Conductive polymer coated graphite negative electrode material as well as preparation method and application thereof
By forming a conductive polymer cladding layer on the surface of the graphite negative electrode material and calcining under an inert atmosphere, the problems of sulfide electrolyte decomposition and high resistance are solved, the efficiency and stability of sulfide solid-state batteries are improved, and high first-term efficiency and Long cycle life.
Patent Information
- Application Number
- CN202410891229.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing graphite negative electrode materials have decomposed sulfide electrolytes due to the low lithium embedded potential in sulfide electrolytes. The first time Coulomb efficiency is low, and traditional clad materials have limited effects on reducing resistance and improving interface stability.
The liquid phase coating method is used to form a conductive polymer coating layer on the graphite surface and calcined under an inert atmosphere to reduce the contact resistance between the electrolyte and graphite, improve the transmission efficiency of lithium ions and electrons, and remove oxygen and the surface of the material. Moisture to improve battery stability.
The first-time Coulomb efficiency and cycle life of sulfide solid-state batteries are improved, ensuring the high discharge capacity and stability of the battery at large magnification. The first-time discharge specific capacity can reach 369.8-381.86mAh/g, and the first-time Coulomb efficiency can reach 89.42-93.71%.
Smart Images

Figure CN118908200A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a conductive polymer-coated graphite negative electrode material and a preparation method and application thereof. Background Art
[0002] Solid-state batteries have become one of the most promising candidate batteries for the next generation due to their ultra-high energy density and safety. Sulfide electrolytes have become a research hotspot due to their ultra-high ionic conductivity and good cold pressing properties. Graphite, as the most successful commercial negative electrode material, will decompose on its surface due to its low lithium insertion potential in sulfide electrolytes, resulting in a low first coulombic efficiency in the first cycle. In order to overcome this problem, the method of coating graphite is usually used to form a protective film on its surface to play a protective role.
[0003] At present, the methods of graphite coating mainly include physical coating and chemical coating. Physical coating is to form a physical protective layer on the surface of graphite by mechanically mixing graphite with coating materials; chemical coating is to form a chemical protective layer on the surface of graphite. As graphite coating materials, metal oxides, metal phosphates, etc. have good performance and stability and are widely used in graphite coating. However, these coating materials have limited effects on reducing the resistance between graphite and sulfide electrolytes, promoting the transmission of lithium ions and electrons, and improving interface stability. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a conductive polymer-coated graphite negative electrode material and a preparation method and application thereof. The surface of the graphite negative electrode material described in the present invention has a conductive polymer coating layer, which can reduce the contact resistance between graphite and sulfide electrolyte, promote the transmission of lithium ions and electrons, and improve the first coulomb efficiency; at the same time, the coating layer has a good improvement effect on the interface stability between sulfide and graphite, which is conducive to the realization of sulfide solid-state batteries with high first efficiency and long cycle life.
[0005] The inventive concept of the present invention is as follows: the present invention adopts a liquid phase coating method to coat a conductive polymer layer on the surface of graphite, and calcines it in an inert atmosphere. The obtained coating layer can effectively reduce the contact resistance between the electrolyte and the graphite, and improve the first coulombic efficiency of the battery; and can protect the graphite when the battery is charged and discharged at a high rate, maintain the integrity of the electrode, and ensure the high discharge capacity of the battery at a high rate; and its own conductivity provides a conductive channel for the graphite negative electrode during the first lithium insertion process, reducing the irreversible capacity of the first cycle, thereby improving the first coulombic efficiency. At the same time, calcination in an inert atmosphere can effectively remove oxygen and moisture on the surface of the material, avoid its adverse effects on the subsequent assembly of the battery, and further improve the stability of the sulfide solid-state battery.
[0006] In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing a graphite negative electrode material, comprising the following steps:
[0007] (1) adding graphite to a conductive polymer solution and mixing to obtain a suspension;
[0008] (2) subjecting the suspension to solid-liquid separation to obtain a solid product;
[0009] (3) After drying the solid product, calcining it in an inert atmosphere to obtain a graphite negative electrode material coated with a conductive polymer.
[0010] Preferably, the conductive polymer solution comprises a polyaniline solution.
[0011] Preferably, the solvent of the polyaniline solution is water or anhydrous ethanol.
[0012] Preferably, the concentration of the conductive polymer solution is 0.05-0.5 g / mL.
[0013] Further preferably, the concentration of the conductive polymer solution is 0.1-0.5 g / mL.
[0014] Preferably, the graphite is selected from natural graphite and / or mesocarbon microbeads.
[0015] Further preferably, the graphite is selected from mesocarbon microbeads.
[0016] Preferably, in the suspension, the mass ratio of the graphite to the conductive polymer is 100:(0.5-5).
