Process for preparing iron phosphate from lithium iron phosphate waste and iron phosphate
Through high-temperature impurity removal and roasting transformation, the lithium iron phosphate waste is treated, combined with acid leach and iron-to-phosphorus ratio, the recycling problem of lithium iron phosphate waste with high copper-aluminum impurity content is solved, and high-purity battery-grade iron phosphate preparation is achieved, which has expanded the Its industrial application.
Patent Information
- Application Number
- CN202410965984.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively treat lithium iron phosphate waste with high copper and aluminum impurities, resulting in the inability to achieve full component recycling, limiting the purity of iron phosphate and industrial applications.
By mixing the first leaching slag of lithium iron phosphate waste with acid, it is subjected to high temperature removal and calcination transformation, then acid leaching and iron-phosphorus ratio are adjusted, and finally a battery-grade iron phosphate is formed in the alkali reaction.
It has achieved effective removal of copper and aluminum impurities, improved the quality and purity of iron phosphate, and made it suitable for all lithium iron phosphate waste materials, expanding the scope of industrial application.
Smart Images

Figure CN118908163A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery waste recycling, and in particular to a process for preparing iron phosphate by utilizing lithium iron phosphate waste and the iron phosphate. Background Art
[0002] Due to its low price, environmental friendliness, safety and other advantages, the market demand for lithium iron phosphate is also increasing year by year. In the new energy vehicle market, the current installation volume of lithium iron phosphate batteries has exceeded that of ternary batteries. The increase in demand for lithium iron phosphate batteries will inevitably lead to an increase in the subsequent scrap volume. There are currently two paths for the recycling of waste batteries. The first is to use them in application scenarios with lower performance requirements, and the second is to directly recycle the valuable metals in the battery. The second path of hydrometallurgy has the advantages of high purity, high recovery rate, low temperature operation and low carbon emissions, so it is widely used.
[0003] At present, the recovery process is mainly divided into full-component leaching and selective leaching. Compared with the full-component dissolution process, the selective leaching method has the advantages of higher lithium leaching rate, separable lithium and iron, less reagent consumption, and short process flow, so it is widely used. Selective leaching either loses a large amount of phosphorus iron in order to improve the lithium leaching rate, increasing the cost of lithium salt impurity removal, or improves the selectivity effect by adjusting the amount of auxiliary materials added, but it will cause most of the copper and aluminum impurities in the waste to remain in the leaching residue. These impurities have a greater impact on the purity of iron phosphate after acid dissolution synthesis. Therefore, if you want to prepare qualified battery-grade iron phosphate, you can only select waste with low copper and aluminum impurity content for recycling. For lithium iron phosphate waste with high copper and aluminum impurity content (for example, the content of copper and aluminum is ≥1%), there is currently no effective method to achieve full component recovery.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a process for preparing iron phosphate using lithium iron phosphate waste and iron phosphate. The process provided in the embodiment of the present invention is suitable for treating various lithium iron phosphate wastes, especially lithium iron phosphate wastes with high copper and aluminum impurity contents, and recovering high-purity battery-grade iron phosphate from the above lithium iron phosphate wastes.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a process for preparing iron phosphate using lithium iron phosphate waste, comprising: mixing first leaching residue formed by leaching lithium iron phosphate waste with acid and performing high-temperature impurity removal under heating conditions to form second leaching residue;
[0008] Next, the second leached residue is subjected to roasting and transformation.
[0009] In an optional embodiment, the acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid; further preferably sulfuric acid;
[0010] Preferably, the amount of acid added is controlled by controlling the sulfur-to-iron ratio; wherein the sulfur-to-iron molar ratio is (0.1-1.5):1, preferably (0.1-0.9):1.
[0011] In an optional embodiment, the heating conditions include: a temperature of 70°C to 95°C; a time of 2 hours to 6 hours;
[0012] Preferably, the liquid-to-solid ratio of the mixed reaction liquid of the first leaching residue and the acid is 2ml-10ml:1g, and further optimized to 2ml-6ml:1g;
[0013] Preferably, the method comprises: returning the leaching solution formed by high-temperature impurity removal to the material from which the lithium iron phosphate waste is leached.
[0014] In an optional embodiment, the calcination temperature is 250°C-750°C; preferably 300°C-550°C; and the calcination time is 2 hours-4 hours.
