application provides a low-silver vacuum solder, the solder comprising the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Other margin.
[0006] By adopting the above technical solution, the mass fraction of silver in the solder is optimized in this application, relative to the eutectic silver-copper (Ag 72 Cu 28) solder, the mass fraction of silver is reduced, which effectively reduces the production cost of the solder, and it is not easy to increase the melting point of the solder too much, so that the solder can still obtain a suitable melting point. In this scheme, Ge is added to the solder. Ge has a skin effect and can form a layer of GeO film on the surface of the solder, which can hinder the combination of other elements in the solder and oxygen, effectively improve the anti-oxidation performance of the solder, and maintain the fluidity of the solder in a molten state. The amount of Ge added is optimized. The appropriate amount of Ge added can improve the anti-oxidation performance of the solder, and has a low impact on the melting point of the solder, and it is not easy to increase the melting point of the solder. In addition, Yb element is added to the solder. Rare earth Yb as a rare earth element can appropriately reduce the melting temperature of the solder, effectively improve the wettability of the solder and the mechanical strength of the weld. The amount of Yb element added is optimized. The appropriate amount of Yb added can enable the solder to maintain suitable fluidity, refine the eutectic grain size, and improve the mechanical strength of the weld.
[0007] Optionally, the solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Ni 0.1%-0.5%; Co 0.1%-0.5%; Other margin.
[0008] By adopting the above technical scheme, the Ni element is added to the solder in this scheme. The Ni element can effectively improve the wettability, gap filling ability and fluidity of the solder, and play a role in solid solution strengthening and grain refinement of the solder alloy. In addition, Ni can react to generate heat and offset the mechanical heat flow, making the welding interface smoother and further improving the mechanical strength of the weld. The amount of Ni added is optimized, and the appropriate amount of addition can make the GeNi grain size appropriate. At the same time, the Co element is added in this scheme. The introduction of the Co element can coordinate the crystal phase growth in the solder, inhibit the excessive growth of small plane particles, increase the volume fraction of the eutectic structure, and make the lamellae in the eutectic structure smaller, thereby effectively improving the density, oxidation resistance and strength of the solder.
[0009] Optionally, the solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Ni 0.1%-0.5%; Co 0.1%-0.5%; In 0.1%-0.5%; Other margin.
[0010] By adopting the above technical solution, indium is added to the solder in this solution. The addition of indium can form a eutectic with a lower melting point, which can effectively reduce the melting temperature of the solder, refine the coarser particles in the solder, and produce solid solution strengthening to improve the mechanical strength of the welded joint. At the same time, the amount of In added is optimized. The appropriate amount of addition can steadily reduce the solder temperature, refine the grain size in the solder and have a low impact on the anti-oxidation performance of the solder, so that the solder can be used for a long time.
[0011] Optionally, the solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Ni 0.1%-0.5%; Co 0.1%-0.5%; Strengthening particles 0.1%-0.5%; the strengthening particles include any one or more of zirconium oxide, graphene, aluminum oxide, graphite powder and silicon carbide.
[0012] By adopting the above technical solution, it is preferred to add strengthening particles to the solder. The introduction of the strengthening particles can effectively improve the welding strength of the solder.
[0013] Zirconia is preferably used as the reinforcing particle. The addition of zirconium oxide can refine the IMC structure of the welding interface, refine the grain structure in the solder, and stably improve the mechanical properties of the solder.
[0014] The addition of graphene can introduce a lamellar structure into the solder, increase the dislocation density of the solder, organize dislocations to move at grain boundaries, compensate for defects in the solder, and inhibit the corrosion of the solder, so that the solder obtains better strength and corrosion resistance.
[0015] The addition of alumina can make the eutectic structure in the solder more evenly distributed, effectively improving the hardness and tensile strength of the solder.
[0016] The addition of graphite powder can be evenly embedded in the solder, playing a nailing role, effectively improving the mechanical strength of the solder and the mechanical strength of the weld.
[0017] The addition of silicon carbide can refine the grain size in the brazing filler metal, replace the needle-shaped phase particles in the weld, make the weld structure dense, and improve the mechanical strength of the weld joint.
[0018] Optionally, the zirconium oxide is nickel-plated zirconium oxide.
[0019] By adopting the above technical solution, the surface of zirconium oxide is nickel-plated. Nickel-plated zirconium oxide can refine the grain structure in the brazing material, increase the proportion of eutectic structure, improve the wettability of the brazing material, and improve the IMC structure of the welding interface. The dispersion of nickel-plated zirconium oxide in the brazing material can hinder the dislocation movement in the brazing alloy and thus improve the mechanical strength of the brazing material.
