Method for in-situ construction of silicon-based / graphene / ferroelectric composite material on current collector and application of silicon-based / graphene / ferroelectric composite material
By constructing silicon-based/graphene/ferroelectric composite materials in situ on the current collector in lithium-ion batteries, using laser induction and high-voltage corona polarization technology, the insufficient circulation performance of silicon-based anode materials in lithium-ion batteries is solved. Problem, higher lithium ion diffusion rate and cycling stability are achieved.
Patent Information
- Application Number
- CN202410990756.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The cycling performance of silicon-based anode materials in lithium-ion batteries is insufficient at high magnification, mainly due to the insufficient polarization strength of ferroelectric materials and the random spontaneous polarization direction, resulting in poor fast charging stability.
Silicon-based/graphene/ferroelectric composite materials are constructed in situ on the current collector, and the ferroelectric/graphene layer and silicon-based/graphene layer are prepared through laser induction technology, and the high-voltage corona polarization method is used to establish directional Uniform built-in electric field, adjusts ion migration and alleviates stress caused by volume expansion.
It significantly improves the diffusion rate and cyclic stability of lithium ions, optimizes the migration mechanism of lithium ions, delays the formation of lithium dendrites, and enhances the cycling capacity of the battery and the performance under large current density.
Smart Images

Figure CN118908191A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a method for in-situ construction of a silicon-based / graphene / ferroelectric composite material on a current collector and its application. Background Art
[0002] Lithium-ion batteries (LIBs) have been successfully commercialized and widely used in mobile electronic devices due to their high energy density and long service life. However, there is a growing demand for advanced LIBs with higher specific capacity and longer cycle life to drive electric vehicles and high-end electronic devices. The specific capacity of existing electrode materials such as commercialized graphite anodes has reached 360 mAh / g, which is close to its theoretical specific capacity (372 mAh / g), but still cannot meet the demand, which has stimulated the research on new electrode materials.
[0003] Silicon-based anode materials are considered to be potential candidates for graphite anodes due to their high specific capacity (the theoretical specific capacity of elemental silicon is 4200mAh / g, and the specific capacity of silicon oxide is 2680mAh / g) and low working potential (~0.4V). The drastic volume expansion of silicon-based materials during lithium insertion is considered to be a key limitation, and the resulting silicon pulverization will lead to a significant deterioration in performance. By forming silicon-based composite materials with other active conductive materials (carbonaceous materials such as hard carbon, graphene or carbon nanotubes) or by designing a controllable structure to provide buffer space (such as a three-dimensional porous structure), the lithium storage behavior of silicon-based materials can be regulated to improve the first coulombic efficiency and cycle stability. However, the cycling performance of silicon-based anode materials for lithium-ion batteries at high rates still needs to be optimized.
[0004] In recent years, various energy-generating materials (such as piezoelectric, pyroelectric and ferroelectric materials) and their composites have been actively applied to new energy conversion devices. In particular, artificial interfacial layers based on ferroelectric materials (such as polyvinylidene fluoride and barium titanate) have been used to regulate metal deposition in lithium / zinc metal batteries. In addition, ferroelectric materials are also a type of piezoelectric materials that can achieve conversion between mechanical energy and electrical energy. The piezoelectricity in the present invention is caused by internal stress, that is, the large volume expansion of the silicon-based material is transferred to the piezoelectric material, and the piezoelectric material can be polarized. This strategy relies on the ferroelectricity of the coating to induce a uniform and switchable electric polarization surface to guide the orderly ion migration, so that the problem of non-uniformity of ion flux can be solved to a certain extent. In order to realize this concept, strong adhesion between the silicon-based material and the ferroelectric material and the carbon matrix is required. The carbon matrix transfers the mechanical stress caused by the large-scale expansion of the silicon-based material to the piezoelectric material while maintaining the conductive path of lithium ions. However, due to the limited polarization degree of the ferroelectric layer along the perpendicular direction of the negative electrode, the rapid supply of ions is usually still insufficient. This is related to the low intensity of the self-built electric field (E) in the battery, which leads to a limited polarization domain in the direction of the battery's self-built electric field. In addition, the spontaneous polarization direction of ferroelectric materials under pressure is random. Therefore, the fast charging stability is still far from the expected effect.
