Active material slurry as well as preparation method, application and production system thereof
By using a production system designed with screens and inclined mixing leaves in the crushing and mixing system, sand-like active solid waste raw materials are crushed and stirred, which solves the problem of large area, low efficiency and micro powders being difficult to use in autoclaved aerated concrete. The problem of this is to achieve efficient preparation of active material slurry and good performance of autoclaved aerated concrete.
Patent Information
- Application Number
- CN202410960027.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art uses a ball mill to grind and activate the sand-shaped active solid waste raw material, resulting in a large area of the ball mill and low production efficiency. The obtained sand-shaped active solid waste powder is difficult to be used to produce autoclaved aerated concrete blocks. And there are problems of noise pollution and low yield.
The production system including a slurry tank, a slurry pump, a slurry crusher and a storage tank is adopted. The sand-shaped active solid waste raw materials are crushed and stirred through a screen and agitating device. The screen is equipped with 2~2.5mm*20~ The 25mm long screen hole, the stirring shaft is designed as an inclined two-layer stirring leaf group, which realizes effective crushing and uniform mixing of the slurry, and improves preparation efficiency and product fineness.
The crushing efficiency is significantly improved, noise pollution and floor area are reduced, and the obtained active material slurry can effectively reduce the bulk weight of the autoclaved aerated concrete block, while ensuring its strength, improving the uniformity and viscosity of the slurry, and improving Productivity.
Smart Images

Figure CN118906214A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to an active material slurry and a preparation method, application and production system thereof. Background Art
[0002] Sand-like active solid waste raw materials are a special type of solid waste. Due to their potential utilization value and environmental risks, their resource utilization and harmless treatment are particularly critical. Take slag as an example. It is made by rapidly quenching blast furnace slag at high temperature. The slag that has been quenched by water has a high glass content and a high-energy structure, which is unstable. However, the slag powder obtained after the grinding process shows good activity. Therefore, stimulating activity through crushing has become a key step in realizing the resource utilization of sand-like active solid waste raw materials.
[0003] At present, the traditional activation treatment method is to use a ball mill to ball-mill the sand-like active solid waste raw materials or other auxiliary materials together to obtain the corresponding active micropowder. For example, the patent with the publication number "CN 116947429 A" discloses a solid waste source high-activity powder slurry and its preparation method, which processes the solid waste by washing fly ash, desulfurized gypsum, and aluminum ash through drying, grinding, screening, and calcining to obtain an intermediate, and then mixes the intermediate with gypsum and grinds it to obtain a solid waste source sulfur-aluminum-iron series high-activity powder material. The activation treatment of sand-like active solid waste raw materials by ball milling can well meet the required fineness, but in the actual process, there are the following shortcomings: 1. The noise pollution is serious when the ball mill is running, which is not conducive to the health of the staff. 2. The ball mill takes a long time to ball mill the sand-like active solid waste raw materials, and generally the ball milling time for the same batch of materials reaches 1 to 2 hours. 3. Due to the long ball milling time of sand-like active solid waste raw materials, the output is low. Generally, the barrel speed of the Φ900×3000 ball mill is 38r / min, the ball loading is ≤2.7t, the feed particle size is ≤20mm, the discharge particle size is 0.075-0.89mm, the motor power is 22kw, and the hourly output is generally between 1.1-3.5t. 4. The sand-like active solid waste powder obtained after ball milling is relatively regular in shape and is all powder. After applying it to autoclaved aerated concrete blocks, the sand-like active solid waste powder reacts violently and solidifies quickly, making it unable to adapt to the existing process flow, and the activity after excitation cannot be fully utilized. 5. The sand-like active solid waste powder obtained after ball milling is all powder lacking the filling of porous substances, resulting in a larger bulk density of autoclaved aerated concrete blocks. Summary of the invention
[0004] The present invention aims to provide a production system for active material slurry, and to prepare active material slurry through the production system, so as to solve the problems in the prior art of using a ball mill to grind and activate sand-like active solid waste raw materials, resulting in a large area occupied by the ball mill, low production efficiency and the sand-like active solid waste powder produced being difficult to use in the production of autoclaved aerated concrete blocks.