[0020] Optionally, the nickel-plated zirconium oxide is prepared as follows: zirconium oxide is pre-treated by ball milling to obtain pre-treated particles, the pre-treated particles are immersed in a nickel nitrate tetrahydrate solution, magnetically stirred, pyrolyzed, and reduced to obtain the nickel-plated zirconium oxide.
[0021] By adopting the above technical solution, a large number of defects can be formed on the surface of zirconia by ball milling pretreatment of zirconia, providing active points required for the loading of Ni particles, and refining the size of zirconia nanoparticles, reducing the possibility of zirconia agglomeration, so that the strengthening particles can be evenly dispersed in the solder. Nickel nitrate tetrahydrate is used as a precursor, and nickel is loaded on the surface of zirconia by thermal decomposition and reduction. Nickel can form a semi-coherent interface with the interface of zirconia, that is, nickel particles can be stably combined with the surface of zirconia.
[0022] Optionally, the nickel-plated zirconia includes nickel-plated zirconia particles and nickel-plated zirconia fibers.
[0023] By adopting the above technical solution, nickel-plated zirconia particles and nickel-plated zirconia fibers are used as reinforcing particles, a fiber network structure can be introduced into the solder, which plays a stable anchoring role in the solder and effectively improves the mechanical strength of the solder.
[0024] Optionally, the graphene includes copper-plated graphene and silver-plated graphene.
[0025] By adopting the above technical scheme, the surface of graphene is modified with copper / silver, which can effectively improve the compatibility of graphene with other components in the solder, improve the dispersion uniformity of graphene in the solder, and reduce the grain size of the interface IMC and the channels around the grain boundaries, thereby effectively inhibiting the growth of the IMC layer. In addition, copper / silver can serve as a bridge for transferring loads, which can enable the strengthening particles to be closely connected and combined with the solder, thereby improving the wettability and mechanical strength of the solder, and can utilize a large specific surface area to hinder the movement of atoms, thereby further improving the mechanical strength of the solder.
[0026] Optionally, a graphene oxide solution is mixed with a copper nitrate solution to obtain a mixed solution, ammonium bicarbonate is added to the mixed solution, and the reaction is continued for 1-2 hours to prepare copper-plated graphene.
[0027] By adopting the above technical scheme, the preparation method of copper-plated graphene is optimized, and nano-scale copper particles can be loaded on the surface of graphene, and micron-scale copper particles can be loaded on both sides to form a Cu-GO-Cu sandwich structure with oxygen bridging, which effectively hinders the stacking of graphene sheet structures, allowing graphene to be evenly dispersed in the solder, stably playing a reinforcing and corrosion-resistant role.
[0028] In a second aspect, the present application provides a method for preparing a low-silver vacuum solder, using the following technical solution: A method for preparing a low-silver vacuum solder comprises the following steps: S1. Melting: Ag, Cu, Ge and Yb are melted and refined in vacuum according to the proportion to obtain metal ingots; S2. Strip preparation: cleaning the dirt and oxide layer on the surface of the metal ingot, cold rolling, coiling, annealing, cooling, and obtaining the strip; S3. Stamping: Take the strip and continue cold rolling, shearing, stamping, and low silver vacuum solder.
[0029] In summary, this application has the following beneficial effects: 1. Since the present application optimizes the mass fraction of silver in the solder, the mass fraction of silver is reduced relative to the eutectic silver-copper (AgCu28) solder, which effectively reduces the production cost of the solder, and it is not easy to increase the melting point of the solder too much, so that the solder can still obtain a suitable melting point. In this scheme, Ge is added to the solder. Ge has a skin effect and can form a layer of GeO film on the surface of the solder, which can hinder the combination of other elements in the solder and oxygen, effectively improve the anti-oxidation properties of the solder, and maintain the fluidity of the solder in a molten state. The amount of Ge added is optimized, and the appropriate amount of Ge added can improve the anti-oxidation properties of the solder, and has a low effect on the melting point of the solder, and it is not easy to increase the melting point of the solder. In addition, the amount of Yb element added is optimized, and the appropriate amount of Yb added can enable the solder to maintain suitable fluidity, refine the eutectic grain size, and improve the mechanical strength of the weld joint.