[0005] Therefore, if the polarization strength of ferroelectric materials can be enhanced and a directional, uniform and improved built-in electric field can be constructed, the fast charging performance of lithium-ion batteries will inevitably be improved. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for in-situ construction of a silicon-based / graphene / ferroelectric composite material on a current collector, and directly apply the silicon-based / graphene / ferroelectric composite material loaded on the current collector as a negative electrode to a lithium-ion battery. First, corona polarization treatment of the ferroelectric layer can generate a directional and uniform built-in electric field, optimize the nonlinear spatial distribution of the field gradient, and effectively regulate the ion migration between the electrode and the electrolyte. Secondly, the ferroelectric layer also has piezoelectric properties. During the lithiation process, the volume expansion of the silicon particles causes compressive stress, partially reverses the deformation of the ferroelectric layer, and reduces the local built-in field. Subsequently, the diffusion direction of lithium ions also changes, thereby alleviating excessive internal stress. In addition, this silicon-based / graphene / ferroelectric composite material is prepared in-situ on the current collector, ensuring the losslessness of the self-integrated structure. In addition, the silicon-based material is encapsulated in situ into a three-dimensional graphene network to achieve effective physical confinement. At the same time, the three-dimensional hierarchical porous structure promotes ion transport and charge transfer, and alleviates mechanical deformation. Therefore, the silicon-based / graphene / ferroelectric composite material in situ constructed on the current collector has outstanding cycling stability and excellent charge and discharge performance at high rates.
[0007] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0008] The first object of the present invention is to provide a method for in-situ construction of a silicon-based / graphene / ferroelectric composite material on a current collector, comprising the following steps:
[0009] (1) fully mixing a ferroelectric material, a polymer or its precursor, and a solvent, coating the mixture on a current collector, and drying and curing the mixture to form a ferroelectric / polymer film on the current collector;
[0010] (2) Using laser-induced technology to process ferroelectric / polymer films and in-situ construct ferroelectric / graphene composite materials on the current collector;
[0011] (3) fully mixing the silicon-based material, the polymer or its precursor, and the solvent, coating the mixture on the ferroelectric / graphene composite material, drying and curing the mixture, and forming a silicon-based / polymer / ferroelectric / graphene composite material on the current collector;
[0012] (4) Using laser induction technology to process silicon-based / polymer / ferroelectric / graphene composites, in situ constructing silicon-based / graphene / ferroelectric composite materials on current collectors;
[0013] (5) The silicon-based / graphene / ferroelectric composite material was treated by high-voltage corona polarization.
[0014] The present invention utilizes laser induction technology to directly prepare a ferroelectric / graphene layer in situ on a current collector, then utilizes laser induction technology to in situ prepare a silicon-based / graphene layer on the ferroelectric / graphene layer, and finally uses high-voltage corona poling to treat the silicon-based / graphene / ferroelectric composite material constructed in situ on the current collector to obtain a polarized silicon-based / graphene / ferroelectric composite material on the current collector.
[0015] The second object of the present invention is to provide a silicon-based / graphene / ferroelectric / current collector composite material prepared by the aforementioned method.
[0016] The third object of the present invention is to provide application of the silicon-based / graphene / ferroelectric / current collector composite material in lithium-ion batteries.
[0017] A fourth object of the present invention is to provide a lithium-ion battery using the silicon-based / graphene / ferroelectric / current collector composite material as a negative electrode.
[0018] The beneficial effects of the present invention are:
[0019] 1. The present invention mainly utilizes high-voltage corona polarization ferroelectric / graphene coating to establish a built-in electric field in the ferroelectric layer, optimizes the nonlinear spatial distribution of ion concentration and electric field gradient (especially at high rates), optimizes the transport mechanism of lithium ions in solid particles and liquid electrolytes, provides a new driving force for the migration of lithium ions, promotes the diffusion of lithium ions from local high-concentration sites to surrounding areas more quickly and more evenly, and avoids the damage of lithium dendrite growth to battery performance; in addition, the ferroelectric / graphene intermediate layer can reduce the crushing effect of silicon particles caused by volume expansion during lithiation; secondly, ferroelectric materials also have piezoelectric properties. During the lithiation process, the volume expansion of silicon particles causes compressive stress, partially reverses the deformation of the ferroelectric body, and reduces the local Internal electric field (positive piezoelectric effect) is modulated, which promotes the dispersion of lithium ions to alternating sites and dynamically regulates the transport of lithium ions, thereby alleviating excessive internal stress; in addition, the silicon-based / graphene / ferroelectric composite material is prepared in situ on the current collector using laser induced technology, ensuring the losslessness of the self-integrated structure, and there is no need to add additional inactive binders to induce unnecessary side reactions; in situ synthesis ensures that silicon oxide is encapsulated into the three-dimensional graphene network, which has a complete encapsulation effect and prevents particles from falling off; finally, the continuous ion transport channel and conductive network provided by the three-dimensional graphene network increase the contact area between the electrode and the electrolyte, reduce the local current density, delay the formation of lithium dendrites, reduce the steric hindrance of ion transport, and help alleviate volume expansion.