[0015] In an optional embodiment, the contents of copper and aluminum in the lithium iron phosphate waste are both ≥ 1%;
[0016] Preferably, the method comprises: subjecting the roasting slag formed by roasting transformation to acid leaching, adjusting the iron-phosphorus ratio and alkaline reaction.
[0017] In an optional embodiment, the step of acid leaching includes: mixing the roasted slag with an acid to react;
[0018] Preferably, the acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid;
[0019] Preferably, the acid H + The concentration is 1-12 mol / L, preferably 2-5 mol / L;
[0020] Preferably, the molar ratio of H / Fe during acid leaching is 2-5:1;
[0021] Preferably, the acid leaching conditions include: a temperature of 30° C. to 80° C. and a time of 2 hours to 8 hours.
[0022] In an optional embodiment, the step of adjusting the iron-phosphorus ratio includes: mixing the leachate formed by acid leaching with phosphoric acid to adjust the iron-phosphorus molar ratio to 0.8-0.95:1.
[0023] In an optional embodiment, the alkaline reaction step comprises: mixing the ferrophosphorus liquid formed by adjusting the iron-phosphorus ratio with an alkali to a pH of 2-3, and reacting at 80-95°C.
[0024] In an optional embodiment, the step of leaching the lithium iron phosphate waste includes a first stage leaching and a second stage leaching;
[0025] Preferably, the step of one-stage leaching comprises: mixing the lithium iron phosphate waste with an acid to make a pulp, and adding an oxidant to react at 20° C.-75° C. to form a first leaching residue and a first leaching liquid;
[0026] Preferably, the acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid; further preferably sulfuric acid;
[0027] Preferably, the amount of the acid used is 0.9-2.0 times, preferably 1-1.4 times, the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction;
[0028] Preferably, the liquid-to-solid ratio of pulping is 2ml-7ml:1g;
[0029] Preferably, the reaction time is 2-6h;
[0030] Preferably, the oxidant is selected from any one of hydrogen peroxide, oxygen, ozone and sodium hypochlorite;
[0031] Preferably, the amount of the oxidant is 1-2 times, preferably 1-1.5 times, the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction;
[0032] Preferably, the second-stage leaching step includes: using lithium iron phosphate waste to adjust the pH of the first leaching solution and reacting with an oxidant to form a third leaching residue and a lithium iron phosphate leaching solution respectively;
[0033] Wherein, the pH is adjusted to 1-2, preferably 1.5-2;
[0034] Preferably, the temperature, amount and selection of the oxidant in the pH adjustment process are consistent with those in the first stage leaching;
[0035] Preferably, the iron-lithium leaching solution is subjected to impurity removal to form a lithium salt product;
[0036] Preferably, the method comprises: returning the third leaching residue to the first stage leaching.
[0037] In a second aspect, the present invention provides an iron phosphate, which is prepared by the process for preparing iron phosphate using lithium iron phosphate waste as described in any one of the aforementioned embodiments,
[0038] Preferably, the iron phosphate is battery grade iron phosphate.
[0039] The present invention has the following beneficial effects: the embodiment of the present invention can not only better remove copper and aluminum impurities by performing high-temperature impurity removal and roasting transformation on the first leached slag formed by lithium iron phosphate waste, but also improve the quality of the formed iron phosphate, which can be used as battery-grade iron phosphate. At the same time, the lithium iron phosphate waste treated by this method is not only suitable for raw materials with low copper and aluminum content, but also can be used to treat raw materials with high copper and aluminum content, that is, it can be applied to all lithium iron phosphate waste, solve the limitation of the existing raw material impurity content on the process, and expand industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0041] Figure 1 XRD pattern provided for test example 1;
[0042] Figure 2 This is the SEM image provided for test example 1. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0044] In a first aspect, the present invention provides a process for preparing iron phosphate using lithium iron phosphate waste, wherein the lithium iron phosphate waste can be any existing waste, that is, waste with high copper and aluminum impurity content or waste with low copper and aluminum impurity content can be subjected to the above process. For example, the copper and aluminum contents in the lithium iron phosphate waste are both ≥ 1%.
[0045] Specific operations include:
[0046] S1, one-stage leaching;
[0047] The lithium iron phosphate waste is mixed with acid to make pulp, and an oxidant is added to react at 20-75°C. After the reaction is completed, solid-liquid separation is performed to form a first leaching residue (hereinafter referred to as leaching residue B) and a first leaching solution (hereinafter referred to as leaching solution A). The first stage of leaching can selectively leach lithium and preliminarily achieve the separation of iron phosphate and lithium. At this time, most of the copper and aluminum are distributed in the leaching solution A, which also contains lithium and part of phosphorus and iron, while a small amount of copper and aluminum exists in the leaching residue B, and a large amount of the leaching residue B is iron phosphate.
