Method for recovering positive electrode of waste lithium iron phosphate battery
By employing roasting, leaching, and crystallization processes, combined with pH adjustment using hydrogen peroxide, the problem of non-compliant iron-phosphorus ratios in lithium iron phosphate recovery in existing technologies has been solved. This achieves efficient and low-cost iron phosphate recovery, meeting the application requirements of secondary batteries.
Patent Information
- Application Number
- CN202411195173.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
AI Technical Summary
Existing recycling methods are insufficient to obtain iron phosphate with the required iron-phosphorus molar ratio, which limits its application in the field of secondary batteries. Furthermore, high-temperature solid-state methods and hydrometallurgical methods suffer from high energy consumption and high costs.
By roasting waste lithium iron phosphate with (NH4)2SO4, leaching treatment, mixing with phosphoric acid solution, and crystallizing with hydrogen peroxide, adjusting the pH value within the range of 0.7 to 2.5 to control the crystallization process, and finally calcining, iron phosphate with an iron-to-phosphorus molar ratio of (0.96 to 1):1 is obtained.
It achieves efficient removal of impurities and organic matter, reduces energy consumption and acid usage, lowers recycling costs, obtains iron phosphate products that meet the requirements of secondary batteries, and increases product added value.
Smart Images

Figure CN118908167A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of waste battery recycling, and in particular to a method for recycling positive electrodes of waste lithium iron phosphate batteries. Background Art
[0002] With the rapid development of the new energy vehicle industry, a large number of retired lithium iron phosphate batteries have appeared, and the number is showing a rapid growth trend. The harmful parts of retired lithium iron phosphate batteries will not only cause serious pollution when entering the environment, but also pose safety hazards such as fire and explosion. Therefore, the recycling of waste lithium iron phosphate batteries is very urgent. It not only solves environmental problems and eliminates safety hazards, but also brings certain economic effects.
[0003] At present, the recycling methods include high-temperature solid-phase method and hydrometallurgical method. The high-temperature solid-phase method mainly realizes the repair of composition and structure by adding lithium salts, carbon sources, etc. Hydrometallurgy mainly uses acid solution to leach lithium from waste lithium iron phosphate positive electrode powder to liquid phase, and then obtains lithium carbonate, lithium phosphate or lithium chloride products through methods such as impurity removal, precipitation, evaporation, etc., and the iron phosphate after lithium extraction is discarded as residue. For example, through the principle of coordinated control of sulfate melt infiltration-oxidation, elements such as lithium, iron, and phosphorus are recovered, but the iron-phosphorus molar ratio of the final product is not within the range of (0.96 to 1): 1, which cannot meet the requirements of iron phosphate in the field of secondary batteries, thereby limiting the scope of application of the recycled products. Summary of the invention
[0004] The purpose of this application is to provide a method for recycling the positive electrode of waste lithium iron phosphate batteries, and the recycled product iron phosphate meets the requirements of iron phosphate in the field of secondary batteries. The specific technical solution is as follows:
[0005] The first aspect of the present application provides a method for recycling a positive electrode of a waste lithium iron phosphate battery, comprising the following steps:
[0006] (1) dismantling waste lithium iron phosphate batteries to obtain waste lithium iron phosphate, mixing the waste lithium iron phosphate with (NH4)2SO4 and then calcining to obtain a calcined product;
[0007] (2) mixing the roasted product with water for leaching, and then filtering to obtain a leachate and a solid intermediate product;
[0008] (3) mixing the intermediate product with a phosphoric acid solution, dissolving the mixture, and filtering the mixture to obtain a first filtrate;
[0009] (4) Mixing the first filtrate with water to obtain a mixed solution, then performing a crystallization treatment, adding hydrogen peroxide during the crystallization treatment, and then filtering to obtain a filter residue and a second filtrate, and calcining the filter residue to obtain a product ferric phosphate; wherein the pH of the mixed solution is 0.7 to 2.5.
[0010] In some embodiments of the present application, in step (3), the concentration C of the phosphoric acid solution is 1 mol / L to 6 mol / L, and the mass ratio Y of the intermediate product to the phosphoric acid solution is 1:(5 to 20).
[0011] In some embodiments of the present application, in step (3), the dissolution time t2 is 3 h to 12 h, and the dissolution temperature T2 is 15 to 35°C.
[0012] In some embodiments of the present application, in step (4), the addition rate V of hydrogen peroxide is 0.017 mL / min to 0.03 mL / min; preferably, the total amount of hydrogen peroxide added is: 1 ml to 2 ml of hydrogen peroxide is added for every 3 g of waste lithium iron phosphate treated; preferably, the hydrogen peroxide is added dropwise.
[0013] In some embodiments of the present application, the pH of the mixed solution is 0.9 to 1.2.