[0020] 2. The silicon-based / graphene / ferroelectric composite material in-situ constructed on the current collector of the present invention can be applied to the negative electrode of lithium-ion batteries, and has a high lithium ion diffusion rate and excellent cycle capacity and cycle stability under high current density; and the method provided by the present invention is easy to operate and has strong scalability, and has broad application prospects in the field of secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The scanning electron microscope image and particle size distribution diagram of barium titanate in Example 1;
[0022] Figure 2 is the X-ray diffraction pattern of barium titanate in Example 1;
[0023] Figure 3 is the Raman spectrum of barium titanate in Example 1;
[0024] Figure 4 This is a test diagram of the contact angle of Si / LIG / UBTO prepared in Example 1 to the lithium-ion battery electrolyte;
[0025] Figure 5 This is a test diagram of the contact angle of Si / LIG / NBTO prepared in Comparative Example 1 to the lithium-ion battery electrolyte;
[0026] Figure 6 A comparison of lithium ion diffusion coefficients of lithium ion batteries assembled using Si / LIG / UBTO prepared in Example 1, Si / LIG / NBTO prepared in Comparative Example 1, and Si / LIG prepared in Comparative Example 2 as negative electrodes;
[0027] Figure 7 It is a comparison chart of the cycle performance of lithium-ion batteries assembled with Si / LIG / UBTO prepared in Example 1, Si / LIG / NBTO prepared in Comparative Example 1, and Si / LIG prepared in Comparative Example 2 as negative electrodes. DETAILED DESCRIPTION
[0028] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments and diagrams.
[0029] The present invention provides a method for in-situ construction of a silicon-based / graphene / ferroelectric composite material on a current collector, comprising the following steps:
[0030] (1) fully mixing a ferroelectric material, a polymer or its precursor, and a solvent, coating the mixture on a current collector, and drying and curing the mixture to form a ferroelectric / polymer film on the current collector;
[0031] (2) Using laser-induced technology to process ferroelectric / polymer films and in-situ construct ferroelectric / graphene composite materials on the current collector;
[0032] (3) fully mixing the silicon-based material, the polymer or its precursor, and the solvent, coating the mixture on the ferroelectric / graphene composite material, drying and curing the mixture, and forming a silicon-based / polymer / ferroelectric / graphene composite on the current collector;
[0033] (4) Using laser induction technology to process silicon-based / polymer / ferroelectric / graphene composites, in situ constructing silicon-based / graphene / ferroelectric composite materials on current collectors;
[0034] (5) The silicon-based / graphene / ferroelectric composite material was treated by high-voltage corona polarization.
[0035] Furthermore, the ferroelectric material is selected from one or more of oxide ferroelectrics (such as barium titanate, lead zirconate titanate, lead tungstate, lead titanate, potassium niobate, lithium niobate, etc.), halide ferroelectrics (such as thallium bromide, lead bromide, etc.), chalcogenide ferroelectrics (such as germanium sulfide, gallium sulfide, etc.), hydrogen bond ferroelectrics (such as potassium dihydrogen phosphate, ammonium dihydrogen phosphate, etc.), and organic ferroelectrics (such as polyvinylidene fluoride and its copolymers, polyvinyl alcohol, etc.).
[0036] Furthermore, the size of the ferroelectric material is 1 nm to 100 μm.
[0037] Furthermore, the polymer is selected from one or more of polyethylene, polypropylene, polysulfide rubber, polyvinyl chloride, polyetherimide, polyetheretherketone, polyether, polyimide, polyester, polyamide, polyurethane and the like.