[0048] Wherein, the liquid-solid ratio of pulping is 2ml-7ml:1g; for example, 2ml:1g, 3ml:1g, 4ml:1g, 5ml:1g, 6ml:1g and 7ml:1g, etc., any value between 2ml-7ml:1g. The reaction temperature is 20℃-75℃, for example, the temperature is 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃ and 75℃, etc., any value between 20-75℃. The reaction time is 2 hours-6 hours; for example, 2 hours, 3 hours, 4 hours, 5 hours and 6 hours, etc., any value between 2 hours-6 hours. During the reaction process, no excessive additional heating is required, and the reaction can be carried out using the self-reaction heat.
[0049] The oxidant includes one or more of hydrogen peroxide, oxygen, ozone, sodium hypochlorite, etc., and is further optimized to hydrogen peroxide in consideration of cost and safety; the amount of the oxidant is 1-2 times the total molar amount of lithium, copper and aluminum required for the theoretical reaction in the lithium iron phosphate waste, 1 times, 1.2 times, 1.5 times, 1.8 times and 2.0 times, etc., and any value between 1.0-2.0 times is further optimized to 1-1.5 times.
[0050] The acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid; further preferably sulfuric acid; using sulfuric acid can reduce production costs.
[0051] The amount of acid used is 0.9-2.0 times the total molar amount of lithium, copper and aluminum required for the theoretical reaction in the lithium iron phosphate waste, for example, 0.9 times, 1 times, 1.2 times, 1.5 times, 1.8 times and 2.0 times, etc., any value between 0.9-2.0 times, preferably 1-1.4 times; in the embodiment of the present invention, adding an excess of acid can increase the leaching rate of copper and aluminum and reduce the content of copper and aluminum in the leached slag B. However, as the amount of acid increases, the leaching rate of iron phosphate will also increase, that is, the content of phosphorus and iron in the leachate A will increase, which will then affect the recovery efficiency. Therefore, the leachate A is subjected to two-stage leaching.
[0052] S2, second stage leaching;
[0053] Add new lithium iron phosphate waste to the above leachate A to adjust the pH. Since excessive acid is used in the first stage of leaching, there is still more phosphorus and iron in the leachate A. Therefore, adjusting the pH can allow the iron and phosphorus in the leachate A to precipitate into the slag, reducing the loss of iron and phosphorus, but copper and aluminum will not be dissolved or will be dissolved in small amounts.
[0054] Specifically, the pH is 1-2, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and any value between 1 and 2, preferably 1.5 to 2. If the pH is too low, the purpose of precipitation of iron and phosphorus cannot be achieved, and if it is too high, lithium, aluminum and iron will be co-precipitated.
[0055] At the same time, an oxidant is added for mixed reaction to form a third leaching residue and an iron-lithium leaching solution respectively; the temperature, the amount and the selection of the oxidant in the above pH adjustment process are all consistent with those of the first stage leaching.
[0056] The third leaching residue is returned to the first leaching step for leaching, further improving the recovery efficiency of iron phosphate. The iron-lithium leaching solution is then subjected to impurity removal to form a lithium salt product. The method and operation of impurity removal of the iron-lithium leaching solution are all existing methods and operations, and will not be described in detail in the embodiments of the present invention.
[0057] S3, high temperature impurity removal;
[0058] The leached residue B is subjected to deep impurity removal. Specifically, the leached residue B is mixed with an acid and reacted at 70°C-95°C for 2 hours-6 hours to further remove copper and aluminum in the leached residue B. After the reaction, a leachate C and a leached residue D are obtained. The leachate C is returned to the first leaching step and can be used as an auxiliary acid.
[0059] The reaction temperature is any value between 70°C and 95°C, such as 70°C, 75°C, 80°C, 85°C, 90°C and 95°C. The reaction temperature is a high temperature reaction, and the high temperature promotes the precipitation and transformation of ferrophosphorus to achieve the purpose of rapid impurity removal.
