Sodium-ion battery negative electrode material and preparation method thereof, sodium-ion battery and electric equipment
The preparation of sodium ion battery negative electrode material by combining coal-based materials with biomass-based materials and molten salts has solved the problems of low specific capacity and high cost of existing materials, and achieved high efficiency and low cost electrochemical performance improvement, suitable for sodium Application of ion batteries.
Patent Information
- Application Number
- CN202411002195.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The existing sodium ion battery anode materials cannot have high specific capacity, high first-time efficiency and low cost at the same time, and their electrochemical performance is poor, which limits the development of sodium ion batteries.
The preparation method of coal-based materials, biomass-based materials and molten salt is prepared by pickling, alkaline washing, water washing, thermal activation and carbonization treatment, and the negative electrode material of sodium ion battery is used to increase the spacing between carbon material by sulfur-containing activators. , optimize the electrochemical sodium storage performance.
It improves the specific capacity and first-time efficiency of the negative electrode material of sodium ion battery, reduces production costs, improves electrochemical performance and structural stability, and is suitable for large-scale production.
Smart Images

Figure CN118908206A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of secondary batteries, and in particular to a sodium ion battery negative electrode material and a preparation method thereof, a sodium ion battery and electrical equipment. Background Art
[0002] With the rapid development of social economy, the environmental problems and energy crisis caused by the continuous consumption of fossil energy are becoming increasingly prominent. There is an urgent need to develop new energy storage devices with high energy density, safety and efficiency. Lithium-ion batteries have been rapidly commercialized due to their excellent electrochemical properties. However, lithium resources are limited and unevenly distributed worldwide, which restricts the development of lithium-ion batteries. The development of new non-lithium electrochemical energy storage technologies is imminent. Since sodium and lithium are in the same main group, sodium-ion batteries have similar electrochemical properties to lithium-ion batteries, and sodium resources are abundant and low-cost, so they have greater application potential in the field of large-scale energy storage. Electrode materials are the core components of batteries and play a vital role in the performance of the entire battery.
[0003] At present, the carbon sources of sodium ion battery negative electrode materials on the market mainly include resin materials, asphalt-based materials, coal-based materials and biomass-based materials. Among them, coal-based materials have the advantages of wide sources and low cost, but they have the characteristics of long-range order and short-range disorder, which makes the specific capacity of coal-based materials low. Existing sodium ion battery negative electrode materials cannot have high specific capacity, high first efficiency and low cost at the same time. Therefore, it is necessary to improve the negative electrode materials of sodium ion batteries. Summary of the invention
[0004] The purpose of the present application is to provide a sodium ion battery negative electrode material and a preparation method thereof, a sodium ion battery and an electrical device to solve the above problems.
[0005] To achieve the above objectives, this application adopts the following technical solutions:
[0006] A method for preparing a negative electrode material for a sodium ion battery comprises: mixing a coal-based material with a biomass-based material and a molten salt to obtain a negative electrode material precursor, wherein the molten salt comprises any one of an alkali metal halide and an alkaline earth metal halide; mixing the negative electrode material precursor with a sulfur-containing activator, performing a thermal activation treatment, and obtaining a negative electrode material intermediate; and carbonizing the negative electrode material intermediate to obtain a negative electrode material for a sodium ion battery.
[0007] According to an embodiment of the present application, the coal-based material includes at least one of coking coal, anthracite, and lignite;
[0008] The biomass-based material includes sucrose;
[0009] The sulfur-containing activator includes at least one of sulfur powder, sulfur-containing amino acid, mercaptan, thioether, carbon disulfide, and sulfate;
[0010] And / or, the alkali metal halide includes at least one of KCl and LiCl;
[0011] And / or, before mixing the coal-based material with the biomass-based material and the molten salt, the preparation method further comprises: sequentially acid-washing, alkali-washing and water-washing the coal-based material, and mixing the acid-washed, alkali-washed and water-washed coal-based material with the biomass-based material and the molten salt to obtain a negative electrode material precursor;
[0012] And / or, the solution used for the acid washing includes an HCl solution, the concentration of the HCl solution is 2-5 mol / L, and the acid washing time is 1-3 h; the solution used for the alkali washing includes a NaOH solution, the concentration of the NaOH solution is 2-5 mol / L, and the alkali washing time is 1-3 h; the water washing time is 5-10 h.
[0013] According to an embodiment of the present application, the weight ratio of the coal-based material to the biomass-based material and the molten salt is (10 20): (5-12): (30-45).
[0014] According to an embodiment of the present application, the mass ratio of the sulfur-containing activator to the negative electrode material precursor is (1-1.5):(27-33).
[0015] According to an embodiment of the present application, the temperature of the thermal activation treatment is 300-480°C;
[0016] And / or, the thermal activation treatment time is 2-5h.
