Wood-based moisture absorption gel and preparation method thereof

By forming porous graphene oxide composite materials in natural wood and loading metal salts, the problems of hygroscopic salt loss and low hygroscopic persistence are solved, and efficient and durable hygroscopic effect is achieved, and raw material costs are reduced.

CN118906168APending Publication Date: 2024-11-08HENAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198859.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing hygroscopic salts are easily lost during the hygroscopic process, resulting in low hygroscopic durability, and the autolysis effect causes the loss of hygroscopic salts, affecting hygroscopic efficiency.

Method used

Using natural wood as a carrier, porous graphene oxide composite material is obtained through pretreatment, impregnation and chemical etching, and immersed in metal salt diluent, so that the metal salt is supported inside the porous graphene oxide composite material to form hydroxyl and carboxyl groups distributed The adsorption surface prevents metal salt loss and improves the moisture absorption efficiency and durability of hygroscopic aerogel.

Benefits of technology

Effectively prevent the loss of metal salts, improve the moisture absorption efficiency and durability of hygroscopic aerogels, reduce raw material costs, and enable hygroscopic aerogels to be reused for a long time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906168A_ABST
    Figure CN118906168A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: sequentially carrying out pretreatment, dipping and chemical etching on a carrier to obtain a porous graphene oxide composite material, soaking the porous graphene oxide composite material in a metal salt diluent to enable metal salt to be loaded in the porous graphene oxide composite material, and carrying out freeze drying to obtain the moisture-absorbing gel, the carrier is natural wood, the natural wood is subjected to pretreatment, impregnation and chemical etching to obtain a porous graphene oxide composite material, an adsorption surface on which hydroxyl groups and carboxyl groups are distributed is formed in the porous graphene oxide composite material, and metal salt is loaded on the adsorption surface. Therefore, the moisture absorption efficiency and durability of the moisture absorption gel are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of natural polymer materials, in particular to a wood-based moisture-absorbing aerogel and a preparation method thereof. Background Art

[0002] Water is an indispensable component of the earth's ecosystem and is widely present in nature. However, excessive humidity seriously affects the sustainability of the environment, endangers people's physical and mental health, accelerates the growth of harmful insects, parasites and microorganisms, causes chemical corrosion of metals, and damages building structures.

[0003] At present, the main strategies for capturing water vapor from the air are: cooling condensation, surface adsorption and hygroscopic absorption, among which the cooling condensation method is affected by the high energy consumption in the refrigeration process; the surface adsorbent has a small adsorption rate and a small water capacity; the hygroscopic absorption method mainly uses hygroscopic salts to capture water from the air. For example, Chinese patent CN113215828A provides a perforated graphene aerogel hygroscopic fiber, specifically, a graphene oxide aqueous solution is mixed with a hydrogen peroxide aqueous solution to obtain a perforated graphene oxide; the perforated graphene oxide liquid crystal is injected into a coagulation bath to obtain a perforated graphene hydrogel fiber; finally, the perforated graphene hydrogel is filled with a hygroscopic agent to obtain a hygroscopic fiber. The hygroscopic salt in the hygroscopic fiber will dissolve in the captured water, causing its hygroscopic rate to drop significantly, that is, the hygroscopic persistence is low, and this autolysis effect will cause the loss of hygroscopic salts. Summary of the invention

[0004] In order to solve the problem in the prior art that hygroscopic salts are easily lost and have low hygroscopic durability, the present invention provides a wood-based hygroscopic aerogel and a preparation method thereof. The hygroscopic aerogel obtained by the preparation method can effectively prevent the loss of metal salts, thereby improving the hygroscopic efficiency and durability of the hygroscopic aerogel. At the same time, the preparation cost of the hygroscopic aerogel is low.

[0005] In order to achieve the above-mentioned purpose, the specific scheme adopted by the present invention is: a method for preparing a wood-based hygroscopic aerogel, wherein a carrier is pretreated, impregnated and chemically etched in sequence to obtain a porous graphene oxide composite material, the porous graphene oxide composite material is immersed in a metal salt diluent, so that the metal salt is loaded inside the porous graphene oxide composite material, and freeze-dried to obtain the hygroscopic aerogel; the carrier is natural wood, and the natural wood is pretreated, impregnated and chemically etched to obtain a porous graphene oxide composite material, and an adsorption surface with hydroxyl groups and carboxyl groups distributed is formed inside the porous graphene oxide composite material, and the metal salt is loaded on the adsorption surface.