[0060] Furthermore, the acid used in this step is consistent with the acid used in the first stage leaching, and the acid is controlled by controlling the addition of S / Fe (molar ratio), and the sulfur-iron ratio range is (0.1-1.5):1, for example, any value between (0.1-1.5):1 such as 0.1:1, 0.5:1, 1:1 and 1.5:1, further optimized to (0.1-0.9):1. The more sulfur-iron ratio is added, the higher the impurity leaching rate is. When a certain amount is added, the impurities in the slag are already very low and have little effect on impurity removal.
[0061] The liquid-to-solid ratio of the mixed reaction liquid of the first leaching residue and the acid is 2ml-10ml:1g, for example, 2ml:1g, 3ml:1g, 4ml:1g, 5ml:1g, 6ml:1g, 7ml:1g, 8ml:1g, 9ml:1g and 10ml:1g, etc., and is further optimized to 2ml-6ml:1g.
[0062] S4, roasting transformation;
[0063] The leached slag D obtained from S3 is subjected to high-temperature roasting to obtain roasted slag E. The high-temperature roasting process not only removes free water and crystal water, but also realizes the crystal transformation of iron phosphate, which facilitates subsequent acid leaching and the formation of battery-grade iron phosphate.
[0064] Specifically, the calcination temperature is 250°C-750°C; for example, any value between 250°C-750°C, such as 250°C, 350°C, 450°C, 550°C, 650°C and 750°C, preferably 300°C-550°C; the calcination time is 2 hours-4 hours. The above conditions can ensure the crystal transformation effect, which is beneficial to battery-grade iron phosphate.
[0065] S5, acid leaching;
[0066] The roasted slag E is mixed with an acid for reaction, and after the reaction is completed, a leachate F and a leachate slag G are separated, and the leachate slag G can be used for regenerating graphite after slag washing. The roasted slag E is acid-leached to obtain an iron phosphate solution, which is conducive to the subsequent formation of battery-grade iron phosphate.
[0067] The acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid. + The concentration is 1-12 mol / L, for example, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L and 12 mol / L, etc. Any value between 1-12 mol / L, preferably 2-5 mol / L. The added H / Fe molar ratio is 2-5:1. In the acid dissolution reaction process, too low acid concentration will reduce the reaction rate and affect the production efficiency. Too high acid concentration will make the solution iron concentration too high, resulting in solution instability or excessive acid addition to increase costs.
[0068] Further, the acid leaching conditions include: a temperature of 30°C-80°C and a time of 2 hours-8 hours. For example, the temperature is any value between 30°C-80°C, such as 30°C, 40°C, 50°C, 60°C, 70°C and 80°C. The above acid leaching conditions are conducive to the acid dissolution of the roasted slag E and the obtaining of the iron phosphate solution.
[0069] S6, adjust the iron-phosphorus ratio;
[0070] The above leachate F is mixed with phosphoric acid to adjust the iron-phosphorus ratio of the leachate F. The iron-phosphorus ratio of the ferrophosphorus solution obtained after acid leaching fluctuates to a certain extent, so phosphoric acid needs to be added to adjust the iron-phosphorus ratio to stabilize and control the various indicators of the obtained iron phosphate to be stable and qualified. Specifically, the molar ratio of Fe / P is adjusted to 0.8-0.95:1.
[0071] S7, base reaction;
[0072] The adjusted ferrophosphorus liquid is heated and added to the alkali for reaction. After the reaction is completed, the liquid and solid are separated and washed, dried and dehydrated to obtain battery-grade ferric phosphate. The reaction pH is 2-3 and the temperature is 80-95°C. This step is an existing operation and will not be described in detail in the embodiment of the present invention.
[0073] Through the above process of the embodiment of the present invention, a kind of iron phosphate can be obtained, and the iron phosphate is battery-grade iron phosphate.
[0074] It should be noted that the normal temperature described in the embodiments of the present invention is about 25°C.
[0075] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0076] Example 1
[0077] The embodiment of the present invention provides a process for preparing iron phosphate using lithium iron phosphate waste, wherein the composition of the lithium iron phosphate waste is as shown in the following table:
[0078]
[0079] The method comprises: (1) a first stage leaching: preparing 100 g of lithium iron phosphate waste and mixing it with 300 ml of dilute sulfuric acid (liquid-to-solid ratio of 3:1, the amount of dilute sulfuric acid used is 1.2 times the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction), reacting at room temperature (about 25° C.), continuously adding hydrogen peroxide in an amount of 1.2 times the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction during the reaction, reacting for 4 hours, and filtering after the reaction to obtain a leachate A and a leach residue B.