[0038] Furthermore, the mass ratio of the ferroelectric material, the polymer or its precursor is 1:(0.01-1000).
[0039] Furthermore, the current collector includes but is not limited to one or more of single-sided copper foil, double-sided copper foil, carbon-coated copper foil, foam copper, carbon cloth, carbon paper, nickel foil, and foam nickel, and has a thickness of 100 nm to 100 μm.
[0040] Furthermore, the solvent is N-methylpyrrolidone (NMP). NMP is a commonly used slurry preparation solvent in the preparation process of lithium-ion battery electrodes, and has the advantages of being non-toxic, low in viscosity, low in corrosiveness, good in stability, and good in wettability to current collectors.
[0041] Furthermore, the drying and curing temperature is 25-500° C. The curing can be carried out at room temperature or under heating conditions.
[0042] Furthermore, the laser is selected from one or more of solid laser, gas laser, semiconductor laser, fiber laser, pulse laser, continuous laser and excimer laser, the laser wavelength is 0.01-100 μm, the laser power is 0.1-1000 W, the scanning rate is 0.1-1000 mm / s, the scanning spacing is 0.001-10 mm, the pulse frequency is 0.01-500 kHz, the focal length is 0.1-200 cm, and the pressure range is 1-2000 kV.
[0043] Furthermore, the silicon-based material includes but is not limited to one or more of silicon, silicon-carbon, silicon-oxygen, and silicon-oxygen-carbon.
[0044] Furthermore, the size of the silicon-based material is 1 nm to 30 μm.
[0045] Furthermore, the mass ratio of the silicon-based material, the polymer or its precursor is 1:(0.1-200).
[0046] Furthermore, the polarization voltage of the high-voltage corona polarization is 0.01-1000 kV, the polarization time is 0.001-100 h, the polarization temperature is 5-50° C., and the distance from the tip to the current collector is 0.001-100 cm.
[0047] Furthermore, the mass proportion of the ferroelectric material in the silicon-based / graphene / ferroelectric composite material is 0.1-50%.
[0048] Furthermore, the mass proportion of the silicon-based material in the silicon-based / graphene / ferroelectric composite material is 1-90%.
[0049] The present invention provides a silicon-based / graphene / ferroelectric / current collector composite material prepared by the aforementioned method.
[0050] The present invention provides application of the silicon-based / graphene / ferroelectric / current collector composite material in a lithium-ion battery.
[0051] The present invention provides a lithium ion battery, using the silicon-based / graphene / ferroelectric / current collector composite material as a negative electrode.
[0052] The technical solution of the present invention is described in detail below through specific embodiments:
[0053] Example 1
[0054] (1) 10 g of barium titanate particles (D50 = 200 nm) were ultrasonically dispersed in 30 mL of NMP, and 35 g of polyamic acid was added and stirred to obtain a uniform slurry. The slurry was then coated on a 15 μm thick single-sided smooth copper foil with a coating thickness of 50 μm. The slurry was then dried and cured in a vacuum oven (heating program was 60°C / 12 h, 80°C / 2 h, 100°C / 2 h, 120°C / 2 h, 140°C / 2 h, and 250°C / 2 h), and naturally cooled to room temperature to obtain a barium titanate / polyimide film.
[0055] (2) The barium titanate / polyimide film prepared in step (1) was induced by a carbon dioxide infrared laser with a wavelength of 10.6 μm, a laser scanning power of 6.6 W, a scanning rate of 200 mm / s, a scanning spacing of 0.08 mm, a pulse frequency of 20 kHz, a focal length of 3.4 cm, and a voltage of 100 kV to in-situ construct a barium titanate / graphene layer on the copper foil.
[0056] (3) 20 g of elemental silicon particles (D50 = 500 nm) were ultrasonically dispersed in 25 mL of NMP, and 20 g of polyimide was added and stirred to obtain a uniform slurry. The slurry was then applied to the barium titanate / graphene layer prepared in step (2) with a coating thickness of 60 μm. The mixture was then dried and cured in a vacuum oven (heating procedure was 60°C / 24 h, 100°C / 1 h, 150°C / 1 h, 200°C / 1 h, and 250°C / 1 h), and naturally cooled to room temperature to form a silicon / polyimide film on the barium titanate / graphene layer.
