Composite material preparation method, composite material and electronic equipment
Through simulation software analysis and the use of tensioning devices, the problem of fiber defects in spherical structure molding of fiber materials is solved, high-quality composite material preparation is achieved, and the product yield and appearance status are improved.
Patent Information
- Application Number
- CN202411415806.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-10-11
AI Technical Summary
During the spherical structure molding process of fiber materials, the residual material of the prepreg leads to the wrinkles, separation and dislocation of the fibers, and the apparent area of the spherical structure is smaller than the actual area, resulting in defect formation and product quality decline.
Simulation software is used to analyze the sensitive areas during the prepreg molding process, and a tensioning device is set on the outside of the mold to tension the prepreg and perform hot pressing to avoid shearing and bending of the fibers and reduce the occurrence of defects.
It effectively avoids the formation of defects such as fiber wrinkles, separation and deformation, improves the yield and quality of composite materials, and is simple in process and easy to operate.
Smart Images

Figure CN118906499A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of material preparation, and more specifically, to a composite material preparation method, a composite material and an electronic device. Background Art
[0002] In related technologies, such as Figure 4 As shown, during the preparation process of fiber material products, they are usually prepared into prepregs, and then the prepregs are compression molded in a mold. When preparing products with spherical structures, since the apparent actual area of the spherical structure is smaller than the actual area of the required prepreg, it is inevitable that excess material will appear during the prepreg molding process, and the excess material will be stretched or squeezed to form wrinkles on the product, and as the depth of the spherical structure increases, the wrinkles of the excess material will also be aggravated. In addition, the spherical structure will cause the fibers of the prepreg to be severely sheared and bent during compression molding, which can easily lead to the phenomenon of dislocation and separation of the fibers of the prepreg.
[0003] Therefore, it is necessary to provide a new technical solution to solve the above technical problems. Summary of the invention
[0004] An object of the present invention is to provide a method for preparing a composite material, a composite material and a new technical solution for electronic equipment.
[0005] According to a first aspect of the present invention, a method for preparing a composite material is provided. The method comprises: Use simulation software to simulate and analyze the prepreg molding process to determine sensitive areas where defects are likely to form; According to the simulation analysis results, a tensioning device is arranged outside the portion corresponding to the sensitive area in the mold, and the tensioning device is used to tension the sensitive area of the prepreg; The prepreg is placed in the mold, tensioned by a tensioning device, and hot-pressed.
[0006] Optionally, the simulation software includes at least one of Fibersim software, Ansys software, and Pam-Composite software.
[0007] Optionally, the tensioning device includes a pre-pressing device, the pre-pressing device includes an elastic member and a block structure abutting against the elastic member, and when the mold is closed, the block structure abuts against another mold core of the mold or against the block structure located on another mold core; Alternatively, the tensioning device comprises a traction device, and the traction device comprises a clamping device for clamping the prepreg.
[0008] Optionally, before the step of placing the prepreg in the mold, tensioning the prepreg with a tensioning device, and performing hot pressing molding, the method further includes: The simulation software is used to simulate and analyze the molding process of the prepreg after being tensioned by the tensioning device, and the parameters of the tensioning device are output under the condition that the defects in the sensitive area meet the requirements.
[0009] Optionally, the step of using simulation software to simulate and analyze the molding process of the prepreg to determine sensitive areas where defects are easily formed includes: The laying process and pressing process of the prepreg are simulated and analyzed.
[0010] Optionally, the defect includes at least one of fiber wrinkles, fiber separation, and fiber dislocation.
[0011] Optionally, in the step of placing the prepreg in the mold, tensioning the prepreg using a tensioning device, and performing hot pressing molding, The prepreg comprises a thermosetting material, and the prepreg is placed between a male mold core and a female mold core of the mold and is compression molded.
[0012] Optionally, the temperature of the mold is 100°C-160°C, the vacuum time is 100s-300s, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0013] Optionally, in the step of placing the prepreg in the mold, tensioning the prepreg using a tensioning device, and performing hot pressing molding, The prepreg comprises a thermoplastic material, and the prepreg is placed between a male mold core and a female mold core of the mold and is compression molded.
[0014] Optionally, infrared heating is used for compression molding, the infrared heating temperature is 300℃-600℃, the infrared heating time is 10s-100s; the temperature of the mold is 40℃-200℃, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0015] According to a second aspect of the present invention, a composite material is provided. The composite material is prepared according to the composite material preparation method of the present invention.