[0017] According to an embodiment of the present application, the thermal activation treatment is performed in a mixed atmosphere of ammonia and an inert gas, wherein the inert gas includes at least one of nitrogen and argon;
[0018] And / or, before the thermal activation treatment, the inert gas is introduced into the reaction container; within the first 30 minutes of the thermal activation treatment, the flow rate of the ammonia is 20-30 ml / min, and the flow rate of the inert gas is controlled at 170-200 ml / min; in the subsequent thermal activation treatment, the flow rate of the ammonia is 40-60 ml / min, and the flow rate of the inert gas is 130-160 ml / min; in the last half hour of the thermal activation treatment, the flow rate of the ammonia is 15-25 ml / min, and the flow rate of the inert gas is 170-200 ml / min.
[0019] According to an embodiment of the present application, the temperature of the carbonization treatment is 600-1200°C;
[0020] And / or, the carbonization treatment time is 2-6h;
[0021] And / or, the carbonization treatment is performed under a single protective atmosphere, and the single protective atmosphere includes any one of nitrogen and argon.
[0022] The present application also provides a sodium ion battery negative electrode material, which is prepared by the preparation method of the sodium ion battery negative electrode material described above.
[0023] The present application also provides a sodium ion battery, which includes the sodium ion battery negative electrode material described above.
[0024] The present application also provides an electrical device, which includes the sodium ion battery described above.
[0025] Compared with the prior art, the beneficial effects of this application include:
[0026] The molten salt of the present application can fully cross-link the coal-based material and the biomass-based material, construct a heterogeneous microcrystalline structure, improve the structural disorder of the carbon material, and optimize the electrochemical sodium storage performance of the negative electrode material, thereby improving the initial efficiency of the negative electrode material. Moreover, the sulfur-containing activator of the present application can increase the interlayer spacing of the carbon material, thereby improving the specific capacity of the negative electrode material. In addition, the present application also has the advantages of simple operation and low raw material prices, which can reduce production costs. In general, the method of the present application can make the prepared sodium ion battery negative electrode material have the advantages of higher specific capacity, higher initial efficiency and lower cost at the same time.
[0027] The sodium ion battery and electrical equipment of the present application also have excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0029] Figure 1 This is the SEM image of the negative electrode material of the sodium ion battery in Example 1. DETAILED DESCRIPTION
[0030] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:
[0031] A method for preparing a negative electrode material for a sodium ion battery, comprising:
[0032] Mixing a coal-based material with a biomass-based material and a molten salt to obtain a negative electrode material precursor, wherein the molten salt includes any one of an alkali metal halide and an alkaline earth metal halide;
[0033] The negative electrode material precursor is mixed with a sulfur-containing activator and subjected to thermal activation treatment to obtain a negative electrode material intermediate;
[0034] The negative electrode material intermediate is carbonized to obtain a negative electrode material for a sodium ion battery.
[0035] Therefore, by adding molten salt, the present application can fully cross-link the coal-based material and the biomass-based material to construct a heterogeneous microcrystalline structure, which not only improves the structural disorder of the carbon material, but also optimizes the electrochemical sodium storage performance of the negative electrode material, thereby improving the first efficiency of the negative electrode material. Moreover, the addition of the sulfur-containing activator in the present application can increase the interlayer spacing of the carbon material and improve the specific capacity of the negative electrode material. In addition, the method of the present application also has the advantages of simple operation and low raw material prices, which can reduce production costs. In general, the preparation method of the present application can make the prepared sodium ion battery negative electrode material have a higher specific capacity, a higher first efficiency and a lower production cost at the same time, which improves the defects of the existing sodium ion battery negative electrode materials with poor electrochemical performance and high production costs.
[0036] The molten salt of the present application can improve the cross-linking effect of coal-based materials and biomass-based materials, making the structures of coal-based materials and biomass-based materials more disordered, thereby increasing the carbon layer spacing. The method of the present application does not require the use of a cross-linking agent, and the process is simpler and has the advantages of being environmentally friendly. Moreover, the molten salt added in the present application can be decomposed in the high-temperature carbonization step, avoiding the removal step in the subsequent stage, the process is simple, in line with the concept of green environmental protection, and suitable for large-scale production.
[0037] According to an embodiment of the present application, the coal-based material includes at least one of coking coal, anthracite, and lignite; the above-mentioned coal-based material has the characteristic of good isotropy. Moreover, the coal-based material forms amorphous carbon after carbonization treatment, and the amorphous carbon is formed on the outer surface of the negative electrode material, which can improve the first coulombic efficiency of the negative electrode material.
[0038] The biomass-based material includes sucrose; the biomass-based material has the characteristics of high specific capacity and high compaction density. The biomass-based material and the coal-based material cooperate with each other to improve the sodium storage capacity of the negative electrode material of the sodium ion battery.
