Stretch-resistant foaming diffusion plate and preparation method thereof
The generation of uniform bubble cells by dissolving gas release method and the arrangement of nanocellulose-based carbon dot composite films around the foam core layer solves the deformation and edge blue light leakage of the quantum dot diffusion plate in high temperature and high humidity environment, and improves the resistance of the quantum dot diffusion plate. Tensile properties and light uniformity.
Patent Information
- Application Number
- CN202411075105.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing quantum dot diffusion plates are prone to deform and warping in high temperature and high humidity environments, resulting in brightness attenuation and severe leakage of blue light at the edges, affecting the display effect.
Micro-nano bubbles are generated by the dissolved gas release method to form a uniform cell structure, and a nanocellulose-based carbon dot composite film is installed around the foam core layer to improve tensile resistance and edge blue light utilization.
It improves the deformation resistance and light uniformity of the foamed diffusion plate, reduces the leakage of edge blue light and the darkness of the surrounding frames, and enhances brightness and color performance.
Smart Images

Figure CN118906596A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of diffusion plates, and in particular to a stretch-resistant foaming diffusion plate and a preparation method thereof. Background Art
[0002] Liquid crystal display is a flat-panel display technology widely used in electronic devices, such as computer monitors, televisions, mobile phones, and tablet computers. It uses the optical properties of liquid crystal molecules to display images. The basic structure of a liquid crystal display consists of several layers, one of the key components of which is the diffuser. The diffuser is located between the backlight source and the liquid crystal panel. The backlight source is usually an LED light bar. Since the light generated by the backlight source itself is often not uniform, the role of the diffuser is to evenly distribute the light to the entire liquid crystal screen through its special optical design. The use of quantum dot light source conversion materials combined with blue light backlights can achieve a wider color gamut, allowing the display to present more realistic and vivid colors. However, as people's requirements for visual experience increase, the problems faced by liquid crystal displays have gradually become prominent, one of which is the problem of edge blue light. Edge blue light refers to the phenomenon that when a liquid crystal display displays an image, if a quantum dot backlight solution is used, the surrounding blue light is not fully excited, and a visual blue frame may appear. Blue light leakage is more harmful to the human eye.
[0003] Conventional direct-type backlight modules have limited luminous angles and short optical paths, so insufficient light energy reaches the four sides and corners, which easily leads to dark frames on the four sides. By improving the utilization rate of light at the edge of the diffuser plate of the light-evening component, the problem of dark edges of the diffuser plate of the light-evening component can be solved.
[0004] In order to save costs, the industry has been working hard to disperse quantum dots into diffusers. However, since quantum dots are easily oxidized, this method has limitations in the production and application of quantum dot diffuser plates. In order to solve this problem, the prior art discloses a new method for preparing a quantum dot optical functional plate. Specifically, the method first uses a raw material containing a chemical foaming agent to prepare a resin-based granular material with holes, and then loads the quantum dots into the holes. Next, a high-temperature foaming agent and other components are added for mixing, and extrusion molding is performed to finally obtain a quantum dot optical functional plate. For example, a Chinese patent application number CN202010812282.0 and a patent name "Light Diffuser Plate and Method for Making It" discloses a foamed quantum dot diffuser plate. The diffuser has a pore diameter between 60-400 μm. Obviously, due to the large pore size and uneven distribution formed by the chemical foaming agent, the number of reflections and refractions of light in the pores is reduced, thereby reducing the effect of uniform light. In addition, the larger pore diameter also leads to a decrease in the strength of the quantum dot optical functional board, which is prone to deformation and warping, especially in high temperature and high humidity environments, further leading to increased brightness attenuation. Summary of the invention
[0005] The purpose of the present invention is to provide a stretch-resistant foam diffuser plate and a preparation method thereof, using the dissolved gas release method to improve the distribution uniformity of the bubbles in the foam core layer, and at the same time using a nanocellulose-based carbon dot composite film to increase the stretch resistance of the foam diffuser plate and reduce the leakage of edge blue light.