[0016] Optionally, the composite material has a thickness of 0.2 mm-2 mm.
[0017] According to a third aspect of the present invention, an electronic device is provided, comprising the composite material of the present invention.
[0018] In the embodiment of the present invention, the simulation software can be used to effectively determine the sensitive area of the prepreg during the molding process, that is, the area where defects are easily formed. By pre-arranging a tensioning device on the mold outside the area and connecting the tensioning device to the prepreg, the prepreg can be effectively positioned and tensioned, thereby effectively avoiding the defects of fiber wrinkles, fiber separation, fiber deformation, etc. in the prepreg caused by the extrusion deformation and displacement of the prepreg during the molding process. The preparation method is simple in process, easy to operate, and has a high yield rate of composite materials.
[0019] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0021] Figure 1 is a flow chart of a method for preparing a composite material according to an embodiment of the present invention.
[0022] Figure 2 is a schematic diagram of a tensioning device according to an embodiment of the present invention.
[0023] Figure 3 is a schematic diagram of a traction device according to an embodiment of the present invention.
[0024] Figure 4 It is a schematic diagram of a method for preparing a composite material in the prior art.
[0025] Description of reference numerals: 101. die core; 102. prepreg; 103. pre-pressing device; 104. clamping device. DETAILED DESCRIPTION
[0026] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0027] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0028] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0029] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0030] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0031] According to one embodiment of the present invention, a method for preparing a composite material is provided. Figure 1-Figure 3 As shown, the preparation method comprises: Using simulation software to simulate and analyze the molding process of the prepreg 102 to determine sensitive areas where defects are likely to form; According to the simulation analysis results, a tensioning device is arranged outside the portion corresponding to the sensitive area in the mold, and the tensioning device is used to tension the sensitive area of the prepreg 102; The prepreg 102 is placed in the mold, tensioned by a tensioning device, and hot-pressed.
[0032] In an embodiment of the present invention, the composite material is compression molded using a prepreg 102. For example, the mold includes a male mold core and a female mold core 101. The male mold core and the female mold core 101 match the structure of the product. During compression molding, the prepreg 102 is first heated to soften; then, the prepreg 102 is clamped between the male mold core and the female mold core 101, and pressed under a set pressure and vacuum conditions. After the prepreg 102 is hardened and formed, a product with a set structure is formed. In the case where the product has a spherical structure, the prepreg 102 is prone to defects such as fiber wrinkles, fiber separation, and fiber deformation during the compression molding process.
[0033] In this embodiment, before placing the prepreg 102 in the mold, simulation software is first used to simulate and analyze the stress and deformation of the prepreg 102 during the molding process. Through simulation analysis, the area where the prepreg 102 is prone to defects is determined. For example, defects include fiber wrinkles, fiber separation, fiber deformation, etc. Usually, the formation of defects such as fiber wrinkles, fiber separation, and fiber deformation is due to the fact that the area of the prepreg 102 is larger than the apparent area of the spherical structure of the mold core, causing the prepreg 102 to move during the molding process. In order to solve this technical problem, according to the simulation analysis results, a tensioning device is set outside the part corresponding to the sensitive area in the mold, and the tensioning device is used to tension the sensitive area of the prepreg 102. For example, the tensioning device is set at a part of the mold outside the area corresponding to the product area. It should be noted that the prepreg 102 includes a product area for forming a product and a non-product area set around the product area. In other words, the tensioning device is set at a part of the mold corresponding to the non-product area. The tensioning device can be fixed on the mold or can be detachably connected to the mold.
[0034] The prepreg 102 is placed in the mold and connected to the tensioning device. For example, the tensioning device is connected to the non-product area of the prepreg 102 to position the prepreg 102, so as to effectively avoid displacement of the prepreg 102 to form fiber separation, fiber deformation, etc.; and the tensioning device can pull the non-product area so as to tension at least part of the prepreg 102 to avoid excess material in the part of the prepreg 102 to form fiber wrinkles.
[0035] For example, the tensioning device may be independently connected to the non-product area of the prepreg 102 , or the tensioning device and the mold may jointly clamp the non-product area of the prepreg 102 .
[0036] Next, the prepreg 102 is compression molded by a mold.