[0014] In some embodiments of the present application, in step (4), the temperature T3 of the crystallization treatment is 70°C to 110°C, and the time t3 is 3h to 6h.
[0015] In some embodiments of the present application, in step (4), the calcination temperature T4 is 400° C. to 700° C., and the calcination time t4 is 1.5 h to 6 h.
[0016] In some embodiments of the present application, the recovery method further includes the following steps: (5) heating the second filtrate to make its volume the same as that of the first filtrate, and then adding it to the first filtrate to continue dissolving the intermediate product.
[0017] In some embodiments of the present application, in step (1), the mass ratio X of the waste lithium iron phosphate to (NH4)2SO4 is 1:(0.6 to 1); the roasting temperature T1 is 250°C to 400°C; and oxygen-containing gas is continuously introduced during the roasting, and the oxygen-containing gas includes oxygen or air.
[0018] In some embodiments of the present application, in step (2), the pH of the slurry obtained by mixing the roasted product with water is ≤3; the leaching solution contains Li + and impurity elements, wherein the impurity elements include Al and / or Ca; and the intermediate product contains phosphorus and iron.
[0019] In some embodiments of the present application, the iron content of the product ferric phosphate is 35.7wt% to 36.7wt%, and the phosphorus content is 20.0wt% to 21.1wt%.
[0020] Beneficial effects of this application:
[0021] The present application provides a method for recovering positive electrodes of waste lithium iron phosphate batteries, comprising the following steps: (1) disassembling waste lithium iron phosphate batteries to obtain waste lithium iron phosphate, mixing the waste lithium iron phosphate with (NH4)2SO4 and then roasting to obtain a roasted product; (2) mixing the roasted product with water for leaching treatment, and then filtering to obtain a leachate and a solid intermediate product; (3) mixing the intermediate product with a phosphoric acid solution, dissolving the mixture, and filtering to obtain a first filtrate; (4) mixing the first filtrate with water to obtain a mixed solution, and then performing a crystallization treatment, adding hydrogen peroxide during the crystallization treatment, and then filtering to obtain a filter residue and a second filtrate, and calcining the filter residue to obtain a product iron phosphate; wherein the pH of the mixed solution is 0.7 to 2.5. The recovery method provided in the present application can basically remove impurity elements (such as Ca, Al, etc.), organic matter and carbon at the same time after roasting and leaching treatment, thereby reducing the energy consumption of removing organic matter and carbon at high temperature alone; in the crystallization process, water is first used to adjust the pH of the first filtrate, thereby avoiding the use of alkali, being more environmentally friendly and lowering the cost. At the same time, the product iron phosphate with the required iron-phosphorus molar ratio is obtained by crystallization, which not only meets the national standard requirements, but also reduces the use of acid compared to the traditional method of using a large amount of acid, further reducing the recovery cost and increasing the product added value of waste lithium iron phosphate.
[0022] In the present application, phosphoric acid is used to dissolve the intermediate product, and only one subsequent crystallization treatment is used to obtain a product iron phosphate with an iron-phosphorus ratio that meets the requirements. This is because phosphoric acid has the function of replenishing phosphorus, which ensures that the content of P element in the crystallization process system is appropriate and simplifies the process.
[0023] In the present application, the roasting process only uses ammonium sulfate with reducing properties to react with waste lithium iron phosphate to convert Fe 2+ Transformed into Fe 3+ The intermediate product is ferric phosphate slag (the iron-phosphorus ratio at this time does not meet the requirements), and the acid dissolution crystallization is continued. The oxidant hydrogen peroxide needs to be added during the crystallization process to avoid Fe 3+ Oxidized to Fe 2+ , which is conducive to obtaining products with iron-phosphorus ratio meeting the requirements.
[0024] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.
[0026] Figure 1 It is the experimental flow chart of Example 1;
[0027] Figure 2 It is a comparison diagram of the mixed solutions in Example 1 and Comparative Example 3. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0029] The present application provides a method for recycling the positive electrode of a waste lithium iron phosphate battery, comprising the following steps:
[0030] (1) dismantling waste lithium iron phosphate batteries to obtain waste lithium iron phosphate, mixing the waste lithium iron phosphate with (NH4)2SO4 and then calcining to obtain a calcined product;
[0031] (2) mixing the roasted product with water for leaching, and then filtering to obtain a leachate and a solid intermediate product;
[0032] (3) mixing the intermediate product with a phosphoric acid solution, dissolving the mixture, and filtering the mixture to obtain a first filtrate;
[0033] (4) Mixing the first filtrate with water to obtain a mixed solution, then performing a crystallization treatment, adding hydrogen peroxide during the crystallization treatment, filtering to obtain a filter residue and a second filtrate, and calcining the filter residue to obtain the product ferric phosphate; wherein the pH of the mixed solution is 0.7 to 2.5. For example, the pH of the mixed solution can be 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4 or 2.5, or between any two of the above numbers.