[0006] In order to achieve the above object, the present invention adopts the following technical solution: A stretch-resistant foam diffusion plate comprises a foam core layer, an upper protective layer, a lower protective layer, and a nanocellulose-based carbon dot composite film; the upper protective layer is arranged on the upper surface of the foam core layer, the lower protective layer is arranged on the lower surface of the foam core layer, the nanocellulose-based carbon dot composite film is arranged on four sides of the foam core layer close to the upper surface, and the arrangement width of the nanocellulose-based carbon dot composite film is less than the thickness of the foam core layer and does not completely cover the foam core layer; preferably, the width of the nanocellulose-based carbon dot composite film arranged on the four sides of the foam core layer accounts for 1 / 8 of the thickness of the foam core layer.
[0007] The thickness ratio of the foamed core layer to the upper protective layer or the lower protective layer is 7:1-9:1.
[0008] The upper protective layer and the lower protective layer are made of the same material, and the raw materials thereof include, by mass percentage: an optical resin matrix content of 98% to 99.8%, a light diffuser content of 0.2% to 1%, an antioxidant content of 0.2% to 1%, a weathering agent content of 0.02% to 1%, a lubricant content of 0% to 0.5%, and an anti-ultraviolet agent content of 0.2% to 1%.
[0009] The raw materials of the foaming core layer include, by mass percentage: 98% to 99.8% of optical resin matrix, the optimal value is 99%, 0.1% to 1% of red quantum dots, the optimal value is 0.2%, 0.1% to 1% of green quantum dots, the optimal value is 0.8%, and 0.2% to 1% of nucleating agent. The particle size of the quantum dots is 2-12nm. A plurality of pores are formed inside the foaming core layer.
[0010] As a preferred solution, the optical resin matrix is one or more of polycarbonate (PC), polymethyl methacrylate (PMMA), polystyrene (GPPS), styrene-methyl methacrylate copolymer (MS) or polypropylene (PP).
[0011] As a preferred embodiment, the light diffuser is one or more of titanium dioxide, silicon dioxide, calcium sulfate, barium sulfate, zinc oxide, organic silicon, and PS microspheres.
[0012] As a preferred embodiment, the antioxidant can be one or more of hindered phenol antioxidants, phosphite antioxidants, metal alkylthiophosphoric acid antioxidants, carbamic acid antioxidants, and organic sulfur antioxidants.
[0013] As a preferred solution, the weathering agent includes a hindered amine light stabilizer and / or an ultraviolet absorber.
[0014] As a preferred embodiment, the lubricant is at least one of vinyl bisstearamide, stearate, polysiloxane, PP wax, PE wax, polysiloxane, and ethylene bisfatty acid amide.
[0015] As a preferred embodiment, the anti-ultraviolet agent is benzotriazole, and hydroxybenzophenone and benzotriazole are used in combination.
[0016] As a preferred embodiment, the quantum dots are composed of quantum dots of CdS, CdSe, CdSeS, ZnS, ZnSe, ZnSeS, ZnCdSeS, InP, CuInS, GaN, GaP, GaAs, InN, InP, InGaP, GalnNP and perovskite types.
[0017] As a preferred embodiment, the nucleating agent is at least one of boron nitride, sodium carbonate, calcium carbonate, ultrafine talc, mica, montmorillonite, silicon dioxide, titanium dioxide, apatite, and magnesium aluminum hydrotalcite.
[0018] As a preferred embodiment, the yellow carbon dots in the nanocellulose-based carbon dot composite film are composed of yellow quantum dots such as CdS, CdSe, CdSeS, ZnS, ZnSe, ZnSeS, ZnCdSeS, InP, CuInS, GaN, GaP, GaAs, InN, InP, InGaP, GalnNP and perovskite.
[0019] As a preferred solution, the upper protective layer and the lower protective layer are provided with patterns on the side away from the foaming core layer to improve the refraction and reflection performance of light.
[0020] A method for preparing a stretch-resistant foaming diffusion plate comprises the following steps: S1, preparing two portions of protective layer raw materials with the same composition, one portion of foaming core layer raw material, and one portion of nanocellulose-based carbon dot composite film; S2, mixing the protective layer raw material and the foaming core layer raw material respectively and uniformly; S3, adding the mixed protective layer raw materials into a screw extruder to heat them to form a molten state; after heating the mixed foaming core layer raw materials to form a molten state, generating micro-nano bubbles by a dissolved gas release method, and then adding them to the screw extruder; cutting the nanocellulose-based carbon dot composite film and adding it to the screw extruder; S4. Finally, the upper protective layer, the foaming core layer and the lower protective layer are extruded through the die head of the screw extrusion equipment in the form of sheets, and the nano-cellulose-based carbon dot composite film is extruded in the form of strips. The upper protective layer is arranged on the upper surface of the foaming core layer, and the lower protective layer is arranged on the lower surface of the foaming core layer. The nano-cellulose-based carbon dot composite film is arranged on the four sides of the foaming core layer close to the upper surface, and the arrangement width of the nano-cellulose-based carbon dot composite film is smaller than the thickness of the foaming core layer, and does not completely cover the foaming core layer.