[0006] As an optimized solution of the preparation method of the above-mentioned wood-based moisture-absorbing aerogel, it comprises the following steps:

[0007] S1, slicing natural wood, soaking the wood slices in a bleaching solution at a temperature of 110-160° C. for bleaching, and freeze-drying to obtain white wood;

[0008] S2, soaking the white wood in a graphene oxide aqueous solution for impregnation, and freeze-drying to obtain a graphene oxide composite material;

[0009] S3, immersing the graphene oxide composite material obtained in S2 in an etchant for chemical etching to obtain a porous graphene oxide composite material;

[0010] S4, soaking the porous graphene oxide composite material obtained in S3 in a metal salt diluent to load the metal salt on the adsorption surface, and freeze-drying to obtain a hygroscopic aerogel.

[0011] As another optimization scheme of the preparation method of the above-mentioned wood-based hygroscopic aerogel: in S1, the thickness of the wood chip is 2-4 mm.

[0012] As another optimization scheme for the preparation method of the above-mentioned wood-based hygroscopic aerogel: in S1, the bleaching solution is NaClO 2 Solution or H 2 O 2 Solution.

[0013] As another optimized solution of the method for preparing the above-mentioned wood-based moisture-absorbing aerogel: in S1, the obtained white wood is reacted with a sodium periodate solution under light-proof conditions.

[0014] As another optimization scheme of the preparation method of the above-mentioned wood-based hygroscopic aerogel: in S2, the concentration of the graphene oxide aqueous solution is 0.1-2 mg / ml.

[0015] As another optimization scheme for the preparation method of the above-mentioned wood-based hygroscopic aerogel: in S3, the etching agent is H 2 O 2 Aqueous solution, with an etchant temperature of 90-110°C and a concentration of 10%-30%.

[0016] As another optimization scheme for the preparation method of the above-mentioned wood-based hygroscopic aerogel: the metal salt diluent is LiCl solution or CaCl 2 Solution.

[0017] As another optimization scheme of the preparation method of the above-mentioned wood-based moisture-absorbing aerogel: the concentration of the metal salt diluent is 3wt%-7wt%.

[0018] A wood-based moisture-absorbing aerogel is obtained by the above preparation method.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. A wood-based hygroscopic aerogel and a preparation method thereof, which uses natural wood as a carrier, pre-treats, impregnates and etches the natural wood, and fixes graphene oxide inside the natural wood. Fixing graphene oxide inside the natural wood can prevent the collapse of the wood structure, and the combination of graphene oxide and wood fiber of the wood forms an adsorption surface with rich hydroxyl and carboxyl groups inside the natural wood. Metal salts penetrate into the structure, and strong interactions are generated between the metal salts and the hydroxyl and carboxyl groups, which effectively prevents the loss of metal salts, increases the moisture absorption durability and moisture absorption efficiency of the hygroscopic aerogel, and enables the hygroscopic aerogel to be reused for a long time.

[0021] 2. In the present invention, the natural wood used is cheap and renewable, which greatly reduces the cost of raw materials.

[0022] 3. In the present invention, the obtained white wood is reacted with sodium periodate under light-proof conditions to increase the distribution of hydroxyl groups in the white wood and further prevent the loss of metal salts. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a SEM image of white wood obtained in Example 3;

[0024] Figure 2 is a SEM image of the graphene oxide composite material obtained in Example 3;

[0025] Figure 3 is a SEM image of the porous graphene oxide composite material obtained in Example 3;

[0026] Figure 4 is a SEM image of the hygroscopic aerogel obtained in Example 3;

[0027] Figure 5 This is the hygroscopicity experiment of the hygroscopic aerogel obtained in Example 3. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further elaborated in detail below in conjunction with specific embodiments. The parts of the present invention that are not described and disclosed in detail in the following embodiments should be understood as the prior art known or should be known to those skilled in the art.