[0034] The present application does not particularly limit the method of obtaining waste lithium iron phosphate. For example, the waste lithium iron phosphate battery is disassembled to obtain the positive electrode, and the positive electrode current collector and the positive electrode material layer of the disassembled positive electrode are separated. The obtained positive electrode material layer is also the waste lithium iron phosphate, and the waste lithium iron phosphate may include but is not limited to lithium iron phosphate, organic matter, carbon, etc. The present application does not limit the above-mentioned organic matter and carbon. For example, the organic matter can be a binder in the positive electrode material layer, and the carbon can be a conductive agent in the positive electrode material layer.
[0035] The impurity removal method provided in the present application, through roasting, the impurity elements in the waste lithium iron phosphate react with (NH4)2SO4 to generate sulfates of the impurity elements (CaSO4 and Al2(SO4)3), the iron elements and lithium elements in the waste lithium iron phosphate react with (NH4)2SO4 to generate iron phosphate and lithium sulfate, and the organic matter and carbon in the waste lithium iron phosphate can also be removed. Subsequently, the roasted product after roasting is leached with water. Since the sulfates of the impurity elements are soluble in water or slightly soluble in water, and iron phosphate is insoluble in water, the iron phosphate can be separated from the impurity elements by filtering after the leaching treatment; at the same time, lithium sulfate is soluble in water, and the leaching of lithium elements is also achieved by the leaching treatment. Then, the intermediate product is mixed with a phosphoric acid solution, which can not only fully dissolve the intermediate product, but also facilitate the subsequent recrystallization process, and more importantly, phosphoric acid has the effect of supplementing phosphorus, and a product with an iron-phosphorus ratio that meets the requirements can be obtained by one-step recrystallization, and there is no need to supplement phosphorus separately in the future, which simplifies the process steps. Finally, the pH of the first filtrate obtained by dissolving and filtering is adjusted by water, and then crystallized. In the process of crystallization, hydrogen peroxide is added to reduce the Fe 3+ Converted to Fe 2+ The probability of reducing Fe 2+ The phosphate compound is produced, so that the compound obtained by crystallization is iron phosphate, and the impurity elements in the iron phosphate are further reduced; after the crystallization is completed, the filter is filtered, and the obtained filter residue is calcined to obtain the product iron phosphate, and its iron-phosphorus molar ratio is in the range of (0.96 to 1):1, which meets the requirements of iron phosphate in the field of secondary batteries.
[0036] In step (4), if the pH of the mixed solution is too low, for example, lower than 0.7, iron phosphate cannot be precipitated during the crystallization process or the amount of precipitation is too low; if the pH is too high, for example, higher than 2.5, white precipitate Fe(OH)3 is easily formed during the crystallization process, and a product with an iron-phosphorus ratio that meets the requirements cannot be obtained. Therefore, by regulating the pH of the mixed solution within the above range, it is beneficial to obtain a product with an iron phosphate ratio that meets the requirements.
[0037] Furthermore, in the present process, the pH of the mixed solution is adjusted to 0.9 to 1.2, which can not only obtain an iron phosphate product with an iron-phosphorus ratio that meets the requirements, but also increase the recovery rate of iron phosphate to more than 90%. In addition, the amount of water used to adjust the pH during the recovery process is moderate, and a large amount of water will not be used, thereby reducing the energy consumption in the subsequent evaporation and crystallization process.
[0038] Therefore, the impurity removal method provided in the present application can basically remove impurity elements, organic matter and carbon at the same time after roasting and leaching treatment, reducing the energy consumption of removing organic matter and carbon separately; in the crystallization process, only water is used to adjust the pH, avoiding the use of alkali, which is more environmentally friendly and lower in cost. At the same time, the product iron phosphate with the required iron-phosphorus molar ratio is obtained by crystallization. Compared with the traditional method of using a large amount of acid, the use of acid is also reduced, further reducing the recovery cost, and increasing the product added value of waste lithium iron phosphate.
[0039] In some embodiments of the present application, in step (3), the concentration C of phosphoric acid solution is 1mol / L to 6mol / L, and the mass ratio Y of the intermediate product to the phosphoric acid solution is 1:(5 to 20). For example, the concentration C of phosphoric acid solution can be 1mol / L, 1.5mol / L, 2mol / L, 2.5mol / L, 3mol / L, 3.5mol / L, 4mol / L, 4.5mol / L, 5mol / L, 5.5mol / L or 6mol / L, or between any two of the above numbers. For example, the mass ratio Y can be 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20, or between any two of the above numbers. By regulating the concentration C and the mass ratio Y within the above range, it is beneficial for the intermediate product to be fully dissolved, so as to obtain the product iron phosphate with the required iron-phosphorus molar ratio in the subsequent crystallization process.