[0037] In the embodiment of the present invention, the simulation software can be used to effectively determine the sensitive area of the prepreg 102 during the molding process, that is, the area where defects are easily formed. By pre-arranging a tensioning device on the mold outside the area and connecting the tensioning device to the prepreg 102, the prepreg 102 can be effectively positioned and tensioned, thereby effectively avoiding the defects such as fiber wrinkles, fiber separation, and fiber deformation in the prepreg 102 caused by the extrusion deformation and displacement of the prepreg 102 during the molding process. The preparation method is simple in process, easy to operate, and has a high yield rate of the composite material.
[0038] In one embodiment of the present invention, the simulation software includes at least one of Fibersim software, Ansys software, and Pam-Composite software.
[0039] Any one or more of the above software can be used for simulation analysis. When in use, the parameters of the mold, the parameters of the prepreg 102, and the process parameters of the compression molding are input into Fibersim software, Ansys software, and / or Pam-Composite software for simulation. The above software can effectively determine the sensitive area of the prepreg 102.
[0040] In one embodiment of the present invention, the tensioning device includes a pre-pressing device 103, and the pre-pressing device 103 includes an elastic member and a block structure abutting against the elastic member. When the mold is closed, the block structure abuts against another mold core of the mold or against the block structure located at another mold core; Alternatively, the tensioning device comprises a traction device, and the traction device comprises a clamping device 104 for clamping the prepreg.
[0041] In an embodiment, Figure 2 As shown, the pre-pressing device 103 can press at least a part of the non-product area of the prepreg 102 after the prepreg 102 is placed on the mold. For example, the mold includes a male mold core and a female mold core 101. Taking the female mold core 101 as an example, a mounting hole is arranged at the edge of the female mold core 101, the block structure is located in the mounting hole and can slide along the mounting hole, a part of the block structure can protrude from the opening of the mounting hole, and an elastic member is arranged between the block structure and the bottom of the mounting hole, and the elastic member is, for example, a spring, a spring, an elastic rubber member, etc. The elastic member supports the block structure so that a part of the block structure protrudes from the opening of the mounting hole. When installing the prepreg 102, the prepreg 102 is placed on the female mold core 101. The non-product area of the prepreg 102 covers the protruding part of the block structure. When the female mold core 101 and the male mold core are molded together, the block structure and the edge of the male mold core jointly clamp at least part of the non-product area of the prepreg 102, so that at least part of the prepreg 102 can be tensioned. As the mold is closed, the block structure gradually retracts into the mounting hole. Under the elastic force of the spring, the clamping force of the block structure and the male mold core on the prepreg 102 gradually increases. The prepreg 102 is rectangular. The prepressing device 103 is arranged on two or four opposite sides of the prepreg 102.
[0042] In other embodiments, a mounting hole may be provided on the male mold core. An elastic member and a block structure are provided in the mounting hole. Part of the block structure protrudes from the opening of the mounting hole. When the mold is closed, the block structure and the edge of the female mold core 101 jointly clamp the non-product area of the prepreg 102.
[0043] Of course, the pre-pressing device 103 may also be provided with a sleeve. The elastic member and the block structure are located in the sleeve, so that the pre-pressing device 103 forms an independent structure. The sleeve is installed at the edge of the male die core and / or the female die core 101.
[0044] In the above embodiment, when clamped, the prepreg 102 is attached to the male mold core or the female mold core 101. When the temperature of the male mold core or the female mold core 101 is too high, the prepreg 102 is easily damaged. In order to solve this technical problem, mounting holes are provided on both the male mold core and the female mold core 101, and the two mounting holes are arranged opposite to each other. Elastic parts and block structures are provided in both mounting holes. Parts of the block structures protrude from the openings of the mounting holes in which they are located. In this way, when the mold is closed, the two block structures jointly extrude the non-product area of the prepreg 102, thereby tensioning at least part of the prepreg 102. Since both block structures protrude from the openings of the mounting holes in which they are located, when the non-product area of the prepreg 102 is clamped, the prepreg 102 can be suspended relative to the male mold core and the female mold core 101, instead of being attached to the male mold core or the female mold core 101. This can effectively prevent at least a portion of the prepreg 102 from coming into contact with the male mold core and / or female mold core 101 having an excessively high temperature when being tensioned by the tensioning device.