[0021] As a preferred embodiment, the screw extruder in step S3 includes three heating zones, the temperature of the first heating zone is 140-220°C, the temperature of the second heating zone is 160-240°C, and the temperature of the third heating zone is 180-260°C.
[0022] As a preferred solution, the gas used in the dissolved gas release method in step S3 is CO2 or nitrogen, or other inert gases.
[0023] As a preferred solution, the temperature control range of the die extrusion in step S4 is 170-260°C.
[0024] As a preferred solution, the screw extruder in step S4 is provided with a plurality of feed ports, so that a variety of different raw materials can be put into the screw extruder.
[0025] The beneficial effects of a foaming diffusion plate disclosed in the present invention are as follows: micro-nano bubbles are generated in the foaming core layer by a dissolved gas release method, the pore size is greatly reduced, the pore size is more uniform, the force is more uniform, and the deformation resistance is improved; at the same time, a nano-cellulose-based carbon dot composite film is arranged on the edges (four sides) of the foaming core layer close to the upper protective layer, so the tensile resistance of the foaming diffusion plate and the ability to utilize edge blue light are improved, and the blue light leakage at the edge of the diffusion plate and the dark borders on the surrounding edges are reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a flow chart of the preparation of the yellow carbon dots described in the present invention.
[0027] Figure 2 It is a flow chart of the preparation of the nanocellulose described in the present invention.
[0028] Figure 3 It is a flow chart for preparing the nanocellulose-based carbon dot composite film described in the present invention.
[0029] Figure 4 It is a top view of the nano-cellulose-based carbon dot composite film of the present invention arranged around the foaming core layer.
[0030] Figure 5It is a side view of the stretch-resistant foam diffuser plate of the present invention.
[0031] Figure 6 It is a cross-sectional view of the stretch-resistant foam diffuser plate of the present invention.
[0032] Figure 7 This is a TEM image of the nanocellulose-based carbon dot composite film prepared in Example 1 of the present invention.
[0033] Description of the numbers in the figure: 1. Upper protective layer and lower protective layer; 2. Nanocellulose-based carbon dot composite film; 30. Foaming core layer; 31. Red quantum dots; 32. Green quantum dots; 33. Cells distributed in the foaming core layer. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0035] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0037] Example 1 The optical resin selected in this example is polystyrene, the light diffuser is methyl phenyl silicone resin (organic silicone), the antioxidant is 1076 antioxidant, the anti-ultraviolet agent is benzotriazole, the red and green quantum dots are CdSe quantum dots, the weathering agent is HALS770, the lubricant is PETS-AP, and the nucleating agent is silicon dioxide.
[0038] See also Figure 4 and Figure 5 In the present invention, a stretch-resistant foam diffusion plate includes a foam core layer 30, an upper protective layer and a lower protective layer 1, and a nanocellulose-based carbon dot composite film 2. The upper protective layer 1 is arranged on the upper surface of the foam core layer 30, the lower protective layer 1 is arranged on the lower surface of the foam core layer 30, and the nanocellulose-based carbon dot composite film 2 is arranged on four sides of the foam core layer 30 close to the upper protective layer 1. The foam core layer 30 is provided with red quantum dots 31, green quantum dots 32 and pores 33.
[0039] This example provides a stretch-resistant foam diffuser plate and a preparation method thereof, and a prepared foam quantum dot diffuser plate, and the specific steps are as follows: (1) Preparation of yellow carbon dots (Y-CDs) aqueous solution: 0.210 g o-phenylenediamine and 0.435 g L-tyrosine were weighed into a beaker, 15 mL of anhydrous ethanol was added to the beaker, and then 15 mL of secondary water was added. The solution was ultrasonicated for 20 min to make a clear solution. The solution was transferred to a 50 mL hydrothermal synthesis reactor and reacted at 160 °C for 8 h. The reactor was cooled to room temperature and the cooled solution was placed in a round-bottom flask for rotary evaporation. The solid after rotary evaporation was diluted with secondary water, filtered with a filter membrane (0.22 μm), and finally dialyzed with a dialysis bag with a molecular weight cutoff of 300 for 24 h. Finally, the concentration was diluted to obtain 1.0×10 -3 mol L -1 Yellow carbon dots aqueous solution.