[0040] In some embodiments of the present application, in step (3), the time t2 of dissolution is 3h to 12h, and the temperature T2 of dissolution is 15 to 35°C. For example, the time t2 of dissolution can be 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h, or between any two of the above numbers. For example, the temperature T2 of dissolution can be 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C or 35°C, or between any two of the above numbers. By regulating the temperature T2 and time t2 of dissolution within the above range, it is beneficial for the intermediate product to be fully dissolved, so as to obtain the product iron phosphate with the required iron-phosphorus molar ratio in the subsequent crystallization process.
[0041] In some embodiments of the present application, in step (4), the pH of the first filtrate is adjusted with water so that the pH of the obtained mixed solution is in the range of 0.7 to 2.5, and then crystallization is performed. During the crystallization process, H2O2 needs to be continuously added to reduce the Fe content in the mixed solution. 3+ Converted to Fe2+ If H2O2 is added too quickly, the pH of the mixed solution will be difficult to control, and some H2O2 will not have enough time to inhibit Fe 3+ Converted to Fe 2+ It has been thermally decomposed (because the crystallization process is carried out at high temperature), and H2O2 will produce oxygen after thermal decomposition, which will affect the crystallization of iron phosphate and thus affect the yield of iron phosphate; if the H2O2 is added too slowly, H2O2 is basically used to inhibit Fe 3+ Converted to Fe 2+ , it will not decompose in large quantities to produce oxygen and affect crystallization, but will cause a large number of crystals to precipitate, causing the iron phosphate crystals to agglomerate and increase the particle size. Excessive particle size may affect the electrochemical performance of the subsequently synthesized lithium iron phosphate. Therefore, it is necessary to control the addition speed and amount of H2O2 and select a suitable addition method, which is more conducive to obtaining the product iron phosphate with the required iron-phosphorus molar ratio and particle size, and improving the final recovery rate.
[0042] In some embodiments of the present application, in step (4), the rate V of addition of hydrogen peroxide is 0.017 mL / min to 0.03 mL / min. For example, the rate V of addition can be 0.017 mL / min, 0.018 mL / min, 0.019 mL / min, 0.02 mL / min, 0.021 mL / min, 0.022 mL / min, 0.023 mL / min, 0.024 mL / min, 0.025 mL / min, 0.026 mL / min, 0.027 mL / min, 0.028 mL / min, 0.029 mL / min or 0.03 mL / min, or between any two of the above numbers. By regulating the rate V of addition of hydrogen peroxide within the above range, part of the H2O2 is thermally decomposed to produce oxygen, which can inhibit the crystallization of iron phosphate to a certain extent, and the other part of the H2O2 is used to inhibit the crystallization of Fe 3+ Converted to Fe 2+ , which is beneficial to obtain the product iron phosphate with the required iron-phosphorus molar ratio and particle size, and improve the final recovery rate.
[0043] In this process, H2O2 needs to be added slowly and continuously during the regeneration and crystallization of iron phosphate to avoid Fe 3+ Converted to Fe 2+ , ensuring that no Fe is generated during the crystallization process 2+ The phosphate compound is added to ensure that a product that meets the iron-phosphorus ratio requirements is obtained, and further by controlling the addition speed, not only a high yield of iron phosphate is guaranteed, but also an iron phosphate product with a grain size that meets the requirements is obtained.
[0044] In some embodiments of the present application, the total amount of hydrogen peroxide added is: 1ml to 2ml of hydrogen peroxide is added for every 3g of waste lithium iron phosphate treated. For example, the amount of hydrogen peroxide added may be 1ml, 1.1ml, 1.2ml, 1.3ml, 1.4ml, 1.5ml, 1.6ml, 1.7ml, 1.8ml, 1.9ml or 2ml, or between any two of the above numbers. By regulating the total amount of hydrogen peroxide added within the above range, it is beneficial to obtain the product iron phosphate with the desired iron-phosphorus molar ratio and particle size, and to improve the final recovery rate.
[0045] In some embodiments of the present application, hydrogen peroxide is added in a dropwise manner, which has high operability and controllability and is also conducive to large-scale recovery and processing.
[0046] In some embodiments of the present application, in step (4), the temperature T3 of the crystallization treatment is 70°C to 110°C, and the time t3 is 3h to 6h. For example, the temperature T3 of the crystallization treatment can be 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C or 105°C, 110°C, or between any two of the above numbers. For example, the time t3 of the crystallization treatment can be 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, or between any two of the above numbers. By regulating the temperature T3 and time t3 of the crystallization treatment within the above range, it is beneficial to fully crystallize the iron phosphate and improve the recovery rate of the iron phosphate.
