Anti-corrosion wear-resistant waterproof coiled material and preparation method thereof

By combining the polyester nonwoven base layer, corrosion-proof layer, wear-resistant layer and waterproof layer in the coil, the problem of insufficient chemical resistance and environmental adaptability of traditional materials is solved, and a longer service life and higher Reliability and durability.

CN118906586AInactive Publication Date: 2024-11-08QUZHOU YIWO TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410973549.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional anti-corrosion, wear-resistant and waterproof materials face problems in modern industries and buildings with insufficient chemical resistance, physical strength and environmental adaptability, and cannot effectively block the long-term penetration and mechanical wear of corrosive media, resulting in a shorter service life and an increased maintenance cost. .

Method used

A composite coil consisting of a polyester non-woven base layer, anti-corrosion layer, wear-resistant layer and waterproof layer. The anti-corrosion layer consists of epoxy resin, polyamide resin, glass flakes, zinc phosphate anti-rust pigment and mica powder, which is wear-resistant The layer consists of polyurethane resin, silicon carbide particles, ceramic microbeads and talc powder, and the waterproof layer consists of asphalt, SBS modifier and rubber powder. A multi-layer structure is formed through a specific process to enhance performance.

Benefits of technology

It achieves excellent corrosion resistance, wear resistance and waterproof performance, extends service life, improves reliability and overall toughness in humid environments, and is suitable for a variety of harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906586A_ABST
    Figure CN118906586A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coiled materials, and discloses an anti-corrosion and wear-resistant waterproof coiled material and a preparation method thereof.The anti-corrosion and wear-resistant waterproof coiled material comprises a polyester non-woven fabric base layer, an anti-corrosion layer, a wear-resistant layer and a waterproof layer which are sequentially arranged; the anti-corrosion layer is prepared from the following raw materials in parts by weight: 40 parts of epoxy resin, 25 parts of polyamide resin, 20 parts of glass flakes, 8 parts of zinc phosphate anti-rust pigment and 8 parts of mica powder; the wear-resistant layer is prepared from the following raw materials in parts by weight: 50 parts of polyurethane resin, 15 parts of silicon carbide particles with the particle size of 20-40 microns, 10 parts of silicon dioxide particles with the particle size of 10-15 microns and 8 parts of ceramic microbeads with the particle size of 60-80 microns. Through specific raw materials and processes, the performance advantages of all the layers are fully exerted, and the coiled material has excellent corrosion resistance, can resist various corrosive media, prolongs the service life, has excellent waterproof performance, effectively prevents water permeation and keeps reliable protection in a humid environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, in particular to an anticorrosive and wear-resistant waterproof coiled material and a preparation method thereof. Background Art

[0002] In the modern industrial and construction fields, with the advancement of science and technology and the changing environmental conditions, the performance requirements for waterproof materials are also constantly increasing, especially in some extreme environments, such as highly corrosive chemical storage, offshore platform construction, sewage treatment systems and other scenarios.

[0003] In modern industry and construction, traditional anti-corrosion, wear-resistant and waterproof materials face multiple challenges. These materials usually have obvious deficiencies in chemical resistance, physical strength or environmental adaptability. For example, they may not effectively block the long-term penetration of corrosive media, or fail quickly after mechanical wear. In addition, the waterproof performance of traditional materials is often limited and cannot provide lasting protection in wet environments. These defects not only shorten the service life of the material, but also increase maintenance costs and reduce the overall reliability of the system. Therefore, it has become particularly urgent to develop a composite material that can overcome these defects of the existing technology. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides an anti-corrosion and wear-resistant waterproof coiled material and a preparation method thereof, aiming to solve the problems of insufficient performance and environmental adaptability of the waterproof materials in the prior art.

[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: an anti-corrosion, wear-resistant and waterproof coiled material, comprising a polyester non-woven fabric base, an anti-corrosion layer, a wear-resistant layer and a waterproof layer arranged in sequence, the anti-corrosion layer is made of the following raw materials in parts by weight: 40 parts of epoxy resin, 25 parts of polyamide resin, 20 parts of glass flakes, 8 parts of zinc phosphate anti-rust pigment and 8 parts of mica powder; the wear-resistant layer is made of the following raw materials in parts by weight: 50 parts of polyurethane resin, 15 parts of silicon carbide particles with a particle size of 20-40μm, 10 parts of silicon dioxide particles with a particle size of 10-15μm and 8 parts of ceramic microbeads with a particle size of 60-80μm; the waterproof layer is made of the following raw materials in parts by weight: 90 parts of asphalt, 10 parts of SBS modifier and 15 parts of rubber powder.