[0045] like Figure 3 As shown, the traction device is arranged at the edge of the male mold core and / or the female mold core 101. The traction device includes a clamping device 104. The clamping device 104 can clamp the non-product area of the prepreg 102, so as to tension the sensitive area of the prepreg 102. For example, the prepreg 102 is rectangular. The clamping device 104 is arranged on two or four opposite sides of the prepreg 102. Of course, the prepreg 102 can also be in other shapes, and the number and position of the clamping device 104 depend on the specific shape of the prepreg 102.
[0046] In one embodiment of the present invention, before the step of placing the prepreg 102 in the mold, tensioning the prepreg 102 with a tensioning device, and performing hot pressing molding, the method further includes: The simulation software is used to simulate and analyze the molding process of the prepreg 102 after being tensioned by the tensioning device, and hot pressing molding is performed under the condition that the defects in the sensitive area meet the requirements.
[0047] In this embodiment, the parameters of the tensioning device are input into the above-mentioned simulation software, and the tensioning device is used to clamp the non-product area of the prepreg 102, and then the defects such as fiber wrinkles, fiber separation, and fiber deformation are evaluated in the sensitive area of the prepreg 102 during the molding process; or the degree of fiber wrinkles, fiber separation, and fiber deformation, so as to determine whether the type, position, and quantity of the tensioning device meet the requirements of molding. When the prepreg 102 has no defects or the defects are small, it is determined that the tensioning effect of the tensioning device is effective. Under this condition, molding is performed.
[0048] When the defects in the sensitive area do not meet the requirements, the type, position, quantity, etc. of the tensioning device are adjusted, and the prepreg 102 is tensioned again, and the effect of the tensioning device is evaluated again using simulation software until the type, position, quantity, etc. of the tensioning device meet the requirements of compression molding, and then compression molding is performed.
[0049] In one embodiment of the present invention, the step of using simulation software to simulate and analyze the molding process of the prepreg 102 to determine the sensitive area where defects are easily formed includes: The laying process and the pressing process of the prepreg 102 are simulated and analyzed.
[0050] In this embodiment, the prepreg 102 is usually a multi-layer structure. The multi-layer prepreg 102 is sequentially stacked on the male mold core or the female mold core 101 by paving. During the paving process, different layers of prepreg 102 are prone to defects such as fiber wrinkles, fiber separation, and fiber deformation. During the lamination process, the male mold core and the female mold core 101 are molded together to extrude the prepreg 102. During the extrusion process, the prepreg 102 is deformed to form a set structure. In this process, fiber wrinkles are easily formed in the area with excess material. Sensitive areas can be effectively determined by simulating and analyzing the paving process and the lamination process.
[0051] In one embodiment of the present invention, the defect includes at least one of fiber wrinkles, fiber separation, and fiber deformation.
[0052] In this embodiment, fiber wrinkles refer to the bulging, stacking, etc. of the fibers of the prepreg 102 due to the formation of residual materials during the molding process. Fiber separation refers to the separation of fibers arranged in parallel moving perpendicular to the fiber direction. Fiber deformation refers to the deviation of the fiber direction from the initial direction. By providing a tensioning device to clamp the non-product area of the prepreg 102 and tension the prepreg 102, the above defects can be effectively reduced or even eliminated.
[0053] In one embodiment of the present invention, in the step of placing the prepreg 102 in the mold, tensioning the prepreg 102 using a tensioning device, and performing hot pressing molding, The prepreg 102 includes a thermosetting material, and the prepreg 102 is placed between the male mold core and the female mold core 101 of the mold and is compression molded.
[0054] In this embodiment, the prepreg 102 includes a thermosetting material and a fiber material. Thermosetting material refers to a resin material that undergoes chemical changes after heating, gradually solidifies into a shape, and does not soften when heated again. Optionally, epoxy resin and phenolic resin are both thermosetting materials, and the above materials are widely available and low in cost. One or more of these materials can be selected to prepare the prepreg 102. The fiber material is selected from at least one of carbon fiber, glass fiber, and aramid fiber. For example, the weaving method of the fiber material can be a single-layer, unidirectional weaving. The prepreg 102 is suitable for compression molding and has few defects in the preparation process of the composite material.
[0055] It can be that the prepreg 102 containing the thermosetting material is placed on the male mold core, the prepreg 102 is tensioned by a tensioning device, and then the female mold core 101 is molded on the male mold core.