[0029] A method for preparing a wood-based hygroscopic aerogel, wherein a carrier is pretreated, impregnated and chemically etched in sequence to obtain a porous graphene oxide composite material, the porous graphene oxide composite material is immersed in a metal salt diluent, the metal salt is loaded inside the porous graphene oxide composite material, and freeze-dried to obtain a hygroscopic aerogel; the carrier is natural wood, the natural wood is pretreated, impregnated and chemically etched to obtain a porous graphene oxide composite material, and an adsorption surface with hydroxyl and carboxyl groups distributed is formed inside the porous graphene oxide composite material, and the metal salt is loaded on the adsorption surface. Specifically, the method comprises the following steps:

[0030] S1, slice the natural wood into pieces with a thickness of 2-4 mm, soak the wood pieces in a bleaching solution at a temperature of 110-160°C for bleaching, and freeze-dry to obtain white wood. Specifically, the bleaching solution is NaClO 2 Solution or H 2 O 2 The wood chips are immersed in the bleaching solution for more than 1 hour to remove the lignin in the wood chips and expose the wood fibers, thereby obtaining a loose aerogel structure; then, the white wood is taken out of the bleaching solution, and is repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and then freeze-dried to obtain the white wood.

[0031] S2, soaking the white wood in a graphene oxide aqueous solution for impregnation, and freeze-drying to obtain a graphene oxide composite material, namely, a graphene oxide-white wood composite material (GOW); the concentration of the graphene oxide aqueous solution is 0.1-2 mg / ml.

[0032] S3, immersing the graphene oxide composite material obtained in S2 in an etchant for chemical etching to obtain a porous graphene oxide composite material, namely, a porous graphene oxide-white wood composite material (HGOW); the etchant is H 2 O 2 The aqueous solution, and the etching agent temperature is 90-110°C and the concentration is 10%-30%. The porosity of the wood fiber in the white wood is relatively large, and the structure is prone to collapse during the moisture absorption process. Therefore, the white wood is impregnated and etched to fix the graphene oxide inside the white wood structure to obtain a porous graphene oxide composite material, which effectively prevents the structural collapse. The combination of graphene oxide and wood fiber forms an adsorption surface with hydroxyl and carboxyl groups distributed inside the porous graphene oxide composite material.

[0033] S4, soaking the porous graphene oxide composite material obtained in S3 in a metal salt diluent, so that the metal salt is loaded on the adsorption surface, and freeze-drying to obtain a hygroscopic aerogel. The metal salt diluent is a LiCl solution or a CaCl 2The solution is prepared by mixing the metal salt diluent with the porous graphene oxide composite material, and the concentration of the metal salt diluent is 3wt%-7wt%. The metal salt enters the porous graphene oxide composite material structure and has a strong interaction with the hydroxyl and carboxyl groups on the adsorption surface, effectively preventing the loss of the metal salt, increasing the moisture absorption durability and moisture absorption efficiency of the hygroscopic aerogel, and enabling the hygroscopic aerogel to be reused for a long time.

[0034] In the above method, the natural wood used is cheap and renewable, which greatly reduces the cost of raw materials; at the same time, it is conducive to the processing and disposal of materials and has no pollution to the environment.

[0035] Example 1

[0036] S1, cut the natural wood into wood chips with a thickness of 2 mm, and soak the wood chips in NaClO at a temperature of 110℃. 2 The solution was boiled for 4 h, and then the residual chemicals were removed by repeated washing with ethanol and deionized water, and then freeze-dried to obtain white wood.

[0037] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0038] S3, the graphene oxide composite material obtained in S2 is immersed in 10% H2O at 90°C. 2 O 2 The aqueous solution was boiled for 1 h, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0039] S4, immersing the porous graphene oxide composite material obtained in S3 in a 3wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel.

[0040] Example 2

[0041] S1, cut the natural wood into wood chips with a thickness of 4 mm, and soak the wood chips in NaClO at a temperature of 160℃. 2 The solution was boiled for 4 h, and then the residual chemicals were removed by repeated washing with ethanol and deionized water, and then freeze-dried to obtain white wood.

[0042] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 2 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0043] S3, the graphene oxide composite material obtained in S2 is immersed in 30% H2O at 110°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0044] S4, immersing the porous graphene oxide composite material obtained in S3 in a 7wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel.

