Preparation method of few-layer graphene

By selecting specific graphene oxide raw materials and performing specific treatments, the problems of oligo-layer graphene preparation and dispersant residues are solved, and efficient oligo-layer graphene preparation and lithium battery performance improvement are achieved.

CN118908195AInactive Publication Date: 2024-11-08THE SIXTH ELEMENT CHANGZHOU MATERIALS TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411157171.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to accurately control and macro-preparation of oligolayer graphene in the prior art, and in common methods, the residue of dispersant will affect the high-voltage resistance of lithium-ion batteries and cannot meet the fast charging requirements.

Method used

By selecting graphene oxide raw materials with an oxygen content of 49.5-60 wt%, and a carbon content of 40-50 wt%, it is subjected to low-temperature drying, crushing, fluffing treatment and expansion heat reduction, combined with high-temperature calcination, an oligolayer graphene powder is prepared. Overcome interlayer forces and achieve efficient peeling.

Benefits of technology

The macro preparation of oligolayer graphene has been realized, which improves the conductivity and energy density and fast charging performance of lithium batteries, and meets the needs of high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908195A_ABST
    Figure CN118908195A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of few-layer graphene powder. The preparation method comprises the following steps: preparing single-layer graphene oxide; drying and crushing the graphene oxide to obtain graphene oxide powder; performing fluffy treatment on the graphene oxide powder obtained by crushing treatment to obtain fluffy graphene oxide powder; performing expansion heat treatment on the fluffy graphene oxide powder to obtain fluffy reduced graphene oxide powder; and carrying out high-temperature calcination on the fluffy reduced graphene oxide powder to obtain the few-layer graphene powder. The few-layer graphene prepared by the preparation method disclosed by the invention makes up a part of difference between the conductivity of graphene powder in the market and the conductivity of theoretical graphene, further improves the practical application value of graphene, provides favorable support for realizing high energy density and higher fast charging performance of a lithium battery, realizes macro preparation of the few-layer graphene powder, and has a wide application prospect. And the requirements of downstream application are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of thin-layer graphene materials, and in particular to a method for preparing few-layer graphene. Background Art

[0002] Graphene is a carbon atom 2 The two-dimensional structure layer formed by hybridization is honeycomb-shaped and is the basic structural unit of other carbon materials. Since its advent, it has been a research hotspot in the field of materials science due to its outstanding physical and chemical properties.

[0003] Few-layer graphene generally refers to graphene with less than 5 layers. Compared with other multi-layer graphene, few-layer graphene is thinner and more flexible, and has outstanding performance in nanoelectronic devices, composite materials, etc. Adding few-layer graphene to batteries can increase conductivity, enhance battery capacity and cycle life.

[0004] There are many methods for preparing graphene, including mechanical exfoliation, liquid phase exfoliation, chemical oxidation, crystal epitaxial growth, chemical vapor deposition, organic synthesis and carbon nanotube exfoliation.

[0005] The mechanical exfoliation method is to overcome the interaction between the sheets in the graphite by mechanical means, separate the graphite using photoresist, and successfully obtain a single layer of graphene. Although this method can produce fewer graphene layers than the general mechanical exfoliation method, it is still difficult to accurately control the purity of graphene and the yield is extremely low, making it difficult to achieve large-scale preparation of graphene. The currently commercialized mechanical exfoliation method generally uses sand mills, homogenizers and other means to break and peel the graphite. The thickness of the obtained graphene material is generally ≥10 layers, which belongs to multi-layer graphene material. It is impossible to prepare graphene with few or few layers, and a small amount of dispersant needs to be added to stabilize the graphene while these devices are breaking and peeling. The dispersant will have adverse effects during the use of downstream lithium-ion batteries, and it is impossible to achieve higher-end applications of graphene materials.

[0006] The liquid phase exfoliation method uses ultrasound, heating and other means to exfoliate graphite to prepare single-layer or multi-layer graphene solutions. This method requires the addition of a lot of dispersants in the process of preparing graphene. The dispersant has the function of stabilizing the graphene sheets in the graphene solution. However, when preparing lithium-ion batteries downstream, the dispersant on the surface of graphene as a conductive agent cannot be separated out, so that dispersants will be present in the pole pieces when the positive and negative electrodes are assembled. The presence of these dispersants will reduce the high-voltage resistance of the battery after the pole pieces are assembled into batteries. The fundamental reason is that dispersants are often some polymer or small molecule materials, which will decompose under high voltage and high current to produce gas and cause cyclic expansion and other undesirable phenomena. Therefore, it is difficult to apply to charging and discharging under high current. In the fast-paced pace of life, this type of graphene conductive agent is difficult to meet the needs of fast charging.