[0056] Alternatively, the prepreg 102 containing the thermosetting material is placed on the female mold core 101 , the prepreg 102 is tensioned by a tensioning device, and then the male mold core is molded on the female mold core 101 .
[0057] In one embodiment of the present invention, the temperature of the mold is 100°C-160°C, the vacuum time is 100s-300s, and the molding pressure is 20 kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0058] In this embodiment, the prepreg 102 is placed on the male mold of the mold for hot pressing. The mold temperature is 100°C-160°C, the vacuum time is 100s-300s, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min. If the temperature of the mold is too low, the prepreg 102 is not easy to soften; conversely, if the temperature of the mold is too high, the thermosetting material is easy to solidify. Within this temperature range, the preform softens, and the gas in the mold can be effectively discharged through vacuuming, so that the prepreg 102 fully fills the gap between the male core and the female core 101. If the molding pressure is too low, it is easy to cause the structure of the product to be loose and it is difficult to achieve the required thickness; if the molding pressure is too high, the requirements for the molding equipment are high. Under the above molding pressure, the prepreg 102 reaches the set thickness and is easy to mold. Since the prepreg 102 contains thermosetting material, under the above molding time, the thermosetting material undergoes a chemical reaction and is solidified and molded, and finally forms a product with a set structure.
[0059] Optionally, the temperature of the mold is 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, etc. The vacuuming time is 100s, 150s, 200s, 250s, 300s, etc. The molding pressure is 20kgf / cm 2 、60kgf / cm 2 、80kgf / cm 2 、100kgf / cm 2 、120kgf / cm 2 、140kgf / cm 2 、160kgf / cm 2 、170kgf / cm 2 、180kgf / cm 2 The molding time is 0.5 min, 1.0 min, 1.5 min, 2.0 min, 2.5 min, 3.0 min, 3.5 min, 4.0 min, 4.5 min, 5 min, etc. The above values enable the prepreg 102 to form a set structure and be cured.
[0060] In one embodiment of the present invention, in the step of placing the prepreg 102 in the mold, tensioning the prepreg 102 using a tensioning device, and performing hot pressing molding, The prepreg 102 includes a thermoplastic material, and the prepreg 102 is placed between the male mold core and the female mold core 101 of the mold and is compression molded.
[0061] In this embodiment, the prepreg 102 includes a thermoplastic material and a fiber material. Thermoplastic material refers to a resin material that softens after heating and hardens after cooling. Optionally, polypropylene, nylon, polycarbonate, and polyetheretherketone are all thermoplastic materials, and one or more of them can be selected to prepare the prepreg 102. The fiber material is, for example, at least one of carbon fiber, glass fiber, and aramid fiber. The fiber material is woven into unidirectional tape, plain weave, twill or satin weave. The prepreg 102 is suitable for preforming and compression molding, and has few defects in the composite material preparation process.
[0062] It can be that the prepreg 102 containing thermoplastic material is placed on the male mold core, the prepreg 102 is tensioned by a tensioning device, and then the female mold core 101 is molded on the male mold core.
[0063] Alternatively, the prepreg 102 containing the thermoplastic material is placed on the female mold core 101 , the prepreg 102 is tensioned by a tensioning device, and then the male mold core is molded on the female mold core 101 .
[0064] In one embodiment of the present invention, infrared heating is used for compression molding, the infrared heating temperature is 300°C-600°C, the infrared heating time is 10s-100s; the temperature of the mold is 40°C-200°C, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0065] In this embodiment, infrared heating is used for compression molding. Infrared heating can directly heat the position of the prepreg 102 without heating the mold itself, that is, the mold can maintain a low temperature, so that after the compression molding is completed, the prepreg 102 can be quickly cooled down to harden the product, thereby reducing the time for heat dissipation of the product. The infrared heating method is particularly suitable for thermoplastic materials, which can quickly harden after the thermoplastic material is compression molded, thereby forming. If the compression molding is performed by directly heating the mold, the time required for the thermoplastic material to harden after compression molding is long because the mold cooling takes a long time. If the infrared heating temperature is too high and / or the heating time is too long, the prepreg 102 is easily damaged; conversely, if the infrared heating temperature is too low and / or the heating time is too short, the prepreg 102 is not easy to soften. The infrared heating temperature is 300℃-600℃, and the infrared heating time is 10s-100s. Within this range, the preform can be softened and the prepreg 102 can be prevented from being damaged due to the high temperature of the preform. The temperature of the mold is 40℃-200℃. Within this range, after the infrared heating is completed, the preform can be cooled quickly to maintain the set structure. The molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min. Within the above range, under the above molding pressure and molding time, the prepreg 102 can reach the set thickness and keep the thickness of each part uniform.