[0057] (4) The silicon / polyimide film prepared in step (3) was induced by a carbon dioxide infrared laser with a wavelength of 10.6 μm, the laser scanning power was 8.0 W, the scanning rate was 100 mm / s, the scanning spacing was 0.1 mm, the pulse frequency was 20 kHz, the focal length was 3.4 cm, and the voltage was 100 kV, to form a silicon / graphene layer on the barium titanate / graphene layer, that is, a silicon / graphene / barium titanate composite material was in situ constructed on the copper foil. The thickness of the barium titanate / graphene layer was 35 μm, and the mass proportion of barium titanate in the composite material was 20%. The thickness of the silicon / graphene layer was 55 μm, and the mass proportion of silicon in the composite material was 55%.
[0058] (5) The silicon / graphene / barium titanate composite material prepared in step (4) was treated by high-voltage corona poling method, with a polarization voltage of 20 kV, a polarization time of 1 h, a distance from the stainless steel tip to the copper foil of 15 cm, and a polarization temperature of 20° C., and finally, a barium titanate / graphene intermediate layer and a silicon / graphene active layer (named Si / LIG / UBTO) were in situ constructed on the copper foil.
[0059] from Figure 1 It can be seen that barium titanate is a monodisperse particle with a size mainly concentrated at 200 nm.
[0060] from Figure 2 It can be seen that barium titanate maintains a good crystal structure and can be precisely matched with tetragonal barium titanate (PDF#05-0626).
[0061] from Figure 3 It can be seen that at 305 and 715 cm -1 The Raman peaks nearby are considered to be characteristic peaks of the ferroelectric tetragonal structure.
[0062] from Figure 4 It can be seen that the Si / LIG / UBTO prepared in Example 1 has good wetting properties to the lithium-ion battery electrolyte (1MLiPF6+EC / DEC).
[0063] Comparative Example 1
[0064] The preparation method of this comparative example is the same as that of Example 1, and the only difference from Example 1 is that the silicon / graphene / barium titanate composite material (named Si / LIG / NBTO) constructed on the copper foil is not treated by high-voltage corona poling.
[0065] from Figure 5 It can be seen that the Si / LIG / NBTO prepared in Comparative Example 1 also has good wetting properties to the lithium-ion battery electrolyte (1MLiPF6+EC / DEC), indicating that corona polarization will not affect the wetting properties of the material to the electrolyte.
[0066] Comparative Example 2
[0067] The preparation method of this comparative example is the same as that of Example 1, and the only difference from Example 1 is that steps (1) and (2) are not performed, that is, the silicon / graphene composite material (named Si / LIG) is directly constructed in situ on the current collector.
[0068] Example 2
[0069] (1) 15 g of thallium bromide (D50 = 500 nm) was ultrasonically dispersed in 40 mL of NMP, and 55 g of polyethylene was added and stirred to obtain a uniform slurry. The slurry was then coated on a 12 μm thick carbon-coated copper foil with a coating thickness of 30 μm. The slurry was then dried and cured in a vacuum oven (heating program was 80°C / 10 h, 100°C / 1 h, 180°C / 1 h, 250°C / 1 h, 300°C / 2 h), and naturally cooled to room temperature to obtain a thallium bromide / polyethylene film.
[0070] (2) The thallium bromide / polyethylene film prepared in step (1) was induced by a carbon dioxide laser with a wavelength of 1064 nm, a laser scanning power of 10.5 W, a scanning rate of 300 mm / s, a scanning spacing of 0.12 mm, a pulse frequency of 30 kHz, a focal length of 3.7 cm, and a voltage of 70 kV to in situ construct a thallium bromide / graphene layer on a carbon-coated copper foil.
[0071] (3) 15 g of silicon dioxide particles (D50 = 300 nm) were ultrasonically dispersed in 30 mL of NMP, and 50 g of polyethylene was added and stirred to obtain a uniform slurry. The slurry was then coated on the thallium bromide / graphene layer prepared in step (2) with a coating thickness of 45 μm. The slurry was then dried and cured in a vacuum oven (heating program was 60°C / 12 h, 140°C / 1 h, 180°C / 1 h, 220°C / 1 h, and 250°C / 1 h), and naturally cooled to room temperature to form a silicon dioxide / polyethylene film on the thallium bromide / graphene layer.