[0030] 2. In the present application, indium is added to the solder. The addition of indium can form a eutectic with a lower melting point, which can effectively reduce the melting temperature of the solder, refine the coarser particles in the solder, and produce solid solution strengthening to improve the mechanical strength of the welded joint. At the same time, the amount of In added is optimized. The appropriate amount of addition can steadily reduce the solder temperature, refine the grain size in the solder, and have a low impact on the anti-oxidation performance of the solder, so that the solder can be used for a long time.
[0031] 3. The present application adds strengthening particles to the solder, and the introduction of the strengthening particles can effectively improve the welding strength of the solder.
[0032] 4. The present application performs nickel plating on the surface of zirconium oxide. Nickel-plated zirconium oxide can refine the grain structure in the solder, increase the proportion of eutectic structure, improve the wettability of the solder, and improve the IMC structure of the welding interface. The dispersion of nickel-plated zirconium oxide in the solder can hinder the dislocation movement in the solder alloy and thus improve the mechanical strength of the solder. DETAILED DESCRIPTION
[0033] The present application is further described in detail below with reference to the embodiments. Preparation Example
[0034] Preparation Example of Nickel-plated Zirconia
[0035] Preparation Example 1 Zirconia was pre-milled in a ball mill at 240 r / min for 1 h to obtain pre-treated particles, the pre-treated particles were immersed in a saturated aqueous solution of nickel nitrate tetrahydrate (solid-to-liquid ratio of 1:10), magnetically stirred, reacted in a water bath at 80°C, crystallized on the surface of the zirconium oxide, filtered, and dried to obtain pre-coated particles, the pre-coated particles were placed in a pyrolysis device (hydrogen: argon = 1:9), kept at 380°C and 500°C for 1 h respectively, cooled with the furnace to obtain nickel-plated zirconium oxide.
[0036] Preparation Example 2 The zirconia fiber was immersed in HF with a mass fraction of 15% for 20 minutes to obtain pretreated particles. The pretreated particles were immersed in a saturated aqueous solution of nickel nitrate tetrahydrate, magnetically stirred, and reacted in a water bath at 80°C. After crystallization on the surface of zirconia, the particles were filtered and dried to obtain pre-coated particles. The pre-coated particles were placed in a pyrolysis device (hydrogen: argon = 1:9), and kept at 380°C and 500°C for 1 hour respectively, and cooled with the furnace to obtain nickel-plated zirconia fibers.
[0037] Copper-coated graphene Preparation Example 3 The graphene oxide solution was mixed with the copper nitrate solution to obtain a mixed solution, and ammonium bicarbonate was added to the mixed solution. The reaction was continued for 1 hour, filtered, dried, and heat treated at 500°C for 1 hour to prepare copper-plated graphene. The concentration of copper nitrate was 0.18 g / mL, the concentration of ammonium bicarbonate was 0.18 g / mL, and the concentration of GO was 0.015 g / mL.
[0038] Preparation Example 4 The graphene oxide solution was mixed with the copper nitrate solution to obtain a mixed solution, and ammonium bicarbonate was added to the mixed solution. The reaction was continued for 2 hours, filtered, dried, and heat treated at 400°C for 1 hour to prepare copper-plated graphene. The concentration of copper nitrate was 0.18 g / mL, the concentration of ammonium bicarbonate was 0.18 g / mL, and the concentration of GO was 0.015 g / mL.
[0039] Silver-coated graphene Preparation Example 5 Take 30 mg of graphene and 10 mg of sodium dodecyl sulfate (SDS), then mix them, take 40 ml of dimethylformamide (DMF), add the mixed 30 mg of graphene and 10 mg of sodium dodecyl sulfate into 40 ml of dimethylformamide, and ultrasonically treat for 2 hours to obtain a graphene solution; take 20 ml of a 0.06 mol / ml silver nitrate solution, add it to the graphene solution after the ultrasonic treatment is completed, and continue ultrasonic treatment for 30 minutes to obtain a mixed solution; continue to heat the mixed solution for 1 hour, then filter (the heating temperature is about 70°C), wash, and store in alcohol to obtain silver-coated graphene.
[0040] Example of preparation of reinforced particles Preparation Example 6-9 Zirconium oxide, graphene and graphite powder were taken respectively to prepare reinforced particles. The specific masses are shown in the table below.
[0041] It is worth noting that the strengthening particles include but are not limited to zirconium oxide, graphene, aluminum oxide, graphite powder and silicon carbide. At the same time, the strengthening particles can be a combination of one or more of the above materials.