[0066] Optionally, the infrared heating temperature is 300°C, 400°C, 500°C, 600°C, etc., and the infrared heating time is 10s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, etc. The temperature of the mold is 40°C, 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, etc. The molding pressure is 20kgf / cm 2 、40kgf / cm 2 、60kgf / cm 2 、80kgf / cm 2 、100kgf / cm 2 、120kgf / cm 2 、140kgf / cm2 、160kgf / cm 2 、180kgf / cm 2 The molding time is 0.5min, 1.0min, 1.5min, 2.0min, 2.5min, 3.0min, 3.5min, 4.0min, 4.5min, 5min, etc. The above values can form the product into the set structure and reduce the processing time.
[0067] According to another embodiment of the present invention, a composite material is provided, which is prepared according to the composite material preparation method of the present invention.
[0068] The composite material has the characteristics of high molding precision, stable structure and high yield rate.
[0069] In a specific embodiment of the present invention, the thickness of the composite material is 0.2 mm-2 mm. For example, the thickness of the composite material is 0.2 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2 mm, etc. The above thicknesses all meet the requirements of thin and light electronic devices. In addition, the composite material has a good appearance without fiber wrinkles, fiber separation, fiber deformation, and other undesirable appearance phenomena.
[0070] According to another embodiment of the present invention, an electronic device is provided, which includes the composite material of the present invention.
[0071] Optionally, the electronic device is a computer, a mobile phone, a watch, a television, a speaker, an AR device, a VR device, etc. For example, the composite material is used to prepare a housing of an electronic device. The electronic device of the present invention also includes at least all the beneficial effects of the above embodiments.
[0072] The following is a detailed description of the composite material preparation method and the composite material according to the embodiment of the present invention in combination with specific embodiments and comparative examples. It is worth noting that the following description is only exemplary and not a specific limitation to the present invention.
[0073] Example 1 The prepreg 102 includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.3 mm and the prepreg is laid in a fiber direction of 0°, 90°, 90°, and 0°. The thermosetting material is epoxy resin.
[0074] Fibersim software and Pam-Composite software were used for simulation to analyze the degree and distribution of defects such as fiber wrinkles, fiber separation and fiber deformation generated during the laying and pressing process of the prepreg 102. According to the results of the simulation analysis, a block structure and a spring are set at the position of the mold (such as the male mold core) corresponding to the non-product area of the prepreg 102. The prepreg 102 is placed in the mold, and the block structure and the female mold core 101 extrude the non-product area of the prepreg 102 to tension the prepreg 102. Next, the mold is closed, the mold temperature is 130°C, the vacuum time is 150s, and the molding pressure is 30kgf / cm 2 The molding time is 3 minutes. Finally, a product with a set structure is obtained.
[0075] Example 2 The prepreg 102 includes glass fiber and thermosetting material, wherein the diameter of the glass fiber is 0.5 mm, and the fiber weaving method is plain weave. The thermosetting material is epoxy resin.
[0076] Fibersim software and Pam-Composite software were used for simulation to analyze the degree and distribution of defects such as fiber wrinkles, fiber separation and fiber deformation generated during the laying and pressing process of the prepreg 102. According to the results of the simulation analysis, a block structure and a spring are set at the position of the mold (such as the male mold core) corresponding to the non-product area of the prepreg 102. The prepreg 102 is placed in the mold, and the block structure and the female mold core 101 extrude the non-product area of the prepreg 102 to tension the prepreg 102. Next, the mold is closed, the mold temperature is 130°C, the vacuum time is 150s, and the molding pressure is 30kgf / cm 2 The molding time is 3 minutes. Finally, a product with a set structure is obtained.
[0077] Example 3 The prepreg 102 includes carbon fiber and thermoplastic material, wherein the diameter of the carbon fiber is 0.3 mm, and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate.