[0080] (2) Second stage leaching: A certain amount of lithium iron phosphate waste is added to the impurity-containing leachate A obtained in step (1) to adjust the pH to 1.2. After the reaction is completed, liquid-solid separation is performed to obtain a low-iron lithium liquid. The lithium liquid is purified to obtain a lithium salt product. The leached residue is returned to the first stage leaching to continue to participate in the reaction.
[0081] (3) High-temperature impurity removal: the leached residue B obtained in step (1) is mixed with dilute sulfuric acid and hydrogen peroxide, wherein the liquid-to-solid ratio is 2.5:1, and the molar ratio of added sulfur and iron is 0.5:1, and the reaction is carried out at 80°C. After the reaction is completed, the leached solution C and the leached residue D are obtained by suction filtration, and the leached solution C is returned to the first leaching stage.
[0082] (4) Calcination transformation: The leached slag D obtained in step (3) is calcined in a kiln at 450° C. for 3 h to obtain calcined slag E.
[0083] (5) Acid leaching: The calcined slag E obtained in step (4) was added to H2O at a molar ratio of H2O / Fe of 4:1. + The reaction is carried out in a sulfuric acid solution with a concentration of 2 at a temperature of 50°C for 4 hours. After the reaction is completed, the leaching liquid F and the leaching residue G are separated. The leaching residue G can be used for regenerating graphite after slag washing.
[0084] (6) Adjusting Fe / P: Phosphoric acid is added to the leaching solution F obtained in step (5) to adjust the iron-phosphorus molar ratio of the solution to 0.9:1.
[0085] (7) Synthesis: The ferrophosphorus solution adjusted with the value obtained in step (6) is heated and added with alkali for reaction. After the reaction is completed, the liquid and solid are separated and washed, dried and dehydrated to obtain battery-grade ferric phosphate. The reaction temperature is 90°C and the pH is 2.
[0086] Example 2
[0087] The embodiment of the present invention provides a process for preparing iron phosphate using lithium iron phosphate waste, wherein the lithium iron phosphate waste is the lithium iron phosphate waste of embodiment 1. The process comprises:
[0088] (1) One-stage leaching: 100 g of lithium iron phosphate powder was mixed with 500 ml of dilute sulfuric acid (liquid-to-solid ratio 5:1, the amount of dilute sulfuric acid was 1.3 times the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction), and reacted at room temperature. During the reaction, 1.2 times the amount of hydrogen peroxide was continuously added. The reaction was continued for 4 hours. After the reaction was completed, leaching solution A and leaching residue B were obtained by filtration.
[0089] (2) Second stage leaching: a certain amount of lithium iron phosphate waste is added to the impurity-containing leachate A obtained in step (1) to adjust the pH to 1.2. After the reaction is completed, liquid-solid separation is performed to obtain a low-iron lithium liquid. After the impurities are removed from the lithium liquid, a lithium salt product is obtained. The leached residue is returned to the first stage leaching.
[0090] (3) High-temperature impurity removal: The leached residue B obtained in step (1) is subjected to deep impurity removal. Specifically, the leached residue B is mixed with dilute sulfuric acid and hydrogen peroxide, wherein the liquid-to-solid ratio is 3:1, and the molar ratio of added sulfur and iron is 0.8:1. The mixture is reacted at 80°C. After the reaction is completed, a leaching solution C and a leaching residue D are obtained by suction filtration, and the leaching solution C is returned to the first leaching step.
[0091] (4) Calcination transformation: The leached slag D obtained in step (3) is calcined in a kiln at 500° C. for 3 h to obtain calcined slag E.
[0092] (5) Acid leaching: The calcined slag E obtained in step (4) was added to H at a molar ratio of H / Fe of 2.5:1. + The reaction is carried out in a sulfuric acid solution with a concentration of 3 at a temperature of 50°C for 4 hours. After the reaction is completed, the leaching liquid F and the leaching residue G are separated. The leaching residue G can be used for regenerating graphite after slag washing.
[0093] (6) Adjusting Fe / P: Phosphoric acid is added to the leaching solution F obtained in step (5) to adjust the iron-phosphorus molar ratio of the solution to 0.9:1.
[0094] (7) Synthesis: The ferrophosphorus solution adjusted in step (6) is heated and added with alkali for reaction. After the reaction is completed, the liquid and solid are separated and washed, dried and dehydrated to obtain battery-grade ferric phosphate. The reaction temperature is 85°C and the pH is 2.5.