[0006] Preferably, 5 parts of aluminum tripolyphosphate anti-rust pigment are added to the anti-corrosion layer to further enhance the anti-corrosion effect.

[0007] Preferably, the wear-resistant layer further comprises 8 parts of talcum powder to improve the processing performance and surface smoothness of the wear-resistant layer.

[0008] Preferably, a method for preparing an anticorrosive, wear-resistant and waterproof coiled material comprises the following steps:

[0009] S1. Preparation of anti-corrosion layer: epoxy resin, polyamide resin, glass flakes, zinc phosphate anti-rust pigment, mica powder and aluminum tripolyphosphate anti-rust pigment are put into a high-speed mixer in proportion, stirred at a stirring speed of 600r / min for 30 minutes to mix them evenly, and then a scraper is used to evenly coat the mixed materials on a polyester non-woven fabric base with a thickness of 0.8mm. The coating thickness is controlled at 0.8mm. Finally, the coated coil is placed in an oven and cured at a temperature of 90°C for 2.5 hours to form an anti-corrosion layer;

[0010] S2. Prepare the wear-resistant layer: Add polyurethane resin, silicon carbide particles, silicon dioxide particles, ceramic microbeads and talcum powder in proportion to a high-powered mixer, stir at a stirring speed of 800r / min for 45 minutes to ensure that the materials are fully mixed, and then use a scraper to apply the mixed material on the formed anti-corrosion layer with a coating thickness of 1.5mm. Subsequently, place the coil in a heating furnace and cure it at a temperature of 130°C for 2 hours to form a wear-resistant layer;

[0011] S3. Prepare waterproof layer: heat the asphalt to 170℃ to make it molten, then add SBS modifier and rubber powder to the molten asphalt, stir for 60 minutes at a stirring speed of 400r / min to make the components evenly distributed, finally use a scraper to coat the stirred material on the wear-resistant layer with a coating thickness of 2.5mm, and naturally cool and shape at room temperature to obtain an anti-corrosion and wear-resistant waterproof membrane.

[0012] Preferably, in the process of preparing the anti-corrosion layer, the wear-resistant layer and the waterproof layer, after each coating is completed, a pressure roller is used to compact the coating to remove bubbles in the coating.

[0013] Preferably, the polyester non-woven fabric substrate needs to be pretreated before use, and the pretreatment step includes uniformly spraying a layer of coupling agent on its surface and drying it at 60° C. for 1 hour.

[0014] Preferably, during the curing process of preparing the anti-corrosion layer and the wear-resistant layer, the oven or the heating furnace is kept well ventilated to discharge the small molecule volatiles generated during the curing process.

[0015] Preferably, the blade angle of the scraper is 30-45 degrees to ensure coating uniformity and coating thickness accuracy.

[0016] Preferably, after the waterproof layer is cooled and formed, the surface flatness and thickness of the coiled material are tested, and the parts that do not meet the requirements are trimmed or re-prepared.

[0017] The present invention provides an anticorrosive, wear-resistant and waterproof coiled material and a preparation method thereof. It has the following beneficial effects:

[0018] 1. The preparation method of the anti-corrosion, wear-resistant and waterproof coiled material of the present invention is scientific and reasonable. Through specific raw materials and processes, the performance advantages of each layer are fully utilized. The coiled material has excellent anti-corrosion performance, can resist a variety of corrosive media, and prolongs its service life. At the same time, it has excellent waterproof performance, effectively prevents moisture penetration, maintains reliable protection in a humid environment, and is suitable for different environmental conditions.

[0019] 2. The coiled material of the present invention has good wear resistance, can withstand frequent friction and mechanical impact, is not easy to be damaged and worn, and the synergistic effect of each layer of material enhances the overall toughness and crack resistance, improves durability and reliability, and the quality is strictly controlled during the preparation process to ensure that the product meets the requirements and has stable performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a cross-sectional view of the waterproof membrane of the present invention.