[0042] Preparation Example 10 The difference from Preparation Example 9 is that an equal mass of nickel-plated zirconium oxide (prepared in Preparation Example 1) is used to replace the zirconium oxide in Preparation Example 9 to prepare the reinforced particles.
[0043] Preparation Example 11 The difference from Preparation Example 9 is that 0.7 kg of nickel-plated zirconia (prepared in Preparation Example 1) and 0.3 kg of nickel-plated zirconia fiber (prepared in Preparation Example 2) are used to replace the zirconia in Preparation Example 9 to prepare the reinforced particles.
[0044] Preparation Example 12 The difference from Preparation Example 9 is that an equal mass of copper-plated graphene (prepared in Preparation Example 3) is used to replace the graphene in Preparation Example 9 to prepare the reinforced particles.
[0045] Preparation Example 13 The difference from Preparation Example 9 is that an equal mass of copper-plated graphene (prepared in Preparation Example 4) is used to replace the graphene in Preparation Example 9 to prepare the reinforced particles.
[0046] Preparation Example 14 The difference from Preparation Example 9 is that an equal mass of silver-coated graphene (prepared in Preparation Example 5) is used to replace the graphene in Preparation Example 9 to prepare the reinforced particles.
[0047] Preparation Example 15 The difference from Preparation Example 11 is that an equal mass of copper-plated graphene (prepared in Preparation Example 3) is used to replace the graphene in Preparation Example 9 to prepare the reinforced particles. Example
[0048] Examples 1-3 On the one hand, the present application provides a low-silver vacuum solder, comprising Ag, Cu, Yb and Ge, and the specific masses are shown in the table below.
[0049] On the other hand, the present application provides a method for preparing a low-silver vacuum solder, comprising the following steps: S1. Melting: Ag, Cu, Ge and Yb are taken in a horizontal continuous casting furnace according to the proportion, and the vacuum is set to 1.0×10 -1 Pa, heating and melting, refining at 880℃ for 10min, and pulling at 900℃ to obtain a metal ingot; wherein the copper is oxygen-free copper.
[0050] S2. Strip preparation: clean the dirt and oxide layer on the surface of the metal ingot, cold roll to 0.2 mm, coil, anneal at 360°C, and cool to obtain the strip; S3. Stamping: Take the strip and continue cold rolling to 20μm, shearing, stamping, low silver vacuum solder.
[0051] Embodiment 4-5 On the one hand, the present application provides a low-silver vacuum solder comprising Ag, Cu, Yb, Ge, Co, Ni and In, and the specific masses are shown in the table below.
[0052] On the other hand, the present application provides a method for preparing a low-silver vacuum solder, comprising the following steps: S1. Melting: Ag, Cu, Ge, Yb, Ge, Co, Ni and In are taken in a horizontal continuous casting furnace according to the proportion, and the vacuum is set to 1.0×10 -1 Pa, heating and melting, refining at 880℃ for 10min, and pulling at 900℃ to obtain a metal ingot; wherein the copper is oxygen-free copper.
[0053] S2. Strip preparation: clean the dirt and oxide layer on the surface of the metal ingot, cold roll to 0.2 mm, coil, anneal at 360°C, and cool to obtain the strip; S3. Stamping: Take the strip and continue cold rolling to 20μm, shearing, stamping, low silver vacuum solder.
[0054] Example 6
[0055] On the one hand, the present application provides a low-silver vacuum solder comprising Ag, Cu, Yb, Ge, Co, Ni, In and strengthening particles, and the specific mass is shown in the table below.
[0056] On the other hand, the present application provides a method for preparing a low-silver vacuum solder, comprising the following steps: S1. Melting: Ag, Cu, Ge, Yb, Ge, Co, Ni and In are taken in a horizontal continuous casting furnace according to the proportion, and the vacuum is set to 1.0×10 -1 Pa, heat and melt, add strengthening particles to the molten liquid, stir vigorously at 80r / min for 15min, stir vigorously at 85r / min for 5min, ultrasonically vibrate at 700W for 60s, repeat twice, and refine at 880℃ for 10min, and pull at 900℃ to obtain a metal ingot; wherein the copper is oxygen-free copper, and the strengthening particles are the strengthening particles prepared in Preparation Example 6.
[0057] S2. Strip preparation: clean the dirt and oxide layer on the surface of the metal ingot, cold roll to 0.2 mm, coil, anneal at 360°C, and cool to obtain the strip; S3. Stamping: Take the strip and continue cold rolling to 20μm, shearing, stamping, low silver vacuum solder.