[0007] Chemical vapor deposition (CVD) is a method of decomposing carbon-containing chemicals (such as methane) at high temperatures. The carbon atoms obtained by the cracking are deposited on the substrate. The carbon atoms combine with carbon atoms to form graphene, which can produce a few or even a single layer of graphene materials. This method is used to prepare transparent graphene films, which can be applied to electronic touch screens, sensors, transistors, etc. The main barrier is how to peel the graphene from the base without damage or pollution, which is still a problem of concern. In addition, the CVD method is not suitable for the preparation of graphene powder materials, and the prepared graphene materials cannot be used as conductive agents in lithium-ion batteries.

[0008] Epitaxial growth, organic synthesis, and carbon tube exfoliation can all produce single-layer and few-layer graphene materials, but their cost and large-scale production are still constraints.

[0009] The redox method uses a chemical method to first oxidize and peel off graphene to obtain high-monolayer graphene oxide (GO), and then reduce GO to obtain graphene. This method is the optimal path to achieve the preparation of high-monolayer graphene powder.

[0010] There are many ways to reduce GO, but thermal reduction is the easiest method for large-scale production. Chemical reduction methods will more or less cause certain pollution, which is not conducive to the commercialization of graphene products. However, in order to obtain a few-layer or single-layer graphene material during thermal reduction, the peeling of GO during reduction is a key step. In this process, it relies on the gases released during the reduction of oxygen-containing functional groups in GO, mainly including H2O, CO2, CO, etc. The faster the release rate of these gases, the higher the peeling degree of the sheets, and the higher the corresponding single-layer rate. The rate of gas release directly affects the air pressure between layers. When the air pressure is much greater than the external air pressure, the van der Waals interaction between the layers can be overcome, thereby achieving the purpose of effective peeling. From this perspective, the main factors affecting the number of layers of reduced graphene oxide (rGO) are: 1) the monolayer rate and functional group content of the raw material GO, that is, the higher the monolayer rate of GO and the more oxygen-containing functional groups, the fewer rGO layers can be prepared; 2) the influence of external pressure, which can be decomposed into the reduction conditions and the density of the dry GO itself. The denser the GO particles, the more difficult it is to release gas and the more difficult it is to peel them off. Summary of the invention

[0011] In order to solve the above problems, the present invention provides a method for preparing a few-layer graphene, comprising the following steps:

[0012] A method for preparing a few-layer graphene powder, characterized in that it comprises the following steps:

[0013] S1: preparing graphene oxide, wherein the graphene oxide satisfies the following conditions:

[0014] Under the test method of T / CSTM 00003-2019, the thickness of graphene oxide dispersion measured under atomic force microscopy is ≤1.2nm;

[0015] S2: drying and crushing the graphene oxide in step S1 to obtain graphene oxide powder;

[0016] S3: Fluffing the graphene oxide powder in step S2 to obtain fluffy graphene oxide powder;

[0017] S4: performing expansion heat treatment on the fluffy graphene oxide powder obtained in step S3 to obtain reduced graphene oxide powder;

[0018] S5: calcining the reduced graphene oxide powder obtained in step S4 at high temperature to obtain a few-layer graphene powder.

[0019] Preferably, in step S1, the oxygen content of the graphene oxide is 49.5-60wt%, and the carbon content is 40-50wt%; further preferably, the oxygen content of the graphene oxide is 49.5-55wt%, and the carbon content is 45-50wt%.

[0020] Preferably, the graphene oxide has a single layer.

[0021] Preferably, in step S2, the drying temperature is 30-65°C, and the drying time is 4-24 hours; further preferably, the drying temperature is 45-65°C, and the drying time is 8-20 hours.

[0022] Preferably, the water content of the dried graphene oxide is ≤5wt%.

[0023] Preferably, in step S2, the particle size of the graphene oxide powder obtained by the pulverization treatment is 60-250 mesh; more preferably 100-150 mesh.

[0024] Preferably, in step S3, the fluffing treatment is performed by placing the graphene oxide powder obtained in step S2 into a sealed container and stirring.

[0025] Preferably, the stirring speed is 500-2000 rpm; further preferably, the stirring speed is 1000-2000 rpm.

[0026] Preferably, the stirring time is 30 to 60 min; further preferably, the stirring time is 40 to 60 min.

[0027] Preferably, the tap density of the fluffy graphene oxide powder is 0.1-0.6 g / cm 3 .

[0028] Preferably, in step S4, the expansion heat treatment is performed by:

[0029] The fluffy graphene oxide powder obtained in step S3 is directly placed in a hot environment for explosive reduction to obtain reduced graphene oxide powder.

[0030] Preferably, the temperature of the expansion heat treatment is 200-400°C; further preferably, the temperature is 280-380°C.

[0031] Preferably, the expansion heat treatment time is 10-40 min40 min; further preferably, the time is 15-25 min.

[0032] Preferably, the tap density of the reduced graphene oxide powder is 0.005-0.09 g / cm 3, more preferably 0.008-0.05g / cm 3 .