[0021] Among them, 1. Polyester non-woven fabric base layer; 2. Anti-corrosion layer; 3. Wear-resistant layer; 4. Waterproof layer. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] Please see attached Figure 1 An embodiment of the present invention provides an anti-corrosion, wear-resistant and waterproof coiled material, comprising a polyester non-woven fabric base, an anti-corrosion layer, a wear-resistant layer and a waterproof layer which are arranged in sequence, wherein the anti-corrosion layer is made of the following raw materials in parts by weight: 40 parts of epoxy resin, 25 parts of polyamide resin, 20 parts of glass flakes, 8 parts of zinc phosphate anti-rust pigment, 8 parts of mica powder and 5 parts of aluminum tripolyphosphate anti-rust pigment; the wear-resistant layer is made of the following raw materials in parts by weight: 50 parts of polyurethane resin, 15 parts of silicon carbide particles with a particle size of 30 μm, 10 parts of silicon dioxide particles with a particle size of 12 μm, 8 parts of ceramic microbeads with a particle size of 70 μm and 8 parts of talc; the waterproof layer is made of the following raw materials in parts by weight: 90 parts of asphalt, 10 parts of SBS modifier and 15 parts of rubber powder.

[0025] Specifically, for the anti-corrosion layer:

[0026] The combination of epoxy resin and polyamide resin forms a strong and stable polymer network structure, which significantly improves the adhesion and chemical corrosion resistance of the coating, can effectively resist the erosion of various corrosive media, and extend the service life of the coil; the addition of glass flakes forms a multi-layer barrier in the coating, hinders the penetration path of corrosion factors, greatly enhances the anti-corrosion performance, and enables the coil to maintain a good protective effect in harsh corrosive environments; the synergistic effect of zinc phosphate anti-rust pigment and aluminum tripolyphosphate anti-rust pigment further enhances the anti-rust and anti-corrosion capabilities and effectively inhibits the rust reaction of the metal substrate; the presence of mica powder improves the weather resistance and insulation of the coating, enabling it to work stably under different climatic conditions, while improving the electrical insulation performance of the coil, increasing the safety and reliability of use;

[0027] For the wear layer:

[0028] As the main component, polyurethane resin provides excellent flexibility and wear resistance, enabling the coil to withstand frequent friction and mechanical impact, and is not prone to breakage and wear; silicon carbide particles, silicon dioxide particles and ceramic microbeads of specific particle sizes are evenly distributed in the polyurethane resin, which significantly improves the hardness and wear resistance of the coating and effectively resists external wear and scratches; the addition of talcum powder not only improves the processing performance of the wear-resistant layer, making it easier to operate and shape during the preparation process, but also improves the surface flatness of the coating, reduces surface defects, and enhances the aesthetics and protective performance;

[0029] For waterproof layer:

[0030] The high proportion of asphalt provides the membrane with excellent waterproof performance, forming a continuous and dense waterproof layer, effectively preventing the penetration of water and ensuring that the membrane plays a reliable waterproof role in a humid environment; the introduction of SBS modifier improves the high and low temperature performance of asphalt, so that it can still maintain good flexibility and elasticity under extreme temperature conditions, avoiding cracking and embrittlement caused by temperature changes; the addition of rubber powder increases the toughness and crack resistance of asphalt, further improving the overall durability and reliability of the waterproof membrane.

[0031] Embodiment 2:

[0032] The embodiment of the present invention provides a method for preparing an anticorrosive, wear-resistant and waterproof coiled material, comprising the following steps:

[0033] S1. Preparation of anti-corrosion layer:

[0034] Weigh 40 parts of epoxy resin, 25 parts of polyamide resin, 20 parts of glass flakes, 8 parts of zinc phosphate antirust pigment, 8 parts of mica powder and 5 parts of aluminum tripolyphosphate antirust pigment. Put these raw materials into a high-speed mixer and stir at a speed of 600r / min for 30 minutes. During the stirring process, the various raw materials are fully integrated, and the epoxy resin and polyamide resin interact with each other to form a stable cross-linked structure. The glass flakes are evenly distributed and can effectively block the penetration of corrosive media. The zinc phosphate antirust pigment and aluminum tripolyphosphate antirust pigment work synergistically to enhance the anti-corrosion performance. The addition of mica powder improves the weather resistance and insulation of the coating.