[0058] Example 7 The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 7 are used in an equal mass fraction to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0059] Example 7
[0060] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 8 with the same mass fraction are used to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0061] Example 8
[0062] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 9 are used in an equal mass fraction to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0063] Example 9
[0064] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 10 with an equal mass fraction are used to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0065] Example 10
[0066] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 11 with an equal mass fraction are used to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0067] Embodiment 11
[0068] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 12 with an equal mass fraction are used to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0069] Example 12
[0070] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 13 with an equal mass fraction are used to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0071] Example 13
[0072] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 14 are used in an equal mass fraction to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder.
[0073] Embodiment 14
[0074] The difference from Example 6 is that the reinforcing particles prepared in Preparation Example 15 with an equal mass fraction are used to replace the reinforcing particles in Example 6 to prepare the low-silver vacuum solder. Comparative Example
[0075] Comparative Example 1 The difference between this comparative example and Example 3 is that the solder in this comparative example is Ag. 72 Cu 28 . Performance testing
[0076] (1) Tensile strength test: The tensile test is carried out according to the ASTM E8M-04 material test standard. The specimen is a circular specimen with a diameter of 4 mm and a gauge length of 25 mm. The experiment is carried out at room temperature and the test equipment is an electric tensile testing machine. The crosshead speed is 2 mm / min. The tensile strength of the specimen can be obtained through the experiment.
[0077] (2) Antioxidant performance test: The samples were placed in a humidified thermostatic chamber with the temperature set at 250°C, humidity at 80%, oxygen at 40%, and storage time at 45 days. The more surface oxide residue there is, the weaker the antioxidant property is.
[0078] Combining the performance test comparison in Table 3, we can find that: 1. By comparing Examples 1-3 with Comparative Examples 1-2, it can be found that the tensile strength of the solder prepared in Examples 1-3 is improved and the amount of oxidized slag is reduced, which indicates that the mass fraction of silver in the solder is optimized in the present application. Compared with the eutectic silver-copper (Ag72Cu28) solder, the mass fraction of silver is reduced, which effectively reduces the production cost of the solder and does not easily increase the melting point of the solder too much, so that the solder can still obtain a suitable melting point. Ge is added to the solder. Ge has a skin effect and can form a GeO film on the surface of the solder, which can hinder the combination of other elements in the solder with oxygen, and effectively improves the anti-oxidation performance of the solder. Yb element is added to the solder. Rare earth Yb, as a rare earth element, can appropriately reduce the melting temperature of the solder, effectively improving the wetting performance of the solder and the mechanical strength of the weld.
[0079] 2. By comparing Example 4-5 with Example 2, it can be found that the tensile strength of the solder prepared in Example 4-5 is improved and the amount of oxidized slag is reduced, which shows that the Ni element in this application can effectively improve the wettability, gap-filling ability and fluidity of the solder, and play a role in solid solution strengthening and grain refinement of the solder alloy, and Ni can react to generate heat and offset the mechanical heat flow. The introduction of the Co element can coordinate the growth of the crystal phase in the solder, inhibit the excessive growth of small plane particles, increase the volume fraction of the eutectic structure, and make the lamellae in the eutectic structure smaller. Indium element is added to the solder. The addition of indium element can form a eutectic with a lower melting point, which can effectively reduce the melting temperature of the solder and refine the coarser particles in the solder. Through the coupling effect of Ni, Co and In, the mechanical strength and antioxidant effect of the solder can be effectively improved.
[0080] 3. By comparing Examples 6-8 with Example 2, it can be found that the tensile strength of the solder prepared in Examples 6-8 is improved and the amount of oxidized slag is reduced, which indicates that the addition of zirconium oxide in the present application can refine the IMC structure of the welding interface, refine the grain structure in the solder, and stably improve the mechanical properties of the solder. It is possible to introduce a lamellar structure into the solder, increase the dislocation density of the solder, and move the dislocation of the structure at the grain boundary, which can make up for the defects generated in the solder and inhibit the corrosion of the solder, so that the solder obtains better strength and corrosion resistance. It can be evenly embedded in the solder, play a nailing role, and effectively improve the mechanical strength of the solder and the mechanical strength of the welded joint.
[0081] 4. By comparing Examples 9-10 with Example 2, it can be found that the tensile strength of the solder prepared in Examples 9-10 is improved and the amount of oxide slag is reduced. This shows that the use of nickel-plated zirconia particles and nickel-plated zirconia fibers as reinforcing particles in the present application can introduce a fiber network structure into the solder, stabilize it in the solder and play an anchoring role, thereby effectively improving the mechanical strength of the solder.