[0078] Fibersim software and Pam-Composite software were used for simulation to analyze the degree and distribution of defects such as fiber wrinkles, fiber separation and fiber deformation generated during the laying and pressing process of the prepreg 102. According to the results of the simulation analysis, a block structure and a spring are set at the position of the mold (such as the male mold core) corresponding to the non-product area of the prepreg 102. The prepreg 102 is placed in the mold, and the block structure and the female mold core 101 extrude the non-product area of the prepreg 102 to tension the prepreg 102. Next, the mold is closed, the mold temperature is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C and the heating time is 1min. The compression molding pressure is 100kgf / cm 2 The molding time is 1 min. Finally, a product with a set structure is obtained.
[0079] Example 4 The prepreg 102 includes glass fiber and thermoplastic material, wherein the diameter of the glass fiber is 0.5 mm, and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate.
[0080] Fibersim software and Pam-Composite software were used for simulation to analyze the degree and distribution of defects such as fiber wrinkles, fiber separation and fiber deformation generated during the laying and pressing process of the prepreg 102. According to the results of the simulation analysis, a block structure and a spring are set at the position of the mold (such as the male mold core) corresponding to the non-product area of the prepreg 102. The prepreg 102 is placed in the mold, and the block structure and the female mold core 101 extrude the non-product area of the prepreg 102 to tension the prepreg 102. Next, the mold is closed, the mold temperature is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C and the heating time is 1min. The compression molding pressure is 100kgf / cm 2 The molding time is 1 min. Finally, a product with a set structure is obtained.
[0081] Comparative Example 1 The prepreg 102 includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.3 mm, and the layers are laid in the fiber direction of 0°, 90°, 90°, and 0°. The thermosetting material is epoxy resin. The prepreg 102 obtained by laying is placed on the concave mold core 101 of the mold for compression molding. The mold temperature is 130°C, the vacuum time is 150s, and the compression molding pressure is 30kgf / cm 2 , the molding time is 3min.
[0082] Comparative Example 2 The prepreg 102 includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.5 mm and the fiber weaving method is plain weave. The thermosetting material is epoxy resin. The prepreg 102 obtained by plying is placed on the concave mold core 101 of the mold and subjected to compression molding. The mold temperature is 130°C, the vacuum time is 150s, and the compression molding pressure is 30kgf / cm 2 , the molding time is 3min.
[0083] Comparative Example 3 The prepreg 102 includes carbon fiber and thermoplastic material, wherein the diameter of the carbon fiber is 0.3 mm, and the fiber weaving method is unidirectional tape. The thermoplastic material is transparent polycarbonate. The prepreg 102 obtained by plying is placed on the concave mold core 101 of the mold for compression molding. The mold temperature is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C, the heating time is 1 minute, and compression molding is performed. The compression molding pressure is 100kgf / cm 2 ; The molding time is 1min.
[0084] Comparative Example 4 The prepreg 102 includes glass fiber and thermoplastic material, wherein the diameter of the glass fiber is 0.5 mm and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate. The prepreg 102 obtained by plying is placed on the concave mold core 101 of the mold for compression molding. The mold temperature is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C, the heating time is 1 minute, and compression molding is performed. The compression molding pressure is 100kgf / cm 2 ; The molding time is 1min.
[0085] The product appearance results of the embodiments and comparative examples are shown in Table 1.
[0086] Table 1 - Comparison of product appearance of examples and comparative examples
[0087] As can be seen from Table 1, the composite products prepared by the preparation method of the present invention in Examples 1-4 are bright in appearance, without fiber wrinkles, separation, deformation and other undesirable appearance phenomena. However, the composite products prepared by the preparation methods of Comparative Examples 1-4 are rough in appearance, with fiber wrinkles, separation, and deformation in some parts, which do not meet the appearance requirements. This shows that the use of simulation software can effectively determine the sensitive areas of the prepreg 102 during the molding process, that is, the areas where defects are easily formed. By pre-arranging a tensioning device on the mold outside the area and connecting the tensioning device to the prepreg 102, the prepreg 102 can be effectively positioned and tensioned, thereby effectively avoiding the local wrinkles, dislocation and other defects of the prepreg 102 caused by the extrusion deformation and displacement of the prepreg 102 during the molding process. The preparation method has a simple process, is easy to operate, and has a high yield rate of composite materials.