[0005] A production system for active material slurry in this scheme includes a slurry making tank, a slurry pump, a slurry crusher and a storage tank. The slurry making tank is connected to the feed end of the slurry crusher through the slurry pump, and the discharge end of the slurry crusher is connected to the storage tank; a stirring device is provided in the slurry making tank, and the stirring device includes a stirring blade, a stirring shaft and a power device for driving the stirring shaft to rotate, and the stirring blade is fixedly connected to the stirring shaft; a screen is provided in the slurry crusher, and the wall of the screen is evenly distributed with long strip-shaped sieve holes with a size of 2~2.5㎜*20~25㎜.
[0006] Beneficial effects of this solution: The mesh diameter of the sieve used by the applicant in the early stage was 2mm, and the prepared slurry was used to prepare autoclaved aerated concrete blocks. The obtained autoclaved aerated concrete blocks had good strength, which could reach more than 4 MPa, but the bulk density was 650kg / m 3 The above makes it unusable; at the same time, the material is also very easy to cause the screen to be blocked, which in turn makes it unusable. The applicant continuously adjusted the screen holes and finally set the screen holes to a long hole structure of 2~2.5㎜*20~25㎜, so that the crushed slurry contains both fine materials and fine aggregates below 2.5mm, which can significantly improve the preparation efficiency of the slurry. In addition, when using porous and lightweight fine aggregates such as slag, it can effectively reduce the bulk density of the autoclaved aerated concrete block when it is embedded in the joints between the pore walls of the autoclaved aerated concrete block, and at the same time ensure that its strength meets the use requirements.
[0007] Furthermore, the stirring shaft is provided with two layers of stirring blade groups, the upper stirring blade group is composed of two stirring blades fixedly connected to the opposite sides of the stirring shaft, and the lower stirring blade group is composed of three stirring blades uniformly fixed on the stirring shaft, and the stirring blades of the upper and lower layers are inclined at 40° to the stirring shaft. The stirring blades adopt an upper and lower layer design, and there are only two stirring blades in the upper layer and three stirring blades in the lower layer, and the stirring blades are inclined at 40° to the stirring shaft. This design can effectively promote the forced movement of the material in the axial direction, ensuring the comprehensive circulation and deep mixing of the material. Compared with the traditional design, it has lower shear stress and higher fluid motion randomness, and the asymmetric circulation loop formed helps to enhance the turbulent effect. At different speeds, the device can flexibly realize the transition from convection circulation to turbulent state. Especially at high speeds, the larger blade inclination angle and twist can produce a more efficient flow field, significantly enhancing the collision and friction between material particles, thereby greatly improving the movement frequency and crossover opportunities of the mixed material, so that the uniformity and viscosity of the slurry are significantly improved.
[0008] Furthermore, a stirring device is also provided in the storage tank.
[0009] Furthermore, the size of the sieve hole is 2.5mm*25mm.
[0010] Based on the above production system, the present application also provides a method for preparing an active material slurry, comprising the following steps:
[0011] Step 1: Add sand-like active solid waste raw materials and water into a pulping tank at a weight ratio of 17:3-4 to obtain a mixture, and then stir the mixture into slurry through a stirring device in the pulping tank. The stirring time is 30-50 minutes, and the stirring speed of the stirring shaft is 20-25 r / min;
[0012] Step 2: Use a slurry pump to transport the slurry to a slurry crusher for impact crushing, so that the slurry reaches a fineness of ≤30% (200 mesh);
[0013] Step 3: The slurry after impact crushing falls freely into the storage tank through the screen. The stirring device in the storage tank stirs the slurry to obtain active material slurry. The stirring time is 40 to 60 minutes, and the stirring speed of the stirring shaft is 20 to 25 r / min.