[0033] Preferably, the expansion heat treatment environment is an inert environment.

[0034] Preferably, the gas of the inert environment is nitrogen.

[0035] Preferably, in step S5, the temperature of the high temperature calcination is 1000-1500°C, and the calcination time is 1-6h; further preferably, the temperature of the high temperature calcination is 1000-1300°C, and the calcination time is 2-4h.

[0036] Preferably, in step S5, the high-temperature calcination environment is an inert environment.

[0037] A second aspect of the present invention provides a few-layer graphene powder prepared by the above-mentioned preparation method; preferably, the number of layers of the graphene powder is ≤5.

[0038] The working principle of the present invention is as follows: first, the raw material GO is selected, and a single-layer GO with an oxygen content of 49.5-60wt% and a carbon content of 40-50wt% is selected to ensure that a sufficient amount of gas is released in the subsequent reduction step; then, the GO is dried at low temperature and crushed to obtain powder particles with a certain particle size; then the GO particles are stirred at high speed and fluffed, thereby reducing the tap density of the GO powder, so as to reduce the external pressure of the gas released during heat treatment, and achieve the effect of overcoming the force between layers; and then during thermal reduction, the gas released by the instantaneous heat exchange of GO is used to overcome the stacking effect caused by the π-π force, thereby promoting good rGO peeling; finally, the rGO is directly repaired at high temperature to obtain a powder material of a few-layer graphene. In the above process, by selecting single-layer GO, controlling the particle size of GO powder, fluffing the GO powder and performing expansion heat treatment, the rGO powder before high-temperature repair can achieve a thin layer effect, and then a few-layer graphene powder is prepared by high-temperature repair, thereby realizing the large-scale preparation of few-layer graphene powder to meet the requirements of downstream applications.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The development of few-layer graphene powder materials has partially filled the gap between the conductivity of graphene powder on the market and theoretical graphene, further enhancing the practical application value of graphene;

[0041] (2) It provides favorable support for lithium batteries to achieve high energy density and faster charging performance;

[0042] (3) Realize the large-scale preparation of few-layer graphene powder to meet the requirements of downstream applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0044] Figure 1 It is a schematic diagram of the preparation method of the few-layer graphene provided by the present invention;

[0045] Figure 2 is an atomic force microscope image of the raw material GO in an embodiment of the present invention;

[0046] Figure 3 is a transmission electron microscope image of a few-layer graphene obtained by the preparation method of an embodiment of the present invention;

[0047] Figure 4 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Example 1 of the present invention;

[0048] Figure 5 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Example 2 of the present invention;

[0049] Figure 6 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Example 3 of the present invention;

[0050] Figure 7 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Example 4 of the present invention;

[0051] Figure 8 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Example 5 of the present invention;

[0052] Fig. 9 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Comparative Example 1 of the present invention;

[0053] Fig.10 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Comparative Example 2 of the present invention;

[0054] Fig.11 is a scanning electron microscope image of a few-layer graphene obtained according to the preparation method of Comparative Example 3 of the present invention;

[0055] Fig.12 3 is a scanning electron microscope image of the few-layer graphene obtained by the preparation method of Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0056] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0057] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0058] This article relates to numerical ranges. Unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0059] The temperature parameters herein, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.

[0060] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0061] like Figure 1 It is a schematic diagram of the method for preparing few-layer graphene provided by the present invention.

[0062] The present invention provides a method for preparing a few-layer graphene, comprising the following steps:

[0063] (1) Selection of raw material GO.

[0064] The present invention selects a single-layer GO raw material with an oxygen content of 49.5-60wt% and a carbon content of 40-50wt%. Preferably, the oxygen content of graphene oxide is 49.5-55wt%, and the carbon content is 45-50wt%.

[0065] When the oxygen content is <49.5wt%, the amount of gas generated during thermal reduction is small, and it is impossible to overcome the interlayer force and obtain a few-layer rGO material; when the oxygen content is >60wt%, there are many defects caused after reduction, which is not conducive to the repair of rGO in the high-temperature section.

[0066] When the C content is <40wt%, GO has more oxygen-containing groups, and more defects are caused after reduction, which is not conducive to the repair of rGO in the high-temperature section; when the C content is >50wt%, GO has fewer oxygen-containing groups, which is not conducive to the explosion of GO powder in the thermal reduction stage, resulting in thicker layers of rGO.

[0067] Therefore, a single-layer GO raw material with a C content of 40–50% and an O content of 49.5–60% was selected.

[0068] The selection of the above raw materials is to ensure that GO can release a sufficient amount of gas during thermal reduction. It is necessary to have a large number of oxygen-containing functional groups on GO and to ensure that GO is in a single-layer state. Based on this, the oxidation effect of GO itself needs to be relatively good.