[0072] (4) The silicon oxide / polyethylene film prepared in step (3) is induced by a carbon dioxide laser with a wavelength of 1064 nm, the laser scanning power is 8.8 W, the scanning rate is 150 mm / s, the scanning interval is 0.12 mm, the pulse frequency is 30 kHz, the focal length is 3.7 cm, and the voltage is 70 kV, to form a silicon oxide / graphene layer on the thallium bromide / graphene layer, that is, a silicon oxide / graphene / thallium bromide composite material is in situ constructed on the carbon-coated copper foil. The thickness of the thallium bromide / graphene layer is 25 μm, and the mass proportion of thallium bromide in the composite material is 25%, and the thickness of the silicon oxide / graphene layer is 45 μm, and the mass proportion of silicon oxide material in the composite material is 25%.
[0073] (5) The silicon dioxide / graphene / thallium bromide composite material constructed on the carbon-coated copper foil in step (4) was treated by high-voltage corona polarization method, with a polarization voltage of 30 kV, a polarization time of 3 h, a distance from the stainless steel tip to the carbon-coated copper foil of 10 cm, and a polarization temperature of 25° C., and finally, a thallium bromide / graphene intermediate layer and a silicon dioxide / graphene active layer were in situ constructed on the carbon-coated copper foil.
[0074] Example 3
[0075] (1) 50 g of germanium sulfide (D50 = 1 μm) was ultrasonically dispersed in 24 mL of NMP, and 70 g of polyetheretherketone was added and stirred to obtain a uniform slurry. The slurry was then coated on a 10 μm thick carbon cloth with a coating thickness of 10 μm. The slurry was then dried and cured in a vacuum oven (heating program was 60°C / 8 h, 150°C / 2 h, 200°C / 2 h, 250°C / 1 h, and 350°C / 2 h), and naturally cooled to room temperature to obtain a germanium sulfide / polyetheretherketone film.
[0076] (2) The germanium sulfide / polyetheretherketone film prepared in step (1) was induced by visible light laser with a wavelength of 405 nm, the laser scanning power was 14.5 W, the scanning rate was 250 mm / s, the scanning spacing was 0.05 mm, the pulse frequency was 55 kHz, the focal length was 4.2 cm, and the voltage was 100 kV, and the germanium sulfide / graphene layer was in situ constructed on the carbon cloth.
[0077] (3) Ultrasonic dispersion of 25 g of silicon oxide carbon particles (D50 = 800 nm) in 50 mL of NMP, and then adding 60 g of polyetheretherketone, stirring to obtain a uniform slurry, and then coating the slurry on the germanium sulfide / graphene layer prepared in step (2) with a coating thickness of 75 μm, followed by drying and curing in a vacuum oven (heating program of 60°C / 12 h, 140°C / 2 h, 200°C / 1 h, 250°C / 1 h, 320°C / 1 h), and naturally cooling to room temperature to form a silicon oxide carbon / polyetheretherketone film on the germanium sulfide / graphene layer.
[0078] (4) Using visible light laser with a wavelength of 405 nm to induce the silicon oxygen carbon / polyether ether ketone film prepared in step (3), the laser scanning power is 5.4 W, the scanning rate is 200 mm / s, the scanning interval is 0.15 mm, the pulse frequency is 50 kHz, the focal length is 4.2 cm, and the voltage is 40 kV, a silicon oxygen carbon / graphene layer is formed on the germanium sulfide / graphene layer, that is, a silicon oxygen carbon / graphene / germanium sulfide composite material is in situ constructed on the carbon cloth. The thickness of the germanium sulfide / graphene layer is 15 μm, the mass proportion of germanium sulfide in the composite material is 20%, the thickness of the silicon oxygen carbon / graphene layer is 65 μm, and the mass proportion of the silicon oxygen carbon material in the composite material is 45%.
[0079] (5) The silicon oxygen carbon / graphene / germanium sulfide composite material constructed on the carbon cloth in step (4) was treated by high voltage corona polarization method, with a polarization voltage of 50 kV, a polarization time of 12 h, a distance from the stainless steel tip to the carbon cloth of 6 cm, and a polarization temperature of 15°C. Finally, a germanium sulfide / graphene intermediate layer and a silicon oxygen carbon / graphene active layer were in situ constructed on the carbon cloth.