[0095] Example 3
[0096] In this embodiment, a process for preparing iron phosphate using lithium iron phosphate waste is provided, wherein the composition of the lithium iron phosphate waste is as shown in the following table:
[0097]
[0098] The specific steps include:
[0099] (1) One-stage leaching: 100 g of lithium iron phosphate powder was mixed with 300 ml of dilute sulfuric acid (liquid-to-solid ratio 3:1, the amount of dilute sulfuric acid was 1.2 times the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction), and reacted at room temperature. During the reaction, 1.2 times the amount of hydrogen peroxide was continuously added. The reaction was continued for 4 hours. After the reaction was completed, leaching solution A and leaching residue B were obtained by filtration.
[0100] (2) Second stage leaching: A certain amount of lithium iron phosphate waste is added to the impurity-containing leachate A obtained in step (1) to adjust the pH to 1.2. After the reaction is completed, liquid-solid separation is performed to obtain a low-iron lithium liquid. The lithium liquid is purified to obtain a lithium salt product. The leached residue is returned to the first stage leaching to continue to participate in the reaction.
[0101] (3) High-temperature impurity removal: The leached residue B obtained in step (1) is subjected to deep impurity removal. Specifically, the leached residue B is mixed with dilute sulfuric acid and hydrogen peroxide, wherein the liquid-to-solid ratio is 2.5:1, and the molar ratio of added sulfur and iron is 0.65:1. The mixture is reacted at 90°C. After the reaction is completed, the leached solution C and the leached residue D are obtained by suction filtration, and the leached solution C is returned to the first leaching step.
[0102] (4) Calcination transformation: The leached slag D obtained in step (3) is calcined in a kiln at 400° C. for 3 h to obtain calcined slag E.
[0103] (5) Acid leaching: The calcined slag E obtained in step (4) was added to a dilute acid H2O at a molar ratio of H2O / Fe of 3:1. + The reaction was carried out in a sulfuric acid solution with a concentration of 3.2 at a temperature of 50°C for 4 hours. After the reaction was completed, the leaching liquid F and the leaching residue G were separated. The leaching residue G can be used for regenerating graphite after slag washing.
[0104] (6) Adjusting Fe / P: Phosphoric acid is added to the leaching solution F obtained in step (5) to adjust the iron-phosphorus molar ratio of the solution to 0.9:1.
[0105] (7) Synthesis: The ferrophosphorus solution adjusted in step (6) is heated and added to a base for reaction. After the reaction is completed, the liquid and solid are separated and washed, dried and dehydrated to obtain battery-grade ferric phosphate. The reaction temperature is 8.5 and the pH is 2.
[0106] Comparative Example 1
[0107] This comparative example provides a process for preparing iron phosphate using lithium iron phosphate waste, wherein the lithium iron phosphate waste is the lithium iron phosphate waste of Example 1. It includes:
[0108] (1) Leaching: Prepare 100 g of lithium iron phosphate powder and mix it with 500 ml of dilute sulfuric acid (liquid-to-solid ratio of 5:1, the amount of dilute sulfuric acid is 1.2 times the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction), react at room temperature, and continuously add 1.3 times hydrogen peroxide during the reaction process. The reaction is carried out for 4 hours. After the reaction is completed, the leachate and leach residue are obtained by suction filtration.
[0109] (2) Acid leaching: The leached residue obtained in step (1) was added to a dilute acid H2O2 solution at a molar ratio of H2O2 / Fe of 3:1. + The reaction was carried out in a sulfuric acid solution with a concentration of 3 at a temperature of 50°C for 4 hours. After the reaction was completed, the leaching liquid and the leaching residue were separated by suction filtration.
[0110] (3) Adjusting Fe / P: Phosphoric acid is added to the leaching solution obtained in step (2) to adjust the iron-phosphorus molar ratio of the solution to 0.9:1.
[0111] (4) Synthesis: The adjusted ferrophosphorus solution is heated and added with alkali for reaction. After the reaction is completed, the liquid and solid are separated and washed, dried and dehydrated to obtain ferric phosphate.
[0112] Comparative Example 2
[0113] This comparative example provides a process for preparing iron phosphate using lithium iron phosphate waste, wherein the lithium iron phosphate waste is the lithium iron phosphate waste of Example 1. It includes:
[0114] (1) One-stage leaching: 100 g of lithium iron phosphate powder was mixed with 300 ml of dilute sulfuric acid (liquid-to-solid ratio 3:1, the amount of dilute sulfuric acid was 1.2 times the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction), and reacted at room temperature. During the reaction, 1.2 times of hydrogen peroxide was continuously added. The reaction was continued for 4 hours. After the reaction was completed, the leachate and leach residue were obtained by filtration.