[0069] In order to meet the requirements of oxygen-containing functional groups of GO, the oxygen content is used to evaluate the relative functional groups. In the present invention, the C and O contents in GO are tested by elemental analysis.

[0070] In order to confirm that the selected raw material GO is a single layer, the raw material can be tested by atomic force microscopy. The test results are as follows Figure 2 As shown, the AFM test method reference: T / CSTM 00003-2019. Under this test method, when the thickness of the GO sheet in the GO dispersion is ≤1.2nm, it can be determined to be in a single-layer state. As can be seen from the figure, the raw material GO is basically in a single-layer state. This shows that the raw material GO is very easy to disperse into a single layer.

[0071] In the present invention, the number of layers of the raw material GO refers to the number of layers of GO when the raw material is dispersed into a dispersion under the test method of T / CSTM 00003-2019.

[0072] (2) Preparation of GO powder.

[0073] The GO is dried at low temperature, the drying temperature is 30°C-65°C, the drying time is 4-24h, preferably the drying temperature is 45-65°C, the drying time is 8-20h, so that the moisture content of the GO after drying is ≤5wt%, and then the dried GO is crushed to 60-250 mesh, preferably 100-150 mesh. The crushing can be carried out by a paddle blade, a jet mill, a grinding disc mill, etc., which are not limited here.

[0074] If the moisture content of GO is too high, it will easily stick to the blade during crushing, which will not only cause corrosion of the blade and introduce metal impurities into the GO powder, but also cause uneven particles due to sticking problems. Therefore, the moisture content of GO after drying is ≤5wt%.

[0075] Since GO itself has poor thermal stability, the drying temperature here should not be too high. If the temperature is lower than 30°C, the drying time will be too long and the efficiency will be low; if the temperature is too high, the oxygen-containing functional groups will be easily decomposed.

[0076] The drying time is 4-24h. If the drying time is too short, the drying effect cannot be achieved and GO with a water content of ≤5wt% cannot be obtained. If the drying time is too long, the production efficiency will be reduced, resources will be wasted, and GO may be over-dried, resulting in folding (single-layer GO becomes multi-layer GO).

[0077] For the size of GO particles, if the mesh number of GO particles is too high or too low, few-layer graphene materials cannot be obtained. When the mesh number of the particles is too low, that is, the GO particles are too large, the external pressure is too high, and the gas pressure released during thermal reduction is less than the external pressure, resulting in failure to completely peel off; when the mesh number of the particles is too high, that is, the GO particles are too small, the overall gas release is small, the volume generated by instantaneous thermal expansion is too small, and the pressure generated is less than the external air pressure, and it is also impossible to completely peel off.

[0078] (3) Fluffy GO powder.

[0079] In order to reduce the density of GO powder and prepare fluffy GO powder, the GO powder is stirred at high speed in a closed container, the stirring speed is 500-2000 rpm, the stirring time is 30-60 min, preferably, the stirring speed is 1000-2000 rpm, the stirring time is 40-60 min, and refluxes up and down at the same time.

[0080] Here, the stirring device in patent CN213611236U can be applied to stir the GO powder by utilizing the principle of stirring convection to perform fluffy treatment, thereby reducing the tap density of the GO powder and reducing the external pressure of the gas released during heat treatment, thereby achieving the effect of overcoming the force between layers, thereby realizing the preparation of few-layer graphene materials.

[0081] The tap density of GO powder before fluffing treatment is 0.6-1.3g / cm 3 The tap density of GO powder after fluffing treatment is 0.1-0.6g / cm 3 This shows that the fluffing treatment of GO powder reduces the density of GO powder, making it easier to overcome the interaction between GO layers during the subsequent thermal reduction of GO expansion, laying the foundation for the subsequent preparation of few-layer graphene.

[0082] Tap density refers to the mass per unit volume of powder in a container measured after being tapped under specified conditions.

[0083] (4) Expansion thermal reduction of fluffy GO powder.

[0084] Place a heat-conducting vessel (not sealed) in an oven, introduce nitrogen to make the overall atmosphere in the oven inert, and raise the oven temperature to 200-400°C, preferably 280-380°C. Take a small amount of the above-mentioned fluffy GO powder, pour the fluffy GO powder into the nitrogen-protected heat-conducting vessel through the feed port, and heat treat for 10-40 minutes, preferably 15-25 minutes, to obtain fluffy rGO black powder. At this time, the tap density of the fluffy rGO black powder is 0.005-0.09g / cm 3 , preferably 0.008-0.05g / cm 3 .

[0085] The fluffy GO powder is thermally reduced. In order to fully exfoliate GO, the GO powder needs to be directly exposed to an environment of 200-400°C to avoid a slow heating process, thereby achieving an instantaneous explosion. The large amount of gas released reduces and exfoliates the GO dry aggregate (i.e., fluffy GO powder) to obtain rGO powder. In the present invention, the fluffy GO powder is instantly placed in a high-temperature environment, and GO explodes instantly and is reduced to rGO powder. Since GO powder is thermally reduced to rGO, its volume will expand 100 to 1000 times. Therefore, the amount of GO powder can be controlled according to the size of the volume expansion to reduce the risk of explosion due to volume expansion.