[0080] Example 4
[0081] The preparation method of this embodiment is the same as that of embodiment 1, and the only difference from embodiment 1 is that the single substance silicon D50=800nm.
[0082] Example 5
[0083] The preparation method of this embodiment is the same as that of Embodiment 2, and the only difference from Embodiment 2 is that the mass of silicon iodide is 35 g.
[0084] Example 6
[0085] The preparation method of this embodiment is the same as that of Embodiment 3, and the only difference from Embodiment 3 is that the corona polarization voltage is 25 kV.
[0086] The Si / LIG / UBTO prepared in Example 1, the Si / LIG / NBTO prepared in Comparative Example 1, and the Si / LIG prepared in Comparative Example 2 were used as negative electrodes to assemble CR2032 button-type lithium-ion half-cells, and their electrochemical properties were tested. The results are shown in FIG. Figure 6 and Figure 7 .
[0087] Si / LIG / UBTO, Si / LIG / NBTO and Si / LIG were punched into disc electrodes with a diameter of 12 mm, and then the assembly process was completed in a glove box filled with argon (water and oxygen content less than 0.1 ppm). Lithium metal sheets were used as counter / reference electrodes, Celgard2400 microporous membranes were used as separators, and 1M LiPF6 dissolved in a mixed solution of ethylene carbonate and diethyl carbonate (volume ratio of 1:1) was used as the electrolyte.
[0088] The lithium ion diffusion coefficient and cycle performance were tested at room temperature using a BlueDian CT2001A battery test system (Wuhan BlueDian Electronics Co., Ltd., China) with a potential window ranging from 0.01 to 3 V (relative to Li / Li + ). All tests were carried out at 25°C.
[0089] The constant current intermittent titration technique (GITT) was used to further analyze the Li + Diffusion coefficient, pulse duration 10min, interval time 30min, 8 cycles of charge-discharge cycling at 0.1A / g before GITT test.1 / 2 When there is a linear correlation, the diffusion rate of lithium ions can be calculated according to Fick's second law of diffusion.
[0090] from Figure 6 It can be seen that Si / LIG without ferroelectric layer exhibits lower Li + The diffusion coefficient is at the -12th power level, which can be attributed to the slow ion transport kinetics inside the battery, especially the solid electrode material and the electrolyte interface, and the large concentration polarization hinders the Li + Diffusion. After constructing a ferroelectric layer between the Si / LIG active layer and the current collector, Si / CNT / NBTO was obtained, which showed an improved lithium ion diffusion coefficient. This is because the BTO layer at room temperature has ferroelectricity and piezoelectricity. The mechanical stress generated by the expansion of silicon is transferred to BTO through the carbon matrix. BTO can be polarized to generate a piezoelectric potential. This local piezoelectric potential can improve the electrochemical performance of the Si / LIG / NBTO nanocomposite anode. However, due to the limited built-in battery strength caused by the volume expansion of silicon and the randomness of the direction of this spontaneous polarization, the rapid supply of ions is still insufficient. Li of Si / LIG / NBTO prepared by high-voltage corona polarization treatment + The diffusion coefficient is significantly enhanced, showing an excellent ion transport rate at the -10th power level, which is beneficial to the improvement of the cycle performance of lithium-ion batteries at high current density. Therefore, the built-in electric field constructed by corona polarization treatment optimizes the spatial distribution of concentration gradient and electric field gradient, showing fast and uniform lithium insertion and extraction behavior.
[0091] from Figure 7 It can be seen that at a higher current density of 2.0A / g, the cycle stability of Si / LIG and Si / LIG / NBTO electrodes is poor, and the capacity decays rapidly. However, the cycle stability of Si / LIG / UBTO after high-voltage corona polarization treatment is significantly improved, showing excellent capacity retention in 100 charge and discharge cycles, and the specific capacity is stably maintained at around 1200mAh / g, which is significantly better than Si / LIG / NBTO and Si / LIG that have not been polarized. High-voltage corona polarization treatment can generate a directional and effective built-in electric field in the ferroelectric layer, promoting the homogenization and self-accelerated migration and deposition of lithium ions. In addition, the interfacial coating also acts as a physical barrier, playing a role in mechanically inhibiting the growth of lithium dendrites.