[0115] (2) Second stage leaching: A certain amount of lithium iron phosphate waste is added to the impurity-containing leachate obtained in step (1) to adjust the pH to 1.2. After the reaction is completed, liquid-solid separation is performed to obtain a low-iron lithium liquid. The lithium liquid is decontaminated to obtain a lithium salt product. The leached residue is returned to the first stage leaching to continue to participate in the reaction.
[0116] (3) Acid leaching: The leached residue obtained in step (1) was added to a dilute acid H2O2 solution at a molar ratio of H2O2 / Fe of 3:1. + The reaction is carried out in a sulfuric acid solution with a concentration of 3.2 at a temperature of 50°C for 4 hours. After the reaction is completed, the leaching liquid and the leaching residue are separated. The leaching residue can be used for regenerating graphite after slag washing.
[0117] (4) Adjusting Fe / P: Phosphoric acid is added to the leaching solution obtained in step (3) to adjust the iron-phosphorus molar ratio of the solution to 0.9:1.
[0118] (5) Synthesis: The ferrophosphorus solution adjusted to the desired temperature in step (4) is heated and added with alkali for reaction. After the reaction is completed, the liquid and solid are separated and washed, dried and dehydrated to obtain ferric phosphate.
[0119] Test Example 1
[0120] X-ray diffraction and electron microscope scanning were performed on the leached slag B prepared in Example 1, the leached slag D formed by high temperature impurity removal, and the roasted slag E. The results are shown in Figure 1 and Figure 2 .
[0121] in, Figure 1 The XRD pattern represented by Figure 1 a in the figure shows the XRD pattern of leached residue B; Figure 1 b shows the XRD pattern of leached residue D; Figure 1 c in the figure shows the XRD pattern of leached residue E. Figure 1It can be seen that the crystal form of leached slag B is mainly isophosphite-type iron phosphate and graphite. After high-temperature impurity removal, the crystal form of the obtained leached slag D is transformed into dihydrate iron phosphate and graphite. The crystal form of roasted slag E after decortication is anhydrous iron phosphate and graphite.
[0122] Figure 2 represents the SEM image, where Figure 2 a and b represent SEM images of leached residue B; Figure 2 c and d show the SEM images of leached residue D; Figure 2 Figures e and f show SEM images of leached residue E. Figure 2 It can be seen that in the leached slag b generated after leaching of lithium iron phosphate waste, the isophosphite-type iron phosphate is evenly wrapped around the graphite; after high-temperature impurity removal, the shape of the particles around the graphite has obviously changed, from the previous interconnected granular state to the lamellar state, and the overall particles are smaller and more evenly distributed than before; the particles of the roasted slag E are more broken after dehydration, and some of the lamellar layers are obviously broken from the enlarged picture.
[0123] Test Example 2
[0124] The iron phosphate and lithium carbonate prepared in the above Examples 1 to 3 and Comparative Examples 1 to 2 were tested for physical and chemical indicators, and the results are shown in Tables 1 and 2 below.
[0125] Table 1 Test results of physical and chemical indicators of anhydrous ferric phosphate
[0126]
[0127]
[0128] Table 2 Physical and chemical index test results of lithium carbonate
[0129]
[0130]
[0131] From the data comparison in Table 1, it can be seen that the anhydrous iron phosphate prepared in the embodiment of the present invention has a higher purity than the anhydrous iron phosphate prepared in the comparative example, especially the copper and aluminum content is significantly reduced. From the data comparison in Table 2, it can be seen that the lithium carbonate prepared in the embodiment of the present invention and the lithium carbonate prepared in the comparative example are not much different, and both meet the lithium carbonate standard. It can be seen that the process provided in the embodiment of the present invention can effectively improve the performance of iron phosphate.
[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing iron phosphate using lithium iron phosphate waste, characterized in that: include: The first leaching residue formed by leaching lithium iron phosphate waste is mixed with acid and subjected to high temperature impurity removal under heating conditions to form a second leaching residue; Next, the second leached residue is subjected to roasting and transformation.