[0086] In the present invention, the thermal reduction temperature is between 200 and 400° C. Within this temperature range, most of the oxygen-containing groups such as hydroxyl, carboxyl, epoxy, carbonyl, etc. can fall off. When the temperature is lower than 200° C., some oxygen-containing groups cannot fall off. When the temperature is higher than 400° C., the H2O molecules generated by thermal reduction and shedding are prone to react with C on the graphene to produce water gas, resulting in more defects in the graphene surface.

[0087] In the present invention, the thermal reduction time is 10-40 minutes. Within this time range, the GO powder can fully absorb heat, so that its oxygen-containing groups can be more completely detached, and the production efficiency can be improved as much as possible. When the thermal reduction time is less than 10 minutes, the functional groups may not be completely detached; when the thermal reduction time is greater than 40 minutes, the production efficiency of the entire process section is affected, resulting in a waste of resources.

[0088] (5) The rGO powder is subjected to high temperature repair to obtain a powder of a few-layer graphene.

[0089] The rGO powder is placed in a high temperature furnace in an inert environment for calcination treatment, the temperature is raised to 1000-1500°C at a heating rate of 10°C / min, and the heat treatment is performed for 1-6 hours to obtain a powder material of a few-layer graphene. Preferably, the high temperature calcination temperature is 1000-1300°C and the calcination time is 2-4 hours. Figure 3 shown.

[0090] Since the shedding of oxygen-containing groups causes defects in rGO, within this temperature range, rGO repairs defects and improves performance. When the temperature is below 1000°C, the oxygen-containing functional groups on the surface of rGO are not completely removed, and its conductivity will be poor; when the temperature is above 1500°C, a rearrangement reaction of C atoms will occur, and a two-dimensional graphene sheet structure with a complete lattice will be repaired, which will cause overlap between graphene sheets (due to π-π forces).

[0091] The few-layer graphene powder prepared by the above preparation method was tested, and the test method was as follows:

[0092] The test method for the mass fraction of C element and O element is: DB32 / T 3595-2019 Elemental analyzer method for determination of carbon, hydrogen, nitrogen, sulfur and oxygen content in graphene materials.

[0093] The test method for ID / IG is: Q / NGSIC 012-2020.

[0094] The test method for specific surface area (BET) is: refer to GBT 7702.20-1997 Test method for pore volume of coal-based granular activated carbon.

[0095] The test method for oil absorption value is: refer to GBT 3780.2-2007 Carbon black Part 2: Determination of oil absorption value.

[0096] The conductivity test method is: Sasha Stankovich, Dmitriy A. Dikin, et al., Synthesis of graphene-based nanosheets via chemical reduction of exfoliated graphite oxide, Carbon 45 (2007): [lines 1558-1565]. The conductivity of the few-layer graphene powder was tested by the method in this document.

[0097] The test results are shown in Table 1.

[0098] Table 1 Performance data of the few-layer graphene powder prepared by the preparation method of the present invention

[0099]

[0100] From the data in Table 1, we can see that C (wt%) ≥ 98.5%, O (wt%) ≤ 0.1%, indicating that the GO raw material is basically reduced to generate graphene; ID / IG ≤ 1.03, the smaller the ID / IG value means the fewer defects in the graphene material, so its conductivity will be higher; BET ≥ 750m 2 / g shows that the specific surface area of ​​graphene prepared by this method is relatively large. At the same time, according to the theoretical specific surface area of ​​graphene, when the specific surface area is 750m 2 / g, the average number of graphene layers is about 3. This shows that the BET of graphene powder is ≥750m 2 / g is a few-layer graphene; the oil absorption value is between 4500 and 6870 ml / 100 g, indicating that the few-layer graphene has good lipophilicity and is easy to disperse in the solvent; the conductivity range is 10 5 ~10 7 S / m shows that few-layer graphene has good high conductivity.

[0101] The present invention is further described below in conjunction with specific embodiments.

[0102] Embodiment 1:

[0103] A method for preparing a few-layer graphene:

[0104] Take the GO with a single layer and an oxygen content of 49.5wt% and a carbon content of 47.2wt%, and dry it in a 30℃ forced air drying oven for 24 hours. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.73g / cc. The GO powder in this particle size range is placed in a high-speed mixer, stirred for 60 minutes at a speed of 500rpm and a temperature of ≤30℃, and the tap density of the powder is tested to be 0.44g / cm 3 .

[0105] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole in an inert atmosphere, and heat it to 200°C. Pour GO powder into the heat-conducting vessel from the feed port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 40 minutes to obtain fluffy rGO powder.