[0040] (2) Preparation of nanocellulose (CNFs): Poplar wood powder (90 g, 60-80 mesh) was placed in a toluene ethanol solution (volume ratio of 2:1), stirred vigorously to disperse the poplar wood powder, and cooked at 75°C for 5 h to remove lignin. After the reaction was completed, it was repeatedly washed with distilled water until neutral to obtain holocellulose with most of the lignin removed. The obtained holocellulose was added to a KOH aqueous solution (5wt%), and was constantly cooked and stirred at 90°C for 2 h to remove hemicellulose. The product was filtered and adjusted to neutrality with distilled water. The product was placed in a NaClO2 solution (5wt%) and cooked at 75°C for 2 h to remove the second lignin. The second hemicellulose removal was cooked in a 5wt% NaOH aqueous solution for 2 h. The product was repeatedly washed with distilled water until neutral, and then the purified cellulose was nano-treated using an ultrasonic instrument. The output power was 1200 W and the reaction time was 30 min to prepare a suspension of CNFs. The product suspension was washed with water by vacuum filtration. It was then purified using a dialysis bag until the pH of the dialysis solution reached 7. Finally, it was stored at 4°C.
[0041] (3) Preparation of TEMPO-CNFs: 2 g of CNFs were added to 200 mL of an aqueous solution containing 0.032 g of 2,2,6,6-tetramethyl-1-piperidinyloxy (TEMPO) (98%) and 0.2 g of NaBr (≥99.0%), and stirred for 15 min; the TEMPO oxidation reaction was started by slowly adding 13 wt % NaClO solution (12 mL) and stirring slowly at room temperature. -1 The pH value was maintained at 10.5 by adding 0.5 mol L NaOH solution. -1The pH was adjusted to 7 with HCl solution; the product was washed thoroughly with water by vacuum filtration. The separated fractions were then placed in dialysis bags for purification until the pH of the dialysate water was 7.
[0042] (4) Preparation of nanocellulose-based carbon dot composite film: 20 mL of Y-CDs aqueous solution (1.0 mmol L -1 ), 1-ethyl-3 (dimethylaminopropyl) carbodiimide hydrochloride (EDC) (98.5%, 10.0 mg) and N-hydroxysuccinimide (NHS) (98%, 10.0 mg) were added to 20 mL of TEMPO-CNF suspension (2.0 wt%) to obtain a TEMPO-CNF / Y-CDs solution with 2 wt%. The resulting solution was dispersed by ultrasonic treatment for 1 h and magnetically stirred at 30 °C for 12 h. The TEMPO-CNF / Y-CDs suspension was placed in a vacuum oven at 60 °C for 1.5 h. Different volumes of the suspension were vacuum filtered in a 500 mL filter device. Thereafter, the prepared wet membrane was placed in two silicon wafers, and the filter membrane was dried at 60 °C at a pressure of 6.5-7 kPa to finally obtain a nanocellulose-based carbon dot composite film (TEMPO-CNF / Y-CDs), whose TEM image is shown in FIG. Figure 7 shown.
[0043] (5) Micro-nano bubble generation process of the foaming core layer: After the heated molten liquid of the foaming core layer and CO2 gas are mixed, they are pressed into a compressed gas tank through a valve to dissolve the gas in the molten liquid of the foaming core layer. The pressure is measured by a pressure gauge. After the pressure reaches 0.5 MPa, it is released through a valve. The dissolution time is 10 minutes and the release angle is 20°. The diameter of the obtained micro-nano bubbles is 5 μm~30 μm, and the cell cross-sectional density is 2×10 3 ~1.15×10 4 Pieces / cm 2 .