[0045] Example 3

[0046] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The solution (pH ~ 5) was boiled for 4 h, and then the residual chemicals were removed by repeated washing with ethanol and deionized water, and then freeze-dried to obtain white wood, such as Figure 1 As shown, this is the SEM image of white wood. It can be seen from the figure that the wood fibers of white wood are regularly arranged and are relatively large in size.

[0047] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material. The SEM image of the graphene oxide composite material is Figure 2 , graphene oxide is fixed inside the white wood structure, filling the gaps and internal pores in the wood, increasing its structure.

[0048] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 100°C. 2 O 2 The aqueous solution was boiled for 1 h, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material, such as Figure 3 As shown, it is a SEM of a porous graphene oxide composite material. As can be seen from the figure, after etching, many holes are generated on the surface of the graphene oxide composite material, and an adsorption surface combining wood fiber and graphene oxide appears.

[0049] S4, soaking the porous graphene oxide composite material obtained in S3 in a 5wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW), such as Figure 4 As shown, this is the SEM image of LiCl@HGOW. It can be seen from the figure that LiCl is fixed inside the porous graphene oxide composite material.

[0050] The hygroscopic aerogel obtained in this example was subjected to a hygroscopicity test. Figure 5 As shown, the water absorption of the hygroscopic aerogel shows a gradual upward trend over time, and reaches an extremely high water absorption of 6.3 g / g (water / aerogel dry weight) at 5 h (air humidity is 60%).

[0051] Example 4

[0052] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 110℃.2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0053] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0054] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 100°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0055] S4, immersing the porous graphene oxide composite material obtained in S3 in a 5wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0056] The hygroscopic aerogel obtained in this example was subjected to a hygroscopicity test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached a water absorption of 1.5 g / g (water / aerogel dry weight) at 5 h (air humidity was 61%).

[0057] Example 5

[0058] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0059] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0060] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 100°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0061] S4, immersing the porous graphene oxide composite material obtained in S3 in a 5wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0062] The hygroscopic aerogel obtained in this example was subjected to a hygroscopicity test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached a water absorption of 3.1 g / g (water / aerogel dry weight) at 5 h (air humidity was 59%).

[0063] Example 6

[0064] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0065] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0066] S3, the graphene oxide composite material obtained in S2 is immersed in 10% H2O at 100°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0067] S4, immersing the porous graphene oxide composite material obtained in S3 in a 5wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0068] The hygroscopic aerogel obtained in this example was subjected to a hygroscopicity test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached a water absorption of 2.9 g / g (water / aerogel dry weight) at 5 h (air humidity was 62%).

[0069] Example 7

[0070] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0071] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0072] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 100°C. 2 O 2The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0073] S4, immersing the porous graphene oxide composite material obtained in S3 in a 3 wt % LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0074] The hygroscopic aerogel obtained in this example was subjected to a hygroscopic test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached a water absorption of 4.2 g / g (water / aerogel dry weight) at 5 h (air humidity was 61%).

[0075] Example 8

[0076] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0077] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0078] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 90°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0079] S4, immersing the porous graphene oxide composite material obtained in S3 in a 7 wt % LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0080] The hygroscopic aerogel obtained in this example was subjected to a hygroscopic test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached a water absorption of 4.7 g / g (water / aerogel dry weight) at 5 h (air humidity was 60%).

[0081] Example 9

[0082] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 160℃. 2 The mixture was boiled in a solution (pH 5) for 2 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0083] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0084] S3, the graphene oxide composite material obtained in S2 is immersed in 20% H2O at 100°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0085] S4, immersing the porous graphene oxide composite material obtained in S3 in a 7 wt % LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0086] The hygroscopic aerogel obtained in this example was subjected to a hygroscopic test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached a water absorption of 5.5 g / g (water / aerogel dry weight) at 5 h (air humidity was 61%).

[0087] Example 10

[0088] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain the white wood.

[0089] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0090] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 110°C. 2 O 2 The aqueous solution was boiled for 1 hour, and then the residual chemical reagents were washed with deionized water to obtain a porous graphene oxide composite material.