[0017] Further preferably, in the suspension, the mass ratio of the graphite to the conductive polymer is 100:(1-5).
[0018] Preferably, in step (1), the mixing is carried out by stirring at a rotation speed of 300-600 rpm for 3-8 hours.
[0019] Further preferably, in step (1), the mixing is performed by stirring at a rotation speed of 350-450 rpm for 3-4 hours.
[0020] Preferably, in step (3), the drying is carried out under a vacuum environment for 10-15 hours.
[0021] Further preferably, in step (3), the drying is performed under a vacuum environment for 11-13 hours.
[0022] Preferably, in step (3), the calcination temperature is 280-350°C.
[0023] Further preferably, in step (3), the calcination temperature is 280-320°C.
[0024] Preferably, in step (3), the calcination time is 2-4 hours.
[0025] More preferably, in step (3), the calcination time is 2.5-3.5 hours.
[0026] Preferably, in step (3), the inert atmosphere is a nitrogen atmosphere.
[0027] The second aspect of the present invention provides a graphite negative electrode material, which is prepared by the method for preparing the graphite negative electrode material described in the first aspect of the present invention.
[0028] The third aspect of the present invention provides a sulfide solid-state battery, comprising a negative electrode, wherein the negative electrode comprises the graphite negative electrode material described in the second aspect of the present invention.
[0029] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:
[0030] When preparing the graphite negative electrode material of the present invention, a liquid phase coating method is adopted to coat a conductive polymer layer on the surface of the graphite. The coating layer can effectively reduce the contact resistance between the electrolyte and the graphite, and improve the first coulombic efficiency of the battery; and can protect the graphite when the battery is charged and discharged at a high rate, maintain the integrity of the electrode, and ensure the high discharge capacity of the battery at a high rate; and its own conductivity provides a conductive channel for the graphite negative electrode during the first lithium insertion process, reduces the irreversible capacity of the first cycle, and thus improves the first coulombic efficiency. At the same time, the present invention also calcines the coating layer under an inert atmosphere, which can effectively remove oxygen and moisture on the surface of the material, avoid its adverse effects on the subsequent assembly of the battery, and further improve the stability of the sulfide solid-state battery. When the graphite negative electrode material prepared by the present invention is applied to a sulfide solid-state battery, the first discharge specific capacity can reach 369.8-381.86mAh / g, and the first coulombic efficiency can reach 89.42-93.71%. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 FTIR image of the graphite negative electrode material prepared in Example 1;
[0032] Figure 2 is a specific capacity-voltage diagram of a sulfide solid-state battery assembled from graphite of Comparative Example 1 at 0.1C;
[0033] Figure 3 This is the specific capacity-voltage diagram of the sulfide solid-state battery assembled with the negative electrode material prepared in Example 1 at 0.1C. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods not mentioned in detail are all process steps or preparation methods known to those skilled in the art.
[0035] Example 1
[0036] A method for preparing a graphite negative electrode material comprises the following steps:
[0037] (1) Weigh 0.02 g of polyaniline, place it in 20 mL of deionized water, and stir evenly to obtain a polyaniline solution;
[0038] (2) Weigh 1.98 g of mesocarbon microsphere graphite, slowly add it to the polyaniline solution prepared in step (1), add 1 mL of anhydrous ethanol, and stir at 400 rpm for 3 hours to form a uniform suspension;
[0039] (3) The suspension obtained in step (2) was centrifugally filtered to obtain a filter cake; the filter cake was then placed in a vacuum oven at 80° C. and dried for 12 hours; and then placed in a nitrogen-filled environment and calcined at 300° C. for 3 hours to obtain the polyaniline-coated graphite negative electrode material of this embodiment.
[0040] Figure 1 is the FTIR graph of the graphite negative electrode material prepared in Example 1, from Figure 1 We can see four obvious peaks, among which 3340cm -1 The peak at 1046 cm is attributed to the OH stretching of water in the air during the test, while the peak at 1046 cm -1 and 1383cm -1The peak at 1635cm is caused by CN stretching. -1 The peak at is NH bending, which indicates that the graphite surface is coated with polyaniline containing N element.
[0041] Example 2
[0042] A method for preparing a graphite negative electrode material comprises the following steps:
[0043] (1) Weigh 0.01 g of polyaniline, place it in 20 mL of deionized water, and stir evenly to obtain a polyaniline solution;
[0044] (2) Weigh 1.99 g of mesocarbon microsphere graphite, slowly add it to the polyaniline solution prepared in step (1), add 1 mL of anhydrous ethanol, and stir at 400 rpm for 3 hours to form a uniform suspension;
[0045] (3) The suspension obtained in step (2) is centrifuged to obtain a filter cake; the filter cake is then placed in a vacuum oven at 80° C. and dried for 12 hours; and then placed in a nitrogen-filled environment and calcined at 300° C. for 3 hours to obtain a polyaniline-coated graphite negative electrode material.