[0035] Then, use a scraper to evenly coat the mixed material on a 0.8mm thick polyester non-woven fabric base layer, and the coating thickness is controlled at 0.8mm. The polyester non-woven fabric base layer provides good strength and support, allowing the anti-corrosion layer to adhere firmly.

[0036] After coating, the coil is placed in an oven and cured at 90°C for 2.5 hours. During the curing period, the resin system further cross-links and solidifies to form a dense anti-corrosion layer, providing reliable anti-corrosion protection for the coil.

[0037] S2. Preparation of wear-resistant layer:

[0038] Weigh 50 parts of polyurethane resin, 15 parts of silicon carbide particles with a particle size of 20-40μm, 10 parts of silicon dioxide particles with a particle size of 10-15μm, 8 parts of ceramic microspheres with a particle size of 60-80μm and 8 parts of talcum powder according to the proportion. Add them to a high-powered mixer and stir at a speed of 800r / min for 45 minutes. During stirring, the polyurethane resin fully wraps the various particles to form a uniform mixture. Silicon carbide particles provide excellent wear resistance, silicon dioxide particles enhance the hardness and wear resistance of the coating, ceramic microspheres help reduce the weight of the coating and improve thermal insulation performance, and talcum powder improves processing performance and surface smoothness.

[0039] Subsequently, the mixed material is coated on the formed anticorrosion layer with a scraper, with a coating thickness of 1.5 mm. The multi-layer coating structure enhances the comprehensive performance of the coil.

[0040] After that, the coil is placed in a heating furnace and cured for 2 hours at 130°C. The curing process fully solidifies the polyurethane resin to form a tough wear-resistant layer, which improves the wear resistance and corrosion resistance of the coil.

[0041] S3. Preparation of waterproof layer:

[0042] First, heat 90 parts of asphalt to 170℃ to melt it, then add 10 parts of SBS modifier and 15 parts of rubber powder, and stir at 400r / min for 60 minutes. The SBS modifier improves the high and low temperature performance of the asphalt, and the rubber powder increases the flexibility and crack resistance of the asphalt.

[0043] Next, the stirred material is applied to the wear-resistant layer with a scraper to a thickness of 2.5 mm and then cooled naturally at room temperature to form. The thicker asphalt layer provides excellent waterproofing properties, ensuring that the membrane is effectively waterproof in a humid environment.

[0044] During the entire preparation process, after each coating is completed, a pressure roller is used to compact the coating to eliminate bubbles in the coating, making the coating denser and improving the protective effect.

[0045] Before using the polyester non-woven fabric base layer, a layer of coupling agent is evenly sprayed on its surface and dried at 60°C for 1 hour to enhance the bonding strength between the base layer and the anti-corrosion layer.

[0046] During the curing process of the anti-corrosion layer and the wear-resistant layer, the oven or heating furnace should be well ventilated to discharge small molecule volatiles in time to ensure the curing quality and coating performance.

[0047] The blade angle of the scraper is 30-45 degrees, ensuring the uniformity of coating and the accuracy of coating thickness.

[0048] After the waterproof layer is cooled and formed, the surface flatness and thickness of the coil are tested, and the parts that do not meet the requirements are trimmed or re-prepared, strictly controlling the product quality and ensuring the performance and use effect of the coil.

[0049] The anti-corrosion, wear-resistant and waterproof coiled material prepared by the above-mentioned embodiment has excellent comprehensive performance and can meet the use requirements in various harsh environments.

[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An anticorrosive, wear-resistant and waterproof coiled material, characterized in that: The invention comprises a polyester non-woven fabric base layer (1), an anti-corrosion layer (2), a wear-resistant layer (3) and a waterproof layer (4) which are arranged in sequence, wherein the anti-corrosion layer (2) is made of the following raw materials in parts by weight: 40 parts of epoxy resin, 25 parts of polyamide resin, 20 parts of glass flakes, 8 parts of zinc phosphate anti-rust pigment and 8 parts of mica powder; the wear-resistant layer (3) is made of the following raw materials in parts by weight: 50 parts of polyurethane resin, 15 parts of silicon carbide particles with a particle size of 20-40 μm, 10 parts of silicon dioxide particles with a particle size of 10-15 μm and 8 parts of ceramic microbeads with a particle size of 60-80 μm; and the waterproof layer (4) is made of the following raw materials in parts by weight: 90 parts of asphalt, 10 parts of SBS modifier and 15 parts of rubber powder.