[0014] Beneficial effects of this solution: Compared with the traditional use of ball mills to grind sand-like active solid waste raw materials to the required fineness: the ball mill needs to occupy at least 50 square meters, and the noise pollution is serious when the ball mill is running, the grinding time is long, and the efficiency is low (1.1-3.5 t / h). This solution abandons the traditional ball mill grinding, and uses a slurry crusher, which only occupies about 3 square meters, has low noise, fast grinding, and high efficiency (about 4.5 t / h). It can also effectively crush the material to the required fineness, and the residue on the 200 mesh sieve (0.088mm square hole sieve residue) is reduced from the original 25% to 28% to 15% to 20%. Since there are both fine powder and fine aggregate with a coarseness of less than 2.5 mm in the slurry, when using waste materials and other porous and lightweight fine aggregates, it can effectively reduce the dry density of the autoclaved aerated concrete blocks when it is embedded in the joint between the pore walls of the autoclaved aerated concrete blocks.
[0015] Furthermore, the particle size of the sand-like active solid waste raw material is ≤7 mm and the Mohs hardness is ≤6.
[0016] Furthermore, the sandy active solid waste raw material is one or more of granulated blast furnace slag, fly ash, and metal tailings slag.
[0017] Based on the good performance of the active material slurry in the present invention, the present application also provides the use of the active material slurry in the preparation of building materials.
[0018] Furthermore, the building material product is an autoclaved aerated concrete block. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a front view of the screen in Example 1 of the present invention;
[0020] Figure 2 for Figure 1 Right view of;
[0021] Figure 3 A top view of the stirring shaft and the stirring blade after being connected in Example 1 of the present invention;
[0022] Figure 4 This is a process flow chart for the production of autoclaved aerated concrete blocks;
[0023] Figures 5 to 7 The fly ash test report for Nayong Power Plant of Guizhou Jinyuan Co., Ltd. of State Power Investment Group;
[0024] Figures 8 to 10 Fly ash test report for Funeng (Guizhou) Power Generation Co., Ltd.
[0025] Figures 11 to 15 Fly ash test report for Datang Guizhou Faer Power Generation Co., Ltd.;
[0026] Fig.16 This is a test record sheet for the autoclaved aerated concrete blocks prepared in Examples 2 to 5. DETAILED DESCRIPTION
[0027] The following is further described in detail through specific implementation methods:
[0028] The reference numerals in the drawings of the specification include: screen 1, screen hole 2, stirring shaft 3, sleeve 4, stirring blade 5, bolt 6.
[0029] Example 1
[0030] Basically as attached Figures 1 to 3 As shown: a production system for active material slurry, including a pulping tank, a pulping pump, a pulp crusher and a storage tank, the pulping tank is connected to the feed end of the pulp crusher through the pulping pump, and the discharge end of the pulp crusher is connected to the storage tank; a stirring device is provided in the pulping tank and the storage tank, the stirring device includes a stirring blade 5, a stirring shaft 3 and a motor for driving the stirring shaft 3 to rotate, the stirring blade 5 has 5 pieces and is divided into two layers and fixedly connected to the stirring shaft 3, specifically: two layers of stirring blade 5 groups are provided on the stirring shaft 3, the upper stirring blade 5 group is composed of two stirring blades 5 fixedly connected to the opposite sides of the stirring shaft 3 (that is, 180 degrees between the two stirring blades 5), the lower stirring blade 5 group is composed of three stirring blades 5 uniformly fixed on the stirring shaft 3, the upper and lower stirring blades 5 are inclined 40 degrees to the stirring shaft 3, more specifically, a sleeve 4 is coaxially welded on the stirring shaft 3, a fixing block is integrally formed on the sleeve 4, and the stirring blade 5 is detachably connected to the fixing block by bolts 6 for easy loading and unloading. The slurry pulverizer uses a chrome alloy double-hammer slurry pulverizer produced by Zhucheng Longchi Machinery Equipment Manufacturing Plant. Two screens 1 are arranged in the slurry pulverizer. The longitudinal section of the screen 1 is semicircular. The wall of the screen 1 is evenly distributed with long strips of sieve holes 2 with a size of 2.5㎜*25㎜, that is, the sieve holes 2 are 25mm long and 2.5mm wide. The two screens 1 are respectively located under the two hammers and half-cover the hammers. The chrome alloy double-hammer slurry pulverizer is installed 5.4 meters above the storage tank, so that the slurry can directly enter the storage tank from the chrome alloy double-hammer slurry pulverizer under the action of gravity, thereby reducing energy consumption.