[0047] In some embodiments of the present application, in step (4), the calcination temperature T4 is 400°C to 700°C, and the time t4 is 1.5h to 6h. For example, the calcination temperature T4 can be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, or between any two of the above numbers. For example, the calcination time t4 can be 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, or between any two of the above numbers. By regulating the calcination temperature T4 and time t4 within the above range, it is beneficial to remove the crystal water in the ferric phosphate and improve the purity of the product ferric phosphate.
[0048] In some embodiments of the present application, the recovery method further comprises the following steps: (5) heating the second filtrate to make its volume the same as that of the first filtrate, and then adding the second filtrate to the first filtrate to continue dissolving the intermediate product. The iron phosphate remaining in the first filtrate can be recovered again to improve the final recovery rate of the iron phosphate.
[0049] In some embodiments of the present application, in step (1), the mass ratio X of waste lithium iron phosphate to (NH4)2SO4 is 1:(0.6 to 1); for example, the mass ratio X can be 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95 or 1:1, or between any two of the above ratios. Oxygen-containing gas is continuously introduced during roasting, and the oxygen-containing gas includes oxygen or air. By regulating the mass ratio X of waste lithium iron phosphate to (NH4)2SO4 within the above range, iron phosphate is not easily lost, which is conducive to obtaining more intermediates, and the leaching rate of lithium element is high, and a better impurity removal effect can be obtained. The calcination temperature T1 is 250°C to 400°C; for example, T1 can be 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, or between any two of the above numbers. By regulating the temperature T1 within the above range, (NH4)2SO4 is liquid and has an acidic pH, and can react with organic matter and carbon in waste lithium iron phosphate at temperature T1, thereby removing the organic matter and carbon. By regulating the temperature T1 and time t1 during roasting within the above range, the waste lithium iron phosphate and (NH4)2SO4 can fully react, which is conducive to the impurity elements and lithium elements forming corresponding sulfates, and the iron element forming iron phosphate, and the iron element is not easily oxidized to iron oxide, thereby achieving effective separation of iron sulfate and impurity elements in step (2), and sufficient leaching of lithium elements.
[0050] The present application has no particular limitation on the flow rate of the oxygen-containing gas, as long as the purpose of the present application can be achieved. For example, the flow rate of the oxygen-containing gas can be 24 L / min to 36 L / min. The volume content of oxygen in the oxygen-containing gas is greater than or equal to 15%.
[0051] In some embodiments of the present application, in step (1), the calcination time t1 is 0.5 h to 12 h.
[0052] The following reactions occur during the calcination process:
[0053] Al2O3+3(NH4)2SO4=Al2(SO4)3+6NH3+3H2O;
[0054] CaO+(NH4)2SO4=CaSO4+2NH3+H2O;
[0055] 4LiFePO4+2(NH4)2SO4+O2=4FePO4+2Li2SO4+4NH3+2H2O.
[0056] Among them, Al2(SO4)3 is soluble in water. After the roasting reaction, the Al element in the waste can be efficiently leached; CaSO4 is slightly soluble in water, with a solubility of about 0.2g / 100ml. Since the Ca content in the waste is not much, even if CaSO4 is slightly soluble in water after the reaction, most of the Ca elements can be effectively leached, so that the Ca content in the obtained iron phosphate slag meets the requirements; Li2SO4 is soluble in water, and FePO4 is insoluble in water. After the leaching treatment, the impurity elements aluminum and calcium can be separated from the iron phosphate, and the leaching of lithium can also be achieved.
[0057] In some embodiments of the present application, in step (2), the pH of the slurry obtained by mixing the roasted product with water is ≤3; the leaching solution contains Li + and impurity elements, including Al and / or Ca; the intermediate product contains phosphorus and iron (iron phosphate slag). For example, the pH of the slurry can be 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3, or between any two of the above numbers. In this process, the amount of water added is controlled, and the amount of water should not be too much. The pH of the slurry is regulated within the above range. The aluminum element exists in the form of ions. After leaching treatment and filtration, it is mainly present in the leachate, which can achieve effective separation from iron phosphate and reduce the content of impurity elements in the intermediate product. If too much water is added to make the pH of the slurry too high, for example, greater than 3, Al(OH)3 precipitation is easily generated, affecting the purity of the intermediate product. In this process, Li is achieved by water leaching. + The separation of impurity elements and iron phosphate is novel and less water is used during water immersion.
[0058] In some embodiments of the present application, the leaching solution in step (2) can further separate Li+ from impurities Al and Ca elements, for example, by adjusting the pH with an alkali solution to precipitate Al and Ca elements and separate them from Li+. The present application does not limit the above-mentioned alkali solution, as long as it can achieve the purpose of the present application.