[0106] The fluffy rGO powder is placed in a high-temperature furnace, nitrogen is introduced to make the high-temperature furnace an inert environment, and the temperature is raised to 1000°C at a heating rate of 10°C / min and kept at this temperature for 6 hours to obtain a few-layer graphene powder, such as Figure 4 The performance of the few-layer graphene powder was tested, see Table 2.

[0107] Embodiment 2:

[0108] A method for preparing a few-layer graphene:

[0109] Take the GO with a single layer and an oxygen content of 52.9wt% and a carbon content of 44.5wt%, and dry it in a 65℃ forced air drying oven for 10 hours. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.7g / cc. The GO powder in this particle size range is placed in a high-speed mixer, stirred for 60 minutes at a speed of 1500rpm and a temperature of ≤30℃, and the tap density of the powder is tested to be 0.46g / cm 3 .

[0110] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole in an inert atmosphere, and heat it to 280°C. Pour GO powder into the heat-conducting vessel from the feed port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 25min to obtain fluffy rGO powder.

[0111] The fluffy rGO powder was placed in a high-temperature furnace, nitrogen was introduced to make the high-temperature furnace an inert environment, and the temperature was raised to 1100°C at a heating rate of 10°C / min and kept at this temperature for 4.5h to obtain a few-layer graphene powder, such as Figure 5 The performance of the few-layer graphene powder was tested, see Table 2.

[0112] Embodiment 3:

[0113] A method for preparing a few-layer graphene:

[0114] Take the GO with a single layer and an oxygen content of 56.2wt% and a carbon content of 41.8wt%, and dry it in a 50℃ forced air drying oven for 18h. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size of 60 to 250 mesh is screened out. The tap density is tested to be 0.67g / cc. The GO powder with this particle size range is placed in a high-speed mixer, stirred for 30 minutes at a speed of 1800rpm and a temperature of ≤30℃, and the tap density of the powder is tested to be 0.48g / cm 3 .

[0115] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole in an inert atmosphere, and heat it to 320°C. Pour GO powder into the heat-conducting vessel from the feed port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 20 minutes to obtain fluffy rGO powder.

[0116] The fluffy rGO powder is placed in a high-temperature furnace, nitrogen is introduced to make the high-temperature furnace an inert environment, and the temperature is raised to 1200°C at a heating rate of 10°C / min and kept at this temperature for 3 hours to obtain a few-layer graphene powder, such as Figure 6The performance of the few-layer graphene powder was tested, see Table 2.

[0117] Embodiment 4:

[0118] A method for preparing a few-layer graphene:

[0119] Take the GO with a single layer and an oxygen content of 57.8wt% and a carbon content of 40.1wt%, and dry it in a 60℃ forced air drying oven for 14h. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.79g / cc. The GO powder in this particle size range is placed in a high-speed mixer, stirred for 30 minutes at a speed of 2000rpm and a temperature of ≤30℃, and the tap density of the powder is tested to be 0.39g / cm 3 .

[0120] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole inert atmosphere, and heat it to 350°C. Pour GO powder into the heat-conducting vessel from the feeding port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 18 minutes to obtain fluffy rGO powder.

[0121] The fluffy rGO powder was placed in a high-temperature furnace, nitrogen was introduced to make the high-temperature furnace an inert environment, and the temperature was raised to 1300°C at a heating rate of 10°C / min and kept at this temperature for 2.5h to obtain a few-layer graphene powder, such as Figure 7 The performance of the few-layer graphene powder was tested, see Table 2.

[0122] Embodiment 5:

[0123] A method for preparing a few-layer graphene:

[0124] Take the GO with a single layer and an oxygen content of 59.7wt% and a carbon content of 40.1wt%, and dry it in a 65℃ forced air drying oven for 10 hours. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.68g / cc. The GO powder in this particle size range is placed in a high-speed mixer, stirred for 30 minutes at a speed of 2000rpm and a temperature of ≤30℃, and the tap density of the powder is tested to be 0.33g / cm 3 .

[0125] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole in an inert atmosphere, and heat it to 400°C. Pour GO powder into the heat-conducting vessel from the feed port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 10 minutes to obtain fluffy rGO powder.

[0126] The fluffy rGO powder is placed in a high-temperature furnace, nitrogen is introduced to make the high-temperature furnace an inert environment, and the temperature is raised to 1500°C at a heating rate of 10°C / min and kept at this temperature for 1h to obtain a few-layer graphene powder, such as Figure 8 The performance of the few-layer graphene powder was tested, see Table 2.

[0127] Comparative Example 1:

[0128] A method for preparing graphene powder:

[0129] Take GO with more than 2 test layers, an oxygen content of 50.8wt%, and a carbon content of 47.1wt%, and dry it in a 60℃ forced air drying oven for 14 hours. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.88g / cc. The GO powder in this particle size range is placed in a high-speed mixer, stirred for 30 minutes at a speed of 2000rpm and a temperature of ≤30℃, and the tap density of the tested powder is 0.53g / cm 3 .