[0031] Example 2
[0032] Refer to the attached Figure 4 The process flow chart in the figure is to prepare autoclaved aerated concrete blocks, comprising the following steps:
[0033] 1. Preparation of active material slurry
[0034] The active material slurry is prepared using the above production system, comprising the following steps:
[0035] Step 1: The sand-like active solid waste raw materials are transported by belt, automatically weighed and fed by automatic feeding metering device, and enter the pulping tank. 15% (mass ratio) of reclaimed water is added to obtain a mixture, and the mixture is stirred by the stirring device in the pulping tank to form a slurry. The stirring time is 35 minutes, and the stirring speed of the stirring shaft 3 is 22r / min.
[0036] Step 2: The slurry mixed in step 1 is transported to a chrome alloy double hammer slurry crusher at a height of about 5.4 meters through a slurry pump. After the chrome alloy double hammer slurry crusher is crushed by counterattack, it passes through the screen 1 and the 2.5mm*25mm long strip sieve hole 2 on the screen 1. The two ends of the sieve hole 2 are provided with arc chamfers, so that fine materials and fine aggregates below 2mm are present in the slurry at the same time, and the slurry reaches a fineness of ≤30% (200 mesh) of the sieve residue. The material particles are strongly ground to stimulate the activity of the material.
[0037] Step 3: After the impact crushing in step 2, the slurry freely falls into the storage tank through the screen 1. The stirring device in the storage tank stirs the slurry to obtain active material slurry. The stirring time is 40 minutes, and the stirring speed of the stirring shaft 3 is 22 r / min.
[0038] Among them, the sand-like active solid waste raw materials are from the Nayong Power Plant of Guizhou Jinyuan Co., Ltd. of State Power Investment Group (attached Figures 5 to 7 )、Fujian (Guizhou) Power Generation Co., Ltd. (Attached Figures 8 to 10 )、Datang Guizhou Faer Power Generation Co., Ltd. (Attached Figures 11 to 15 ) The composition of fly ash produced during the production process is detailed in the inspection report (attached Figures 5 to 15 ), and granulated blast furnace slag produced in the applicant's production process.
[0039] The composition of granulated blast furnace slag is shown in the following table:
[0040]
[0041] 2. Preparation of autoclaved aerated concrete blocks
[0042] (1) Cement, lime powder and slurry are added to the pouring mixing tank according to the weight ratio and stirred. The diffusion degree of the material in the mixing tank is tested to be 130-145 mm and the temperature is 40-45 °C. Aluminum powder is added to the pouring mixing tank according to the weight ratio. The aluminum powder is added under stirring. The aluminum powder stirs the material in the pouring mixing tank during the addition process. After the aluminum powder is added, the stirring is continued for 40-50 seconds.
[0043] (2) Pour the material stirred in the pouring and mixing tank into the mold, and then harden it to obtain the embryo. The hardness of the embryo is required to be 300-360KN. The temperature in the static room is maintained at 40°C-50°C. The static time is 90min. Observe the changes of the static fermentation brick. The foaming requirement of the embryo is that after the gas is completed, crescent-shaped or round hole-shaped bubbles emerge above 30cm on the surface of the embryo. The number of bubbles is 4-6 per square meter, 1-2 per meter around, and the bubbling time is within 15-25 minutes.