[0044] (6) Plate extrusion process: The raw materials of the upper and lower protective layers include, by mass percentage, 98.9% of optical resin matrix, 0.2% of light diffuser, 0.2% of antioxidant, 0.02% of weathering agent, 0.48% of lubricant, and 0.2% of anti-ultraviolet agent. After being fully stirred and mixed, they are divided into two equal parts for use; the raw materials of the foaming core layer include, by mass percentage, 98% of optical resin matrix, 0.2% of red quantum dots, 0.8% of green quantum dots, and 1% of nucleating agent, which are fully stirred and mixed for use; the prepared nanocellulose-based carbon dot composite film is cut into strips with a width of about 10 mm for use; the mixed upper and lower protective layer raw materials, foaming core layer raw materials, and nanocellulose-based carbon dot composite strips are added into four independent lower hoppers respectively, and co-mixed and extruded using a twin-screw extruder at an extrusion temperature of 210°C. After traction and cooling, a multi-layer co-extruded foamed quantum dot diffusion plate is obtained. The upper protective layer and the lower protective layer cover the upper and lower surfaces of the foam core layer, and the nanocellulose-based carbon dot composite film is arranged on the edge of the foam core layer near the upper protective layer. The thickness of the upper protective layer and the lower protective layer is 0.1 mm, the thickness of the foam core layer is 0.8 mm, and the thickness of the nanocellulose-based carbon dot composite film is 0.1 mm.
[0045] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that a nanocellulose film is used instead of a nanocellulose-based carbon dot composite film, and the rest is consistent with Example 1.
[0046] The test brightness and blue light intensity data of Example 1 were compared with those of Comparative Example 1, confirming that the edge brightness increased by 9.16% and the edge blue light intensity decreased by 9.05%.
[0047] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that the nanocellulose-based carbon dot composite film is not used, and the rest is consistent with Example 1.
[0048] The test brightness and blue light intensity data of Example 1 were compared with those of Comparative Example 2, confirming that the edge brightness increased by 8.14% and the edge blue light intensity decreased by 9.07%.
[0049] Performance testing The basic optical properties and mechanical properties of the stretch-resistant foamed diffusion plates prepared in Example 1 and Comparative Examples 1-2 were tested, and the specific test data are shown in Table 1 below.
[0050] Table 1 Light transmittance and haze are two important indicators for evaluating whether light diffusion materials are good or not. Good light diffusion materials should have both high light transmittance and high haze. Light transmittance refers to the ratio of the light flux passing through the material to the light flux irradiated on the material, and is an indicator for measuring the transparency of the material; haze refers to the ratio of the light flux scattered by the material to the light flux irradiated on the material, and is an indicator for measuring the strength of light scattering. Tensile strength refers to the maximum stress that a material can withstand during a tensile test from the beginning of the application of tension to the occurrence of fracture, and is an indicator for measuring the strength of a material's resistance to tensile stress.
[0051] It can be seen from Example 1, Comparative Examples 1-2 and Table 1 that adding a layer of nanocellulose-based carbon dot composite film around the edges of the foam core layer close to the upper protective layer can effectively increase the tensile resistance, increase the absorption of edge blue light to reduce the leakage of edge blue light, and improve the uniformity of light display.
[0052] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0053] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A stretch-resistant foam diffuser plate, Features: It includes a foaming core layer, an upper protective layer, a lower protective layer, and a nanocellulose-based carbon dot composite film; the upper protective layer is arranged on the upper surface of the foaming core layer, the lower protective layer is arranged on the lower surface of the foaming core layer, the nanocellulose-based carbon dot composite film is arranged on four sides of the foaming core layer close to the upper surface, and the arrangement width of the nanocellulose-based carbon dot composite film is smaller than the thickness of the foaming core layer, and the foaming core layer is not completely covered; The thickness ratio of the foamed core layer to the upper protective layer or the lower protective layer is 7:1-9:1; The upper protective layer and the lower protective layer are made of the same material, and the raw materials thereof include, by mass percentage: 98% to 99.8% of optical resin matrix, 0.2% to 1% of light diffusing agent, 0.2% to 1% of antioxidant, 0.02% to 1% of weathering agent, 0% to 0.5% of lubricant, and 0.2% to 1% of anti-ultraviolet agent; The raw materials of the foaming core layer include, by mass percentage: an optical resin matrix content of 98% to 99.8%, a red quantum dot content of 0.1 to 1%, a green quantum dot content of 0.1 to 1%, a nucleating agent content of 0.2 to 1%, and a particle size of the quantum dots of 2-12 nm. A plurality of pores are formed inside the foaming core layer.