[0059] In some embodiments of the present application, in step (2), the solid-to-liquid ratio Z of the roasted product to water is 0.1 g / ml to 0.3 g / ml. For example, the solid-to-liquid ratio Z can be 0.1 g / ml, 0.11 g / ml, 0.12 g / ml, 0.13 g / ml, 0.14 g / ml, 0.15 g / ml, 0.16 g / ml, 0.17 g / ml, 0.18 g / ml, 0.19 g / ml, 0.2 g / ml, 0.21 g / ml, 0.22 g / ml, 0.23 g / ml, 0.24 g / ml, 0.25 g / ml, 0.26 g / ml, 0.27 g / ml, 0.28 g / ml, 0.29 g / ml or 0.3 g / ml, or between any two of the above-mentioned numbers. Al2(SO4)3 has a higher solubility in water, while CaSO4 has a lower solubility in water than Al2(SO4)3. It is slightly soluble in water, with a solubility of about 0.2g / 100ml. Since the Ca content in the waste is less than the Al content, even if CaSO4 is slightly soluble in water after the reaction, most of the Ca elements can be effectively leached. By adjusting the solid-liquid ratio Z within the above range, during the leaching process, CaSO4 and Al2(SO4)3 can be fully dissolved in water, which is conducive to the effective separation of iron phosphate and impurity elements, and improves the purity of the purified iron phosphate slag.
[0060] In some embodiments of the present application, in step (2), the temperature T5 of the leaching treatment is 15°C to 35°C, and the time t5 is 0.5h to 10h. For example, T5 can be 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C or 35°C, or between any two of the above numbers. For example, t5 can be 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h, or between any two of the above numbers. By regulating the temperature T5 and time t5 of the leaching treatment within the above range, CaSO4 and Al2(SO4)3 can be fully dissolved in water, which is conducive to the effective separation of iron phosphate and impurity elements, improving the purity of purified iron phosphate slag, and reducing energy consumption.
[0061] In some embodiments of the present application, in step (2), the intermediate product obtained is further dried. The present application does not limit the drying parameters, as long as the purpose of the present application can be achieved.
[0062] In some embodiments of the present application, in the product ferric phosphate, the iron content W1 is 35.7wt% to 36.7wt%, and the phosphorus content W2 is 20.0wt% to 21.1wt%. For example, the iron content W1 can be 35.7wt%, 35.8wt%, 35.9wt%, 36.0wt%, 36.1wt%, 36.2wt%, 36.3wt%, 36.4wt%, 36.5wt%, 36.6wt% or 36.7wt%, or between any two of the above numbers. For example, the phosphorus content W2 can be 20.0wt%, 20.1wt%, 20.1wt%, 20.3wt%, 20.4wt%, 20.5wt%, 20.6wt%, 20.7wt%, 20.8wt%, 20.9wt%, 21.0wt% or 21.1wt%, or between any two of the above numbers. The iron content of the product iron phosphate is 35.7wt% to 36.7wt%, and the phosphorus content is 20.0wt% to 21.1wt%, which meets the requirements of battery-grade iron phosphate.
[0063] Example
[0064] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0065] Example 1
[0066] Figure 1 The experimental flow chart of Example 1 is as follows:
[0067] Take 3g of waste lithium iron phosphate and mix it with 2.4g of ammonium sulfate. After mixing, at T1=300℃, continue to let air flow for roasting for t1=2h. After roasting, put the roasted product into water according to the solid-liquid ratio Z of 0.3g / ml. The pH of the obtained slurry is 2.1, and then leaching treatment is carried out. The leaching treatment temperature is T5=25℃ and the time is t5=2h. After the leaching treatment is completed, it is filtered and the iron phosphate residue (i.e., the intermediate product) obtained by filtration is dried. The iron-phosphorus molar ratio tested by ICP is not within the range of (0.96 to 1):1, and does not meet the requirements yet.
[0068] Afterwards, the above-mentioned iron phosphate residue after drying is added to C=6mol / L phosphoric acid solution, the mass ratio Y of the intermediate product to the phosphoric acid solution is 1:20, under room temperature conditions, that is, T2=25°C, after stirring and dissolving for t2=12h, the first filtrate is filtered and collected, water is added to the first filtrate to obtain a mixed solution, and the pH of the mixed solution is 0.7. After completion, the above-mentioned mixed solution is regenerated and crystallized under T3=90°C. During the crystallization process, H2O2 needs to be continuously added dropwise, the dropwise addition speed V=0.03mL / min, the dropwise addition time is 1h, and the total dropwise addition amount is 1.8ml; crystallization t3=6h at T3=90°C. Afterwards, filter to obtain the filter residue and the second filtrate, and after the filter residue is dried, calcined under T4=550°C, the calcination time t4=3.5h, remove the crystallization water, and obtain 1.5g product iron phosphate. Among them, the Fe content is 35.8%, and the P content is 20.2%, which meets the requirements. The second filtrate is evaporated to remove the added water until the volume is the same as that of the first filtrate, and then added to the first filtrate for recycling.