[0130] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole inert atmosphere, and heat it to 350°C. Pour GO powder into the heat-conducting vessel from the feeding port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 18 minutes to obtain fluffy rGO powder.

[0131] The fluffy rGO powder is placed in a high-temperature furnace, nitrogen is introduced to make the high-temperature furnace an inert environment, and the temperature is increased to 1200°C at a heating rate of 10°C / min and kept at this temperature for 3 hours to obtain graphene powder. Fig. 9 The performance of graphene powder was tested, see Table 2.

[0132] Comparative Example 2:

[0133] A method for preparing graphene powder:

[0134] Take the GO with a single layer and an oxygen content of 57.8wt% and a carbon content of 40.1wt%, and dry it in a 60℃ forced air drying oven for 14h. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.79g / cm 3 .

[0135] First, place a heat-conducting container (not sealed) into an oven, pass nitrogen into the oven to make the entire oven in an inert atmosphere, raise the temperature to 350°C, pour GO powder into the heat-conducting container from the feeding port, where the mass of GO is 10g and the volume of the container is ≥10L. Perform thermal reduction treatment for 18 minutes to obtain fluffy rGO powder.

[0136] The fluffy rGO powder is placed in a high-temperature furnace, nitrogen is introduced to make the high-temperature furnace an inert environment, and the temperature is increased to 1200°C at a heating rate of 10°C / min and kept at this temperature for 3 hours to obtain graphene powder. Fig.10 The performance of graphene powder was tested, see Table 2.

[0137] Comparative Example 3

[0138] A method for preparing graphene powder:

[0139] Take the GO with a single layer and an oxygen content of 45.2wt% and a carbon content of 54.2wt%, and dry it in a 60℃ forced air drying oven for 14h. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size of 60 to 250 mesh is screened out. The tap density is tested to be 0.86g / cc. The GO powder with this particle size range is placed in a high-speed mixer, stirred for 30 minutes at a speed of 2000rpm and a temperature of ≤30℃, and the tap density of the powder is tested to be 0.39g / cm 3 .

[0140] First, place a heat-conducting vessel (not sealed) in an oven, pass nitrogen into the oven to make the oven as a whole inert atmosphere, and heat it to 350°C. Pour GO powder into the heat-conducting vessel from the feeding port, where the mass of GO is 10g and the volume of the vessel is ≥10L. Heat reduction treatment is performed for 18 minutes to obtain fluffy rGO powder.

[0141] The fluffy rGO powder is placed in a high-temperature furnace, nitrogen is introduced to make the high-temperature furnace an inert environment, and the temperature is increased to 1200°C at a heating rate of 10°C / min and kept at this temperature for 3 hours to obtain graphene powder. Fig.11 The performance of graphene powder was tested, see Table 2.

[0142] Comparative Example 4

[0143] A method for preparing graphene powder:

[0144] Take the GO with a single layer and an oxygen content of 57.8wt% and a carbon content of 40.1wt%, and dry it in a 60℃ forced air drying oven for 14h. The dried GO is placed in a crusher for crushing, and the GO powder with a particle size in the range of 60 to 250 mesh is screened out. The tap density is tested to be 0.79g / cm 3The GO powder of this particle size range was placed in a high-speed mixer and stirred for 30 minutes at a speed of 2000 rpm and a temperature of ≤30°C. The tap density of the powder was tested to be 0.39 g / cc.

[0145] The fluffy GO powder was placed in an oven, nitrogen was introduced to make the oven an inert environment, the temperature was raised to 350°C at a heating rate of 5°C / min and kept for 18 minutes to obtain rGO powder.

[0146] The rGO powder was placed in a high-temperature furnace, nitrogen was introduced to make the high-temperature furnace an inert environment, the temperature was raised to 1200°C at a heating rate of 10°C / min, and the temperature was kept for 3 hours to obtain graphene powder. Fig.12 The performance of graphene powder was tested, see Table 2.

[0147] Table 2 Performance data of few-layer graphene prepared in Examples and Comparative Examples

[0148]

[0149] It can be seen from the data in Table 2 that the graphene prepared by Examples 1-5 all meet the performance range of few-layer graphene, that is, C (wt%) ≥ 98.5%, O (wt%) ≤ 0.1%; ID / IG ≤ 1.03; BET ≥ 750m 2 / g; oil absorption value is 4500~6870ml / 100g; conductivity range is 10 5 ~10 7 S / m.