2. The process for preparing iron phosphate using lithium iron phosphate waste according to claim 1, characterized in that: The acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid; further preferably sulfuric acid; Preferably, the amount of acid added is controlled by controlling the sulfur-iron ratio; wherein the molar ratio of sulfur-iron is (0.1-1.5):1, preferably (0.1-0.9):
1.
3. The process for preparing iron phosphate using lithium iron phosphate waste according to claim 1, characterized in that: The heating conditions include: temperature of 70°C-95°C; time of 2 hours-6 hours; Preferably, the liquid-to-solid ratio of the mixed reaction liquid of the first leaching residue and the acid is 2ml-10ml:1g, and further optimized to 2ml-6ml:1g; Preferably, the method comprises: returning the leaching solution formed by high-temperature impurity removal to the material from which the lithium iron phosphate waste is leached.
4. The process for preparing iron phosphate using lithium iron phosphate waste according to claim 1, characterized in that: The calcination temperature is 250°C-750°C, preferably 300°C-550°C, and the calcination time is 2 hours-4 hours.
5. The process for preparing iron phosphate using lithium iron phosphate waste according to any one of claims 1 to 4, characterized in that: The contents of copper and aluminum in the lithium iron phosphate waste are both ≥ 1%; Preferably, the method comprises: subjecting the roasting slag formed by roasting transformation to acid leaching, adjusting the iron-phosphorus ratio and alkaline reaction.
6. The process for preparing iron phosphate using lithium iron phosphate waste according to claim 5, characterized in that: The acid leaching step includes: mixing the roasted slag with an acid to react; Preferably, the acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid; Preferably, the acid H + The concentration is 1-12 mol / L, preferably 2-5 mol / L; Preferably, the molar ratio of H / Fe during acid leaching is 2-5:1; Preferably, the acid leaching conditions include: a temperature of 30° C. to 80° C. and a time of 2 hours to 8 hours.
7. The process for preparing iron phosphate using lithium iron phosphate waste according to claim 5, characterized in that: The step of adjusting the iron-phosphorus ratio comprises: mixing the leaching solution formed by acid leaching with phosphoric acid to adjust the iron-phosphorus molar ratio to 0.8-0.95:
1.
8. The process for preparing iron phosphate using lithium iron phosphate waste according to claim 5, characterized in that: The step of the alkali reaction comprises: mixing the ferrophosphorus liquid formed by adjusting the iron-phosphorus ratio with alkali until the pH value is 2-3, and reacting at 80-95°C.
9. The process for preparing iron phosphate using lithium iron phosphate waste according to any one of claims 1 to 4, characterized in that: The steps of leaching the lithium iron phosphate waste material include a first-stage leaching and a second-stage leaching; Preferably, the step of one-stage leaching comprises: mixing the lithium iron phosphate waste with an acid to make a pulp, and adding an oxidant to react at 20-75° C. to form a first leaching residue and a first leaching solution; Preferably, the acid is a dilute acid, preferably an inorganic acid, more preferably any one or a combination of at least two of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid; further preferably sulfuric acid; Preferably, the amount of the acid used is 0.9-2.0 times, preferably 1-1.4 times, the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction; Preferably, the liquid-to-solid ratio of pulping is 2ml-7ml:1g; Preferably, the reaction time is 2-6h; Preferably, the oxidant is selected from any one of hydrogen peroxide, oxygen, ozone and sodium hypochlorite; Preferably, the amount of the oxidant is 1-2 times, preferably 1-1.5 times, the total molar amount of lithium, copper and aluminum in the lithium iron phosphate waste required for the theoretical reaction; Preferably, the second-stage leaching step includes: using lithium iron phosphate waste to adjust the pH of the first leaching solution and reacting with an oxidant to form a third leaching residue and a lithium iron phosphate leaching solution respectively; Wherein, the pH is adjusted to 1-2, preferably 1.5-2; Preferably, the temperature, amount and selection of the oxidant in the pH adjustment process are consistent with those in the first stage leaching; Preferably, the iron-lithium leaching solution is subjected to impurity removal to form a lithium salt product; Preferably, the method comprises: returning the third leaching residue to the first stage leaching.
10. An iron phosphate, characterized in that: It is prepared by the process for preparing iron phosphate using lithium iron phosphate waste as described in any one of claims 1 to 9, Preferably, the iron phosphate is battery grade iron phosphate.
Citation Information
Patent Citations
Integral recycling method of lithium iron phosphate positive electrode material
CN108075202A
Method for recovering battery-grade iron phosphate from waste iron phosphate slag
CN112047319A