[0069] In Example 1, through ICP test, the Al content in the waste lithium iron phosphate is 2288ppm, and the Ca content is 156.62ppm. The intermediate product iron phosphate residue obtained in Example 1 is subjected to ICP element test, and the Al content is 300ppm, and the Ca content is 80ppm, which meets the requirements of impurity content. It can be seen that the roasting process of this process has a good impurity removal effect, and the impurity content in the obtained iron phosphate residue meets the requirements, and the next step of dissolution and crystallization can be carried out.
[0070] The particle size D50 of the dried ferric phosphate residue obtained in Example 1 is 16.3 μm, and the particle size D50 of the product ferric phosphate is 2.8 μm. It can be seen that after crystallization treatment, not only the iron-phosphorus ratio in the product ferric phosphate meets the requirements, but also the product particle size meets the requirements.
[0071] Example 2 (pH adjusted to 1.0)
[0072] The only difference from Example 1 is that the pH of the mixed solution is adjusted to 1.0 by using water, and the rest is the same as Example 1. 2.8 g of product ferric phosphate is obtained, and the yield of ferric phosphate is high, wherein the Fe content is 36.1%, and the P content is 20.6%, which meets the requirements.
[0073] The impurity content of the ferric phosphate residue in Example 2 is the same as that in Example 1.
[0074] The particle size D50 of the product iron phosphate is 2.6 microns.
[0075] Example 3 (dropping speed 0.04 mL / min)
[0076] The only difference from Example 1 is that the dropping speed and dropping time of H2O2 are adjusted, the dropping speed V is 0.04mL / min, the dropping time is 45min, the total amount of dropping is 1.8ml, and the rest is the same as Example 1. 1.3g of product iron phosphate is obtained, wherein the Fe content is 35.9% and the P content is 20.2%, which meets the requirements.
[0077] It can be seen that the faster the H2O2 dripping speed is, the more H2O2 will be decomposed by heat before it can participate in the reaction, and the decomposition will produce oxygen. The generated bubbles will affect the crystallization process, resulting in the inability to effectively form grains and a decrease in the yield of iron phosphate.
[0078] The impurity content of the ferric phosphate residue in Example 3 is the same as that in Example 1.
[0079] Example 4 (dropping speed 0.015 mL / min)
[0080] The only difference from Example 1 is that the dropping speed and dropping time of H2O2 are adjusted, the dropping speed V is 0.015mL / min, the dropping time is 120min, the total amount of dropping is 1.8ml, and the rest is the same as Example 1. 1.5g of product ferric phosphate is obtained, wherein the Fe content is 35.9% and the P content is 20.3%, which meets the requirements.
[0081] Compared with Example 1, it was found during the experiment that more iron phosphate was precipitated in a shorter time in Example 4. This was because the dripping speed was slow, and hydrogen peroxide was basically used to inhibit the oxidation of trivalent iron ions in the solution. It would not decompose in large quantities to produce oxygen and affect crystallization, resulting in a large amount of crystals being precipitated in the end. The iron phosphate precipitated too quickly, causing the iron phosphate crystals to agglomerate and the particle size to increase. In this embodiment, the particle size D50 was 11.2 microns, and ball milling was required to obtain a product with a qualified particle size.
[0082] The impurity content of the ferric phosphate residue in Example 4 is the same as that in Example 1.
[0083] Example 5 (pH adjusted to 1.5)
[0084] The only difference from Example 2 is that the pH of the mixed solution is adjusted to 1.5 with water; the crystallization temperature T3 = 105°C, the crystallization t3 = 3h; the dripping speed V of H2O2 = 0.02mL / min, the dripping time is 100min, and the total dripping amount is 2ml; the calcination temperature T4 = 700°C, the calcination time t4 = 2h, and the rest is the same as Example 1. The product iron phosphate is about 2.8g, wherein the Fe content is 36.1% and the P content is 20.9%, which meets the requirements.
[0085] In this embodiment, in the process of adjusting the pH value of the filtrate by water, a product ferric phosphate with a quality similar to that of Example 2 is obtained, which requires more water, about twice that of Example 2, and consumes more energy during subsequent evaporation.
[0086] The impurity content of the ferric phosphate residue in Example 5 is the same as that in Example 2.
[0087] Comparative Example 1 (pH is too low to 0.5)
[0088] The only difference from Example 1 is that the pH of the mixed solution is adjusted to 0.5 by using water, and the rest is the same as Example 1. 0.3 g of product iron phosphate is obtained, wherein the Fe content is 35.9%, the P content is 20.1%, and the iron-phosphorus ratio of the product meets the requirements. This indicates that a large amount of iron phosphate has not been crystallized.