[0150] The GO selected in Comparative Example 1 is multi-layer. Although the C and O contents and ID / IG meet the performance range of few-layer graphene, the BET, oil absorption value and conductivity do not meet the requirements of few-layer graphene. The multi-layer GO itself cannot be further stripped into a few layers. At the same time, the multi-layer GO tends to be easier to fold back during thermal reduction, resulting in a large number of rGO layers, which cannot be used to prepare few-layer graphene.

[0151] In Comparative Example 2, the high-speed stirring process was not performed, and the tap density of the GO powder was relatively high. The external pressure released by the gas during the heat treatment could not overcome the force between the layers, so that the preparation of the few-layer graphene material could not be achieved, and the performance requirements of the few-layer graphene could not be met.

[0152] The GO selected in Comparative Example 3 has a lower oxygen content and produces less gas during thermal reduction, which cannot overcome the interlayer force and thus cannot obtain a few-layer rGO material, nor can it meet the performance requirements of few-layer graphene.

[0153] In Comparative Example 4, no thermal expansion was performed, and the temperature was directly and slowly raised to 1200°C. When the temperature reached about 200°C, the glass window could see a relatively weak volume expansion. Since the functional groups were slowly released as the temperature slowly increased, there was no obvious increase in the specific surface area, and it could only reach 357m 2 / g, and it is impossible to prepare graphene materials with good conductivity and few layers.

[0154] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0155] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a few-layer graphene powder, characterized in that: The steps include: S1: Prepare graphene oxide, wherein the graphene oxide satisfies the following conditions: Under the T / CSTM 00003-2019 test method, the thickness of graphene oxide in the graphene oxide dispersion under atomic force microscopy is ≤1.2nm; S2: drying, crushing and sieving the graphene oxide in step S1 to obtain graphene oxide powder; S3: Fluffing the graphene oxide powder in step S2 to obtain fluffy graphene oxide powder; S4: performing expansion heat treatment on the fluffy graphene oxide powder obtained in step S3 to obtain reduced graphene oxide powder; S5: calcining the reduced graphene oxide powder obtained in step S4 at high temperature to obtain a few-layer graphene powder.

2. The preparation method according to claim 1, characterized in that: In step S1, the oxygen content of the graphene oxide is 49.5-60wt%, and the carbon content is 40-50wt%; Preferably, the graphene oxide has an oxygen content of 49.5-55wt% and a carbon content of 45-50wt%; Preferably, the graphene oxide has a single layer.

3. The preparation method according to claim 1, characterized in that: In step S2, the drying temperature is 30-65°C and the drying time is 4-24h; Preferably, the drying temperature is 45-65°C and the drying time is 8-20h; Preferably, the water content of the dried graphene oxide is ≤5wt%; Preferably, the particle size of the graphene oxide powder obtained by the crushing and sieving treatment is 60-250 mesh; more preferably 100-150 mesh.

4. The preparation method according to claim 1, characterized in that: In step S3, the fluffing treatment is performed by placing the graphene oxide powder obtained in step S2 into a sealed container and stirring; Preferably, the stirring speed is 500-2000 rpm; further preferably, the stirring speed is 1000-2000 rpm; Preferably, the stirring time is 30 to 60 minutes; further preferably, the stirring time is 40 to 60 minutes; Preferably, the tap density of the fluffy graphene oxide powder is 0.1-0.6 g / cm 3 .

5. The preparation method according to claim 1, characterized in that: In step S4, the expansion heat treatment is performed as follows: The fluffy graphene oxide powder obtained in step S3 is directly placed in a hot environment for explosive reduction to obtain reduced graphene oxide powder; Preferably, the temperature of the expansion heat treatment is 200-400°C; further preferably, the temperature is 280-380°C; Preferably, the expansion heat treatment time is 10-40 minutes; more preferably, the time is 15-25 minutes; Preferably, the tap density of the reduced graphene oxide powder is 0.005-0.09 g / cm 3 ; More preferably 0.008-0.05g / cm 3 ; Preferably, the expansion heat treatment environment is an inert environment; Preferably, the gas of the inert environment is nitrogen.

6. The preparation method according to claim 1, characterized in that: In step S5, the high temperature calcination temperature is 1000-1500°C, and the calcination time is 1-6h; further preferably, the high temperature calcination temperature is 1000-1300°C, and the calcination time is 2-4h; Preferably, in step S5, the high-temperature calcination environment is an inert environment.

7. A graphene powder, characterized in that: Prepared by any preparation method of claims 1-6; preferably, the number of layers of the graphene powder is ≤5.

Citation Information

Patent Citations

  • Mixing granulation equipment

    CN213611236U

  • Preparing method of oxidized graphene and high-conductivity graphene

    CN106564891A

  • Small-sized single layer graphene and preparation method thereof

    CN109607520A

  • High-quality graphene, heat-conducting and electric-conducting epoxy resin composite material thereof and preparation method thereof

    CN110615970A

  • Preparation method of reduced graphene oxide and graphene heat-conducting film

    CN113277503A