2. The stretch-resistant foam diffuser plate according to claim 1, Features: The optical resin matrix is one or more of polycarbonate, polymethyl methacrylate, polystyrene, styrene-methyl methacrylate copolymer, and polypropylene; The light diffuser is one or more of titanium dioxide, silicon dioxide, calcium sulfate, barium sulfate, zinc oxide, organic silicon, and PS microspheres; The antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant, a metal alkylthiophosphoric acid antioxidant, a carbamic acid antioxidant, and an organic sulfur antioxidant; The weathering agent includes a hindered amine light stabilizer and / or an ultraviolet absorber; The lubricant is at least one of vinyl bisstearamide, stearate, polysiloxane, PP wax, PE wax, polysiloxane, and ethylene bis fatty acid amide; The anti-ultraviolet agent is benzotriazole, and hydroxybenzophenone and benzotriazole are used in combination.
3. The stretch-resistant foam diffuser plate according to claim 1, Features: The quantum dots are composed of quantum dots of CdS, CdSe, CdSeS, ZnS, ZnSe, ZnSeS, ZnCdSeS, InP, CuInS, GaN, GaP, GaAs, InN, InP, InGaP, GalnNP and perovskite; The nucleating agent is at least one of boron nitride, sodium carbonate, calcium carbonate, ultrafine talc, mica, montmorillonite, silicon dioxide, titanium dioxide, apatite, and magnesium aluminum hydrotalcite.
4. The stretch-resistant foam diffuser plate according to claim 1, Features: The yellow carbon dots in the nanocellulose-based carbon dot composite film are composed of yellow quantum dots of CdS, CdSe, CdSeS, ZnS, ZnSe, ZnSeS, ZnCdSeS, InP, CuInS, GaN, GaP, GaAs, InN, InP, InGaP, GalnNP and perovskite.
5. The stretch-resistant foam diffuser sheet according to claim 1, Features: The upper protective layer and the lower protective layer are provided with patterns on the side away from the foaming core layer to improve the refraction and reflection performance of light.
6. The stretch-resistant foam diffuser sheet according to claim 1, Features: The width of the nano-cellulose-based carbon dot composite film disposed on the four sides of the foaming core layer accounts for 1 / 8 of the thickness of the foaming core layer.
7. A method for preparing a stretch-resistant foaming diffusion plate according to claim 1, Features: The following steps are involved: S1, preparing two portions of protective layer raw materials with the same composition, one portion of foaming core layer raw material, and one portion of nanocellulose-based carbon dot composite film; S2, mixing the protective layer raw material and the foaming core layer raw material respectively and uniformly; S3, adding the mixed protective layer raw materials into a screw extruder to heat them to form a molten state; after heating the mixed foaming core layer raw materials to form a molten state, generating micro-nano bubbles by a dissolved gas release method, and then adding them to the screw extruder; cutting the nanocellulose-based carbon dot composite film and adding it to the screw extruder; S4. Finally, the upper protective layer, the foaming core layer and the lower protective layer are extruded through the die head of the screw extrusion equipment in the form of sheets, and the nano-cellulose-based carbon dot composite film is extruded in the form of strips. The upper protective layer is arranged on the upper surface of the foaming core layer, and the lower protective layer is arranged on the lower surface of the foaming core layer. The nano-cellulose-based carbon dot composite film is arranged on the four sides of the foaming core layer close to the upper surface, and the arrangement width of the nano-cellulose-based carbon dot composite film is smaller than the thickness of the foaming core layer, and does not completely cover the foaming core layer.
8. The method according to claim 7, Features: The screw extruder in step S3 includes three heating zones, the temperature of the first heating zone is 140-220°C, the temperature of the second heating zone is 160-240°C, and the temperature of the third heating zone is 180-260°C.
9. The method according to claim 7, Features: The gas used in the dissolved gas release method in step S3 is CO 2 Or nitrogen, or other inert gases.
10. The method according to claim 7, Features: The temperature control range of the die extrusion in step S4 is 170-260° C.; the screw extrusion equipment in step S4 is provided with a plurality of feed ports, which are suitable for putting a variety of different raw materials into the screw extrusion equipment.
Citation Information
Patent Citations
Preparation method of cellulose-based carbon dots and application in field of blue light resistance
CN113861970A
Foaming quantum dot light diffusion plate and display device
CN219285441U
Light diffusion plate containing nitrogen ball or carbon dioxide gas ball
WO2022222175A1
Cited By
Quantum dot foaming diffusion plate and preparation method thereof
CN121136295A