[0082] 5. By comparing Examples 11-12 with Example 2, it can be found that the tensile strength of the solder prepared in Examples 11-12 is improved and the amount of oxidized slag is reduced, which shows that the present application optimizes the preparation method of copper-plated graphene, and can load nano-scale copper particles on the surface of graphene and micron-scale copper particles on both sides to form a Cu-GO-Cu sandwich structure with oxygen bridging, which effectively hinders the stacking of graphene sheet structures, so that graphene can be evenly dispersed in the solder, stably playing a role in strengthening and corrosion resistance. The reaction time of copper-plated graphene is optimized, and the appropriate reaction time can enable copper-plated graphene to obtain a stable sandwich structure.
[0083] 6. By comparing Examples 13-14 with Example 2, it can be found that the tensile strength of the solder prepared in Examples 13-14 is improved and the amount of oxide slag is reduced, which means that the surface modification of graphene using copper / silver in the present application can effectively improve the compatibility of graphene with the remaining components in the solder, improve the dispersion uniformity of graphene in the solder, and reduce the grain size of the interface IMC and the channels around the grain boundaries, thereby effectively inhibiting the growth of the IMC layer.
[0084] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A low-silver vacuum solder, characterized in that: The solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Other margin.
2. A low-silver vacuum solder according to claim 1, characterized in that: The solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Ni 0.1%-0.5%; Co 0.1%-0.5%; Other margin.
3. A low-silver vacuum solder according to claim 2, characterized in that: The solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Ni 0.1%-0.5%; Co 0.1%-0.5%; In 0.1%-0.5%; Other margin.
4. A low-silver vacuum solder according to claim 2, characterized in that: The solder includes the following metal elements in percentage by mass: Ag 58%-65%; Cu 32%-41%; Yb 0.05%-0.1%; Ge 0.1%-1%; Ni 0.1%-0.5%; Co 0.1%-0.5%; Strengthening particles 0.1%-0.5%; the strengthening particles include any one or more of zirconium oxide, graphene, aluminum oxide, graphite powder and silicon carbide.
5. A low-silver vacuum solder according to claim 4, characterized in that: The zirconium oxide is nickel-plated zirconium oxide.
6. A low-silver vacuum solder according to claim 5, characterized in that: The nickel-plated zirconium oxide is prepared as follows: zirconium oxide is pre-treated by ball milling to obtain pre-treated particles, the pre-treated particles are immersed in a nickel nitrate tetrahydrate solution, magnetically stirred, pyrolyzed, and reduced to obtain the nickel-plated zirconium oxide.
7. The low-silver vacuum solder according to claim 5, characterized in that: The nickel-plated zirconia includes nickel-plated zirconia particles and nickel-plated zirconia fibers.
8. The low-silver vacuum solder according to claim 4, characterized in that: The graphene includes copper-plated graphene and silver-plated graphene.
9. The low-silver vacuum solder according to claim 8, characterized in that: The copper-plated graphene is prepared as follows: a graphene oxide solution is mixed with a copper nitrate solution to obtain a mixed solution, ammonium bicarbonate is added to the mixed solution, the reaction is continued for 1-2 hours, filtering, drying, and heat treatment to prepare the copper-plated graphene.
10. The method for preparing a low-silver vacuum solder according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Melting: Ag, Cu, Ge and Yb are melted and refined in vacuum according to the proportion to obtain metal ingots; S2. Strip preparation: cleaning the dirt and oxide layer on the surface of the metal ingot, cold rolling, coiling, annealing, cooling, and obtaining the strip; S3. Stamping: Take the strip and continue cold rolling, shearing, stamping, and low silver vacuum solder.
Citation Information
Patent Citations
Self-fluxing silver solder containing Yb, Ge and nano Nb
CN105081607A
Vacuum electronic tube-sealed low-silver multi-component alloy material and preparation method thereof
CN106467941A
Graphene-containing high-strength silver-based brazing filler metal and smelting method thereof
CN107309574A
Novel quarternary alloy brazing filler metal and preparation method thereof
CN110238559A
Silver-based brazing filler metal alloy, preparation method of silver-based brazing filler metal alloy, and preparation methods of foil strip and wire
CN112059468A
Cited By
Low-silver lead-free environment-friendly solder and application thereof in high-frequency electronic component packaging
CN122500413A
Welding material powder and preparation method therefor, and flux-cored welding wire and preparation method therefor
WO2026114103A1