[0046] Example 3
[0047] A method for preparing a graphite negative electrode material comprises the following steps:
[0048] (1) Weigh 0.1 g of polyaniline, place it in 20 mL of deionized water, and stir evenly to obtain a polyaniline solution;
[0049] (2) Weigh 1.90 g of mesocarbon microsphere graphite, slowly add it to the polyaniline solution prepared in step (1), add 1 mL of anhydrous ethanol, and stir at 400 rpm for 3 hours to form a uniform suspension;
[0050] (3) The suspension obtained in step (2) is centrifuged to obtain a filter cake; the filter cake is then placed in a vacuum oven at 80° C. and dried for 12 hours; and then placed in a nitrogen-filled environment and calcined at 300° C. for 3 hours to obtain a polyaniline-coated graphite negative electrode material.
[0051] Example 4
[0052] A method for preparing a graphite negative electrode material comprises the following steps:
[0053] (1) Weigh 0.02 g of polyaniline, place it in 20 mL of deionized water, and stir evenly to obtain a polyaniline solution;
[0054] (2) weighing 1.98 g of natural flake graphite, slowly adding it to the polyaniline solution prepared in step (1), adding 1 mL of anhydrous ethanol, and stirring at 400 rpm for 3 hours to form a uniform suspension;
[0055] (3) The suspension obtained in step (2) is centrifuged to obtain a filter cake; the filter cake is then placed in a vacuum oven at 80° C. and dried for 12 hours; and then placed in a nitrogen-filled environment and calcined at 300° C. for 3 hours to obtain a polyaniline-coated graphite negative electrode material.
[0056] Example 5
[0057] A method for preparing a graphite negative electrode material comprises the following steps:
[0058] (1) Weigh 0.02 g of polyaniline, place it in 20 mL of deionized water, and stir evenly to obtain a polyaniline solution;
[0059] (2) Weigh 1.98 g of mesocarbon microsphere graphite, slowly add it to the polyaniline solution prepared in step (1), add 1 mL of anhydrous ethanol, and stir at 400 rpm for 3 hours to form a uniform suspension;
[0060] (3) The suspension obtained in step (2) is centrifuged to obtain a filter cake; the filter cake is then placed in a vacuum oven at 80° C. and dried for 12 hours; and then placed in a nitrogen-filled environment and calcined at 300° C. for 3 hours to obtain a polyaniline-coated graphite negative electrode material.
[0061] Comparative Example 1
[0062] 2.0 g of the mesophase carbon microsphere graphite used in Example 1 was used as the negative electrode material.
[0063] Comparative Example 2
[0064] A method for preparing a graphite negative electrode material comprises the following steps:
[0065] (1) Weigh 0.02 g of polyaniline, place it in 20 mL of deionized water, and stir to obtain a polyaniline solution;
[0066] (2) Weigh 1.98 g of mesophase carbon microsphere graphite, slowly add it to the polyaniline solution prepared in step (1), add 1 mL of anhydrous ethanol, and stir at 400 rpm for 3 hours to form a uniform suspension;
[0067] (3) The suspension obtained in step (2) is centrifuged to obtain a filter cake; the filter cake is then placed in a vacuum oven at 80° C. and dried for 12 hours to obtain a polyaniline-coated graphite negative electrode material.
[0068] Compared with Example 1, in Comparative Example 2, the dried product was not calcined in step (3).
[0069] Comparative Example 3
[0070] A method for preparing a graphite negative electrode material comprises the following steps:
[0071] (1) Weigh 0.02 g of polyaniline, place it in 20 mL of deionized water, and stir to obtain a polyaniline solution;
[0072] (2) Weigh 1.98 g of mesophase carbon microsphere graphite, slowly add it to the polyaniline solution prepared in step (1), add 1 mL of anhydrous ethanol, and stir at 400 rpm for 3 hours to form a uniform suspension;
[0073] (3) The suspension obtained in step (2) is centrifuged to obtain a filter cake; the filter cake is then placed in a vacuum oven at 80° C. and dried for 12 hours; and then calcined at 300° C. in an air atmosphere for 3 hours to obtain a polyaniline-coated graphite negative electrode material.
[0074] Compared with Example 1, Comparative Example 3 carried out calcination in an air atmosphere in step (3).
[0075] Performance Testing
[0076] The graphite negative electrode materials prepared in Examples 1-5 and Comparative Examples 1-3 were ground together with the electrolyte LiP6S5Cl, and then a binder polytetrafluoroethylene (PTFE) was added. After grinding evenly again, the discs were cut into 8 mm diameter discs, placed in a mold, and the electrolyte LiP6S5Cl was added. The counter electrode was a Li-In alloy. The whole was pressed at a pressure of 450MPa to obtain an electrode sheet. When assembling a button cell, stainless steel gaskets were added to both sides of the electrode sheet, and a nickel mesh shrapnel was added to one side for packaging to obtain a sulfide solid-state battery. The first discharge specific capacity and first coulomb efficiency at 0.1C were tested. Wherein: the test conditions are: test pressure 5MPa, charge and discharge range -0.61V to 1.5V, and the test results are shown in Table 1.