2. The anticorrosion, wear-resistant and waterproof coiled material according to claim 1, characterized in that: The anti-corrosion layer (2) is also added with 5 parts of aluminum tripolyphosphate anti-rust pigment to further enhance the anti-corrosion effect.

3. The anticorrosion, wear-resistant and waterproof coiled material according to claim 1, characterized in that: The wear-resistant layer (3) also contains 8 parts of talcum powder, which is used to improve the processing performance and surface smoothness of the wear-resistant layer (3).

4. A method for preparing an anti-corrosion, wear-resistant and waterproof coiled material, using the anti-corrosion, wear-resistant and waterproof coiled material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Preparation of anticorrosion layer (2): epoxy resin, polyamide resin, glass flakes, zinc phosphate antirust pigment, mica powder and aluminum tripolyphosphate antirust pigment are added into a high-speed mixer in proportion, stirred at a stirring speed of 600 r / min for 30 minutes to make them uniformly mixed, and then the mixed materials are evenly coated on a polyester non-woven fabric base layer (1) with a thickness of 0.8 mm using a scraper, and the coating thickness is controlled to be 0.8 mm. Finally, the coated coil is placed in an oven and cured at a temperature of 90° C. for 2.5 hours to form an anticorrosion layer (2); S2. Preparation of wear-resistant layer (3): polyurethane resin, silicon carbide particles, silicon dioxide particles, ceramic microbeads and talcum powder are added to a high-powered mixer in proportion, stirred at a stirring speed of 800 r / min for 45 minutes to ensure that the materials are fully mixed, and then the mixed material is coated on the formed anti-corrosion layer (2) with a scraper, and the coating thickness is 1.5 mm. Subsequently, the coil is placed in a heating furnace and cured at a temperature of 130°C for 2 hours to form a wear-resistant layer (3); S3. Preparation of waterproof layer (4): Heat the asphalt to 170°C to make it molten, then add SBS modifier and rubber powder to the molten asphalt, stir for 60 minutes at a stirring speed of 400r / min to make the components evenly distributed, and finally use a scraper to coat the stirred material on the wear-resistant layer (3) with a coating thickness of 2.5mm, and naturally cool and shape it at room temperature to obtain an anti-corrosion and wear-resistant waterproof membrane.

5. The method for preparing the anticorrosive, wear-resistant and waterproof coiled material according to claim 4, characterized in that: In the process of preparing the anti-corrosion layer (2), the wear-resistant layer (3) and the waterproof layer (4), after each coating is completed, a pressure roller is used to compact the coating to remove bubbles in the coating.

6. The method for preparing the anticorrosive, wear-resistant and waterproof coiled material according to claim 4, characterized in that: The polyester non-woven fabric base layer (1) needs to be pretreated before use, and the pretreatment step includes spraying a layer of coupling agent uniformly on its surface and drying it at 60° C. for 1 hour.

7. The method for preparing the anticorrosive, wear-resistant and waterproof coiled material according to claim 4, characterized in that: During the curing process of preparing the anti-corrosion layer (2) and the wear-resistant layer (3), good ventilation is maintained in the oven or heating furnace to discharge small molecule volatiles generated during the curing process.

8. The method for preparing the anticorrosive, wear-resistant and waterproof coiled material according to claim 4, characterized in that: The blade angle of the scraper is 30-45 degrees, ensuring the uniformity of coating and the thickness accuracy of the coating.

9. The method for preparing the anticorrosive, wear-resistant and waterproof coiled material according to claim 4, characterized in that: After the waterproof layer (4) is cooled and formed, the surface flatness and thickness of the coiled material are tested, and the parts that do not meet the requirements are trimmed or re-prepared.

Citation Information

Patent Citations

  • Wear-resistant anticorrosive self-adhesive polymer-modified asphalt waterproof coiled material

    CN105328942A

  • Anti-aging and water-proof roll and preparation method

    CN106835733A

  • Wearing-resistant reinforced polyurethane material and preparation method thereof

    CN107760012A

  • Nano-modified epoxy heavy-duty anti-corrosion coating

    CN111004557A

  • Modified asphalt waterproofing membrane layer structure

    CN205291759U