[0092] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for in-situ construction of a silicon-based / graphene / ferroelectric composite material on a current collector, characterized in that: The following steps are involved: (1) fully mixing a ferroelectric material, a polymer or its precursor, and a solvent, coating the mixture on a current collector, and drying and curing the mixture to form a ferroelectric / polymer film on the current collector; (2) Using laser-induced technology to process ferroelectric / polymer films and in-situ construct ferroelectric / graphene composite materials on the current collector; (3) fully mixing the silicon-based material, the polymer or its precursor, and the solvent, coating the mixture on the ferroelectric / graphene composite material, drying and curing the mixture, and forming a silicon-based / polymer / ferroelectric / graphene composite material on the current collector; (4) Using laser induction technology to process silicon-based / polymer / ferroelectric / graphene composites, in situ constructing silicon-based / graphene / ferroelectric composite materials on current collectors; (5) The silicon-based / graphene / ferroelectric composite material was treated by high-voltage corona polarization.
2. The method according to claim 1, characterized in that: The ferroelectric material is selected from one or more of oxide ferroelectrics, halide ferroelectrics, chalcogenide ferroelectrics, hydrogen bond ferroelectrics, and organic ferroelectrics; Preferably, the mass ratio of the ferroelectric material, the polymer or its precursor is 1:(0.01-1000).
3. The method according to claim 1, characterized in that: The polymer is selected from one or more of polyethylene, polypropylene, polysulfide rubber, polyvinyl chloride, polyetherimide, polyetheretherketone, polyether, polyimide, polyester, polyamide, and polyurethane; Preferably, the current collector is selected from one or more of single-sided copper foil, double-sided copper foil, carbon-coated copper foil, foamed copper, carbon cloth, carbon paper, nickel foil, and foamed nickel.
4. The method according to claim 1, characterized in that: The silicon-based material is selected from one or more of silicon, silicon-carbon, silicon-oxygen, and silicon-oxygen-carbon; Preferably, the mass ratio of the silicon-based material, the polymer or its precursor is 1:(0.1-200).
5. The method according to claim 1, characterized in that: The laser is selected from one or more of solid laser, gas laser, semiconductor laser, fiber laser, pulse laser, continuous laser and excimer laser, the laser wavelength is 0.01-100 μm, the laser power is 0.1-1000 W, the scanning rate is 0.1-1000 mm / s, the scanning spacing is 0.001-10 mm, the pulse frequency is 0.01-500 kHz, the focal length is 0.1-200 cm, and the pressure range is 1-2000 kV.
6. The method according to claim 1, characterized in that: The polarization voltage of the high-voltage corona polarization is 0.01-1000 kV, the polarization time is 0.001-100 h, the polarization temperature is 5-50° C., and the distance from the tip to the current collector is 0.001-100 cm.
7. The method according to claim 1, characterized in that: The mass proportion of the ferroelectric material in the silicon-based / graphene / ferroelectric composite material is 0.1-50%; the mass proportion of the silicon-based material in the silicon-based / graphene / ferroelectric composite material is 1-90%.
8. A silicon-based / graphene / ferroelectric / current collector composite material prepared by the method according to any one of claims 1 to 7.
9. Use of the silicon-based / graphene / ferroelectric / current collector composite material according to claim 8 in lithium-ion batteries.
10. A lithium-ion battery using the silicon-based / graphene / ferroelectric / current collector composite material as claimed in claim 8 as a negative electrode.
Citation Information
Patent Citations
Doped graphene electrodes as interconnects for ferroelectric capacitors
CN107077966A
Defect-free direct dry delamination of CVD graphene using a polarized ferroelectric polymer
CN107406258A
Silicon-based / graphene / copper current collector integrated composite material and preparation and application thereof
CN117393713A
Electrode assembly, secondary battery, battery module, battery pack, and electric device
CN117652038A
Gate-Tunable Graphene-Ferroelectric Hybrid Structure for Photonics and Plasmonics
US20150155681A1
Cited By
Polarized bismuth titanate / PPy positive electrode material for enhancing polysulfide adsorption, preparation method and application of polarized bismuth titanate / PPy positive electrode material in lithium-sulfur battery
CN119786563A