[0091] S4, immersing the porous graphene oxide composite material obtained in S3 in a 7 wt % LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0092] The hygroscopic aerogel obtained in this example was subjected to a hygroscopicity test. As time went by, the water absorption of the hygroscopic aerogel showed a gradually increasing trend and reached an extremely high water absorption of 6.1 g / g (water / aerogel dry weight) at 5 h (air humidity was 62%).

[0093] Embodiment 11

[0094] S1, cut the natural wood into wood chips with a thickness of 3 mm, and soak the wood chips in NaClO at a temperature of 140℃. 2 The mixture was boiled in a solution (pH 5) for 4 h, then repeatedly rinsed with ethanol and deionized water to remove residual chemicals, and freeze-dried to obtain white wood. The white wood was reacted with a sodium periodate solution under light-proof conditions to increase the carboxyl groups on the surface of the wood fibers and further prevent the loss of LiCl.

[0095] S2, soaking the white wood in a graphene oxide aqueous solution, the concentration of the graphene oxide aqueous solution is 0.1 mg / ml, and freeze-drying to obtain a graphene oxide composite material.

[0096] S3, the graphene oxide composite material obtained in S2 is immersed in 25% H2O at 100°C. 2 O 2 The solution was boiled for 1 h, and then the residual chemical reagents were washed with deionized water.

[0097] S4, immersing the porous graphene oxide composite material obtained in S3 in a 5wt% LiCl solution, and freeze-drying to obtain a hygroscopic aerogel (LiCl@HGOW).

[0098] Example 12

[0099] A wood-based moisture-absorbing aerogel is obtained by the preparation method described in any one of the above embodiments 1-11.

[0100] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a wood-based hygroscopic aerogel, wherein a carrier is pretreated, impregnated and chemically etched in sequence to obtain a porous graphene oxide composite material, the porous graphene oxide composite material is immersed in a metal salt diluent, the metal salt is loaded inside the porous graphene oxide composite material, and freeze-dried to obtain a hygroscopic aerogel; characterized in that: The carrier is natural wood, and the porous graphene oxide composite material is obtained after pretreatment, impregnation and chemical etching of the natural wood. An adsorption surface with hydroxyl groups and carboxyl groups is formed inside the porous graphene oxide composite material, and the metal salt is loaded on the adsorption surface.

2. The method for preparing a wood-based moisture-absorbing aerogel according to claim 1, characterized in that: The following steps are involved: S1, slicing natural wood, soaking the wood slices in a bleaching solution at a temperature of 110-160° C. for bleaching, and freeze-drying to obtain white wood; S2, soaking the white wood in a graphene oxide aqueous solution for impregnation, and freeze-drying to obtain a graphene oxide composite material; S3, immersing the graphene oxide composite material obtained in S2 in an etchant for chemical etching to obtain a porous graphene oxide composite material; S4, soaking the porous graphene oxide composite material obtained in S3 in a metal salt diluent to load the metal salt on the adsorption surface, and freeze-drying to obtain a hygroscopic aerogel.

3. The method for preparing a wood-based moisture-absorbing aerogel according to claim 2, characterized in that: In S1, the thickness of the wood chips is 2-4 mm.

4. The method for preparing a wood-based moisture-absorbing aerogel according to claim 2, characterized in that: In S1, the bleaching solution is a NaClO2 solution or a H2O2 solution.

5. The method for preparing a wood-based moisture-absorbing aerogel according to claim 2, characterized in that: In S1, the obtained white wood is reacted with a sodium periodate solution under light-proof conditions.

6. The method for preparing a wood-based moisture-absorbing aerogel according to claim 2, characterized in that: In S2, the concentration of the graphene oxide aqueous solution is 0.1-2 mg / ml.

7. The method for preparing a wood-based moisture-absorbing aerogel according to claim 2, characterized in that: In the step S3, the etchant is a H2O2 aqueous solution, and the etchant temperature is 90-110°C and the concentration is 10%-30%.

8. The method for preparing a wood-based moisture-absorbing aerogel according to claim 1, characterized in that: The metal salt diluent is a LiCl solution or a CaCl2 solution.

9. The method for preparing a wood-based moisture-absorbing aerogel according to claim 1, characterized in that: The concentration of the metal salt diluent is 3wt%-7wt%.

10. A wood-based hygroscopic aerogel, characterized in that: The method is obtained by the preparation method described in any one of claims 1 to 9.