[0077] Table 1:
[0078]
[0079]
[0080] It can be seen from Table 1 that the sulfide solid-state batteries assembled with the graphite negative electrode materials prepared in Examples 1-5 all have good first discharge specific capacity and first coulombic efficiency, wherein the first discharge specific capacity at 0.1C can reach 369.8-381.86 mAh / g, and the first coulombic efficiency can reach 89.42-93.71%.
[0081] Compared with Example 1, the negative electrode material of Comparative Example 1 is not coated with polyaniline, and the contact resistance between graphite and sulfide electrolyte is large, which is not conducive to the transmission of lithium ions and electrons, resulting in a decrease in battery performance.
[0082] Compared with Example 1, the negative electrode material of Comparative Example 2 was not calcined, and the surface of the material contained a certain amount of oxygen and moisture, resulting in a decrease in the performance of the battery.
[0083] Compared with Example 1, the battery performance of the negative electrode material of Comparative Example 3 dropped sharply when calcined in an air atmosphere. The main reason is that air calcination will add oxygen atoms to the surface of the material, and impurities containing oxygen atoms will consume lithium ions during the first cycle of charge and discharge of the battery, generating more irreversible solid electrolyte interface films (SEI), thereby reducing the initial coulombic efficiency.
[0084] Figure 2 The specific capacity-voltage diagram of the sulfide solid-state battery assembled from the graphite of Comparative Example 1 at 0.1C is shown in FIG. Figure 2 It can be seen that at 0.58V, the curve first decreases and then a peak appears, which is considered to be caused by battery polarization. Figure 3 The voltage curve of the battery assembled with the graphite negative electrode material prepared in Example 1 does not show a polarization peak at the same voltage. In addition, lithium ions begin to embed into graphite at -0.41V, at which time there is a capacity of about 50mAh / g for generating a solid electrolyte interface film (SEI) and other irreversible dead capacity, while the graphite electrode coated with polyaniline reduces this irreversible capacity to about 25mAh / g, thereby improving the reversible capacity of the embedded graphite and further improving the first coulombic efficiency.
[0085] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.
Claims
1. A method for preparing a graphite negative electrode material, characterized in that: The following steps are involved: (1) adding graphite to a conductive polymer solution and mixing to obtain a suspension; (2) subjecting the suspension to solid-liquid separation to obtain a solid product; (3) After drying the solid product, calcining it in an inert atmosphere to obtain a graphite negative electrode material coated with a conductive polymer.
2. The method for preparing a graphite negative electrode material according to claim 1, characterized in that: The conductive polymer solution includes a polyaniline solution.
3. The method for preparing a graphite negative electrode material according to claim 1 or 2, characterized in that: The concentration of the conductive polymer solution is 0.05-0.5 g / mL.
4. The method for preparing a graphite negative electrode material according to claim 1, characterized in that: The graphite is selected from natural graphite and / or mesophase carbon microspheres.
5. The method for preparing a graphite negative electrode material according to claim 1, characterized in that: In the suspension, the mass ratio of the graphite to the conductive polymer is 100:(0.5-5).
6. The method for preparing a graphite negative electrode material according to claim 1, characterized in that: In step (1), the mixing is carried out by stirring at a rotation speed of 300-600 rpm for 3-8 hours.
7. The method for preparing a graphite negative electrode material according to claim 1, characterized in that: In step (3), the drying is carried out under vacuum for 10-15 hours.
8. The method for preparing a graphite negative electrode material according to claim 1, characterized in that: In step (3), the calcination temperature is 280-350° C.; and / or the calcination time is 2-4 hours.
9. A graphite negative electrode material, characterized in that: The graphite negative electrode material is prepared by the preparation method of the graphite negative electrode material according to any one of claims 1 to 8.
10. A sulfide solid-state battery, characterized in that: It comprises a negative electrode, wherein the negative electrode comprises the graphite negative electrode material according to claim 9.
Citation Information
Patent Citations
Lithium ion battery cathode composite material and preparation method thereof
CN101916846A
Electrode negative electrode materials and their preparation methods
CN102299307A
Conducting-polymer dipped and coated lithium-ion battery composite-electrode material and preparation method thereof
CN102522563A
Battery, battery cathode, battery cathode material and preparation method thereof
CN104300129A
Negative electrode material, preparation method of negative electrode material, negative electrode and full-solid-state lithium ion battery
CN107665994A