[0089] Comparative Example 2 (pH is too high at 3)
[0090] The only difference from Example 1 is that the pH of the mixed solution is adjusted to 3 by using water, and the rest is the same as Example 1. A large amount of white precipitate is generated during the crystallization process, and subsequent treatment cannot be performed.
[0091] Comparative Example 3 (without adding H2O2)
[0092] The only difference from Example 1 is that no H2O2 is added during the crystallization process. Figure 2 As shown, the right side is the mixed solution in Comparative Example 3, and the mixed solution is colorless and transparent; the left side is the mixed solution in Example 1, and the mixed solution in Example 1 presents Fe 3+ The yellow color indicates that the iron in the mixed solution is mainly in the form of Fe 3+ Form exists.
[0093] In Comparative Example 3, the Fe content of the product ferric phosphate is 38.5%, and the P content is 20.2%, which cannot meet the requirements.
[0094] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A method for recycling the positive electrode of waste lithium iron phosphate batteries, comprising the following steps: (1) dismantling waste lithium iron phosphate batteries to obtain waste lithium iron phosphate, mixing the waste lithium iron phosphate with (NH4)2SO4 and then calcining to obtain a calcined product; (2) mixing the roasted product with water for leaching, and then filtering to obtain a leachate and a solid intermediate product; (3) mixing the intermediate product with a phosphoric acid solution, dissolving the mixture, and filtering the mixture to obtain a first filtrate; (4) mixing the first filtrate with water to obtain a mixed solution, and then performing a crystallization treatment, adding hydrogen peroxide during the crystallization treatment, and then filtering to obtain a filter residue and a second filtrate, and calcining the filter residue to obtain a product ferric phosphate; Wherein, the pH of the mixed solution is 0.7 to 2.
5.
2. The recycling method according to claim 1, wherein: In step (3), the concentration C of the phosphoric acid solution is 1 mol / L to 6 mol / L, and the mass ratio Y of the intermediate product to the phosphoric acid solution is 1:(5 to 20).
3. The recycling method according to claim 1, wherein: In step (3), the dissolution time t2 is 3 h to 12 h, and the dissolution temperature T2 is 15 to 35 °C.
4. The recycling method according to claim 1, wherein: In step (4), the rate V of addition of hydrogen peroxide is 0.017 mL / min to 0.03 mL / min; Preferably, the total amount of hydrogen peroxide added is: 1 ml to 2 ml of hydrogen peroxide is added for every 3 g of waste lithium iron phosphate treated; Preferably, the hydrogen peroxide is added dropwise.
5. The recycling method according to claim 1, wherein: In step (4), the pH of the mixed solution is 0.9 to 1.
2.
6. The recycling method according to claim 1, wherein: In step (4), the temperature T3 of the crystallization treatment is 70° C. to 110° C., and the time t3 is 3 h to 6 h; Preferably, in step (4), the calcination temperature T4 is 400° C. to 700° C., and the calcination time t4 is 1.5 h to 6 h.
7. The recycling method according to claim 1, wherein: It also includes the following steps: (5) heating the second filtrate to make its volume the same as that of the first filtrate, and then adding it to the first filtrate to continue dissolving the intermediate product.
8. The recovery method according to any one of claims 1 to 7, wherein: In step (1), the mass ratio X of the waste lithium iron phosphate to (NH4)2SO4 is 1:(0.6 to 1); The calcination temperature T1 is 250°C to 400°C; During the calcination, an oxygen-containing gas is continuously introduced, and the oxygen-containing gas includes oxygen or air.
9. The recovery method according to any one of claims 1 to 7, wherein: In step (2), the pH of the slurry obtained by mixing the roasted product with water is ≤3; The leaching solution contains Li + and impurity elements, wherein the impurity elements include Al and / or Ca; The intermediate product contains phosphorus and iron.
10. The recycling method according to claim 1, wherein: The product ferric phosphate has an iron content of 35.7wt% to 36.7wt% and a phosphorus content of 20.0wt% to 21.1wt%.
Citation Information
Patent Citations
Method for recycling waste lithium iron phosphate battery at low temperature regenerating lithium iron phosphate positive electrode material
CN113562717A
Method for treating high-impurity lithium iron phosphate waste powder by using low-consumption phosphoric acid
CN113880064A
Purification treatment method and system for ferrophosphorus slag mixture containing Al and Cu impurities
CN114421044A
Method for recovering iron phosphate slag after lithium extraction of battery
CN117069081A
Method for preparing iron phosphate and use thereof
WO2022116702A1
Cited By
Method for recovering lithium and iron in lithium iron phosphate-containing material
CN121109754A