[0088] Take the composite material prepared by the preparation method of Example 1 and Comparative Example 1 as an example. Before placing the prepreg 102 in the mold, the preparation method of Example 1 first uses simulation software to simulate and analyze the stress and deformation of the prepreg 102 during the molding process. Through simulation analysis, the area where the prepreg 102 is prone to defects is determined. The use of simulation software can effectively determine the sensitive area of the prepreg 102 during the molding process, that is, the area where defects are prone to form. By pre-arranging a tensioning device on the mold outside the area and connecting the tensioning device to the prepreg 102, the prepreg 102 can be effectively positioned and tensioned, thereby effectively avoiding the defects such as fiber wrinkles, fiber separation, and fiber deformation in the prepreg 102 caused by the extrusion deformation and displacement of the prepreg 102 during the molding process. Therefore, the surface of the composite material of Example 1 is bright, without fiber wrinkles, separation, deformation and other bad appearance phenomena. The preparation method of comparative example 1 produces excess material during the molding process of the prepreg 102 , and the excess material will form fiber wrinkles, separation, and deformation on the product when stretched or squeezed.
[0089] The above embodiments focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.
[0090] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A method for preparing a composite material, characterized in that: include: Use simulation software to simulate and analyze the prepreg molding process to determine sensitive areas where defects are likely to form; According to the simulation analysis results, a tensioning device is arranged outside the portion corresponding to the sensitive area in the mold, and the tensioning device is used to tension the sensitive area of the prepreg; The prepreg is placed in the mold, tensioned by a tensioning device, and hot-pressed.
2. The method for preparing a composite material according to claim 1, characterized in that: The simulation software includes at least one of Fibersim software, Ansys software, and Pam-Composite software.
3. The method for preparing a composite material according to claim 1, characterized in that: The tensioning device includes a pre-pressing device, and the pre-pressing device includes an elastic member and a block structure abutting against the elastic member. When the mold is closed, the block structure abuts against another mold core of the mold or against the block structure located on another mold core; Alternatively, the tensioning device comprises a traction device, and the traction device comprises a clamping device for clamping the prepreg.
4. The method for preparing a composite material according to claim 1, characterized in that: Before the step of placing the prepreg in the mold, tensioning the prepreg with a tensioning device, and performing hot pressing molding, the method further includes: The simulation software is used to simulate and analyze the molding process of the prepreg after being tensioned by the tensioning device, and hot pressing molding is performed under the condition that the defects in the sensitive area meet the requirements.
5. The method for preparing a composite material according to claim 1, characterized in that: The step of using simulation software to simulate and analyze the molding process of the prepreg to determine the sensitive area where defects are easily formed includes: The laying process and pressing process of the prepreg are simulated and analyzed.
6. The method for preparing a composite material according to claim 1, characterized in that: The defects include at least one of fiber wrinkles, fiber separation, and fiber dislocation.
7. The method for preparing a composite material according to claim 1, characterized in that: In the step of placing the prepreg in the mold, tensioning the prepreg with a tensioning device, and performing hot pressing molding, The prepreg comprises a thermosetting material, and the prepreg is placed between a male mold core and a female mold core of the mold and is compression molded.
8. The method for preparing a composite material according to claim 7, characterized in that: The temperature of the mold is 100°C-160°C, the vacuum time is 100s-300s, and the molding pressure is 20 kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
9. The method for preparing a composite material according to claim 1, characterized in that: In the step of placing the prepreg in the mold, tensioning the prepreg with a tensioning device, and performing hot pressing molding, The prepreg comprises a thermoplastic material, and the prepreg is placed between a male mold core and a female mold core of the mold and is compression molded.
10. The method for preparing a composite material according to claim 9, characterized in that: Infrared heating is used for compression molding, the infrared heating temperature is 300℃-600℃, the infrared heating time is 10s-100s; the temperature of the mold is 40℃-200℃, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
11. A composite material, characterized in that: The composite material is prepared according to the method for preparing the composite material according to any one of claims 1 to 10.
12. The composite material according to claim 11, characterized in that The thickness of the composite material is 0.2 mm-2 mm.
13. An electronic device, characterized in that: Comprising the composite material as claimed in claim 11 or 12.
Citation Information
Patent Citations
Composite material prepreg laminated plate mold pressing forming mechanism and forming method thereof
CN111844810A
Simulation analysis method for honeycomb sandwich structure aircraft skin detection
CN113533433A
Manufacturing method of light-weight side wall outer plate
CN116374009A
Defect prediction method and device for wide-temperature-range shaping process of multi-layer thermoplastic prepreg
CN116992786A
Compression molding device, method and equipment for composite material battery cover
CN117067634A