[0044] (3) cutting the embryo;
[0045] (4) The embryos cut in step (3) were cured in an autoclave under the conditions of high temperature of 185°C and high pressure of 1.25 MPa. During the autoclave curing, 0.05 MPa steam was first introduced to evacuate the embryos for 40 minutes, and then the pressure was increased to a constant pressure of 1.25 MPa for 80 minutes.
[0046] 240-400min, autoclaved aerated concrete blocks are obtained.
[0047] Example 3
[0048] The preparation of the autoclaved aerated concrete block is different from that of Example 2 only in that the mesh holes 2 on the mesh 1 are conventional circular mesh holes 2, and the diameter of the mesh holes 2 is 2 mm.
[0049] Example 4
[0050] The preparation of the autoclaved aerated concrete blocks differs from that of Example 2 only in that the sandy active solid waste raw materials are not specially treated, but are screened to ensure that the fineness is 25%.
[0051] Example 5
[0052] The preparation of the autoclaved aerated concrete block differs from that of Example 2 only in that the sand-like active solid waste raw material is ground by a ball mill to obtain fine powder. In Example 5, the slurry solidifies too fast due to the fine powder, so that the autoclaved aerated concrete block does not generate gas, and thus has insufficient strength.
[0053] Detailed preparation parameters and performance parameters are attached. Fig.16 "Autoclaved aerated concrete block test record form".
[0054] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A production system for active material slurry, comprising a slurry making tank, a slurry pump, a slurry crusher and a storage tank, characterized in that: The pulping pool is connected with the feed end of the slurry crusher through a slurry pump, and the discharge end of the slurry crusher is connected with the storage tank; a stirring device is arranged in the pulping pool, and the stirring device comprises stirring blades, a stirring shaft and a power device for driving the stirring shaft to rotate, and the stirring blades are fixedly connected to the stirring shaft; a screen is arranged in the slurry crusher, and long strip-shaped sieve holes with a size of 2-2.5 mm*20-25 mm are evenly distributed on the wall of the screen.
2. The active material slurry production system according to claim 1, characterized in that: The stirring shaft is provided with two layers of stirring blade groups, the upper stirring blade group is composed of two stirring blades fixedly connected to the opposite sides of the stirring shaft, and the lower stirring blade group is composed of three stirring blades evenly fixed in a ring on the stirring shaft, and the stirring blades of the upper and lower layers are inclined at 40 degrees to the stirring shaft.
3. The active material slurry production system according to claim 2, characterized in that: A stirring device is also provided in the storage tank.
4. The active material slurry production system according to claim 3, characterized in that: The size of the sieve hole is 2.5mm*25mm.
5. The method for preparing active material slurry by the production system of claim 4, characterized in that: The following steps are involved: Step 1: Add sand-like active solid waste raw materials and water into a pulping tank at a weight ratio of 17:3-4 to obtain a mixture, and then stir the mixture into slurry through a stirring device in the pulping tank. The stirring time is 30-50 minutes, and the stirring speed of the stirring shaft is 20-25 r / min; Step 2: The slurry is transported to the slurry crusher by a slurry pump for impact crushing, so that the slurry reaches a fineness of ≤30% under 200 mesh; Step 3: The slurry after impact crushing falls freely into the storage tank through the screen. The stirring device in the storage tank stirs the slurry to obtain active material slurry. The stirring time is 40 to 60 minutes, and the stirring speed of the stirring shaft is 20 to 25 r / min.
6. The method for preparing active material slurry by the production system according to claim 5, characterized in that: The particle size of the sand-like active solid waste raw material is ≤7 mm and the Mohs hardness is ≤6.
7. The method for preparing active material slurry by the production system according to claim 6, characterized in that: The sand-like active solid waste raw material is one or more of granulated blast furnace slag, fly ash, and metal tailings slag.
8. An active material slurry, characterized in that: It is prepared by the method according to any one of claims 5 to 7.
9. Use of the active material slurry according to claim 8 in the preparation of building materials.