[0039] The sulfur-containing activator includes at least one of sulfur powder, sulfur-containing amino acids, thiols, sulfides, carbon disulfide, and sulfates; the above-mentioned types of sulfur-containing activators can increase the interlayer spacing of carbon materials, thereby improving the specific capacity of negative electrode materials; in addition, during high-temperature carbonization, the sulfur doped in the carbon skeleton nanostructure will volatilize, generating nanopores and defects in the carbon skeleton, increasing the surface area and the disorder of graphite-like crystallites, thereby providing additional sodium storage sites through adsorption of pores and defects, and at the same time, during high-temperature carbonization, as the temperature increases, a portion of sulfur atoms will be embedded in the carbon layer to increase the interlayer spacing, thereby increasing the platform capacity.
[0040] And / or, the alkali metal halide includes at least one of KCl and LiCl;
[0041] And / or, before mixing the coal-based material with the biomass-based material and the molten salt, the preparation method also includes: sequentially acid-washing, alkali-washing and water-washing the coal-based material, and mixing the acid-washed, alkali-washed and water-washed coal-based material with the biomass-based material and the molten salt to obtain a negative electrode material precursor; thereby, impurities in the coal-based material can be removed by acid-washing, alkali-washing and water-washing. If these impurities are not removed, they may affect the electrochemical properties of the material, such as reducing conductivity; the purity of the coal-based material can also be improved, the occurrence of side reactions can be reduced, and the electrochemical stability of the negative electrode material can be improved.
[0042] And / or, the solution used for acid washing includes HCl solution, the concentration of the HCl solution is 2-5 mol / L, and the acid washing time is 1-3 hours; the solution used for alkali washing includes NaOH solution, the concentration of the NaOH solution is 2-5 mol / L, and the alkali washing time is 1-3 hours; the water washing time is 5-10 hours. Thus, under the above conditions, impurities in coal-based materials can be effectively removed, thereby improving the electrochemical performance and stability of sodium ion battery negative electrode materials.
[0043] According to some embodiments of the present invention, before the coal-based material is sequentially acid-washed, alkaline-washed, and water-washed, the preparation method further comprises: crushing and sieving the coal-based material, and sequentially acid-washing, alkaline-washing, and water-washing the crushed and sieved coal-based material. Further, the particle size of the sieved material can be 300 meshes.
[0044] According to an embodiment of the present application, the weight ratio of the coal-based material to the biomass-based material and the molten salt is (10 20): (5-12): (30-45). For example, the weight ratio of the coal-based material to the biomass-based material and the molten salt can be 10:5:30, 10:6:35, 10:10:40, 10:12:45, 20:10:35, 20:12:40, 20:12:45, 20:8:35, 20:10:38, 20:10:40. When the content of the coal-based material, the biomass-based material and the molten salt is within the above range, the final negative electrode material can have excellent electrochemical properties and high structural stability. If the content of the coal-based material, the biomass-based material and the molten salt is not within the above content range, the electrochemical performance of the negative electrode material may decrease.
[0045] According to an embodiment of the present application, the mass ratio of the sulfur-containing activator to the negative electrode material precursor is (1-1.5):(27-33). For example, the mass ratio of the sulfur-containing activator to the negative electrode material precursor can be 1:27, 1:30, 1:33, 1.5:27, 1.5:33.
[0046] According to an embodiment of the present application, the temperature of the thermal activation treatment is 300-480°C; for example, the temperature of the thermal activation treatment may be 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, or 480°C.
[0047] And / or, the time of the thermal activation treatment is 2-5 hours. For example, the time of the thermal activation treatment can be 2 hours, 3 hours, 4 hours, or 5 hours.
[0048] According to an embodiment of the present application, the thermal activation treatment is carried out in a mixed atmosphere of ammonia and an inert gas, wherein the inert gas includes at least one of nitrogen and argon. Thus, in the mixed atmosphere, the generation of non-horse tissue (a quality defect of surface carburization) can be prevented, and the electrochemical performance of the material can be improved.
[0049] and / or, before the thermal activation treatment, the inert gas is introduced into the reaction container; within the first 30 minutes of the thermal activation treatment, the flow rate of the ammonia is 20-30 ml / min (e.g., 20 ml / min, 25 ml / min, 30 ml / min), and the inert gas is controlled at 170-200 ml / min (e.g., 170 ml / min, 180 ml / min, 200 ml / min); in the subsequent thermal activation treatment, the flow rate of the ammonia is 40-60 ml / min (e.g., 40 ml / min, 45 ml / min, 50 ml / min); min, 60ml / min), the flow rate of the inert gas is 130-160ml / min (e.g. 130ml / min, 140ml / min, 150ml / min, 160ml / min); in the last half hour of the thermal activation treatment, the flow rate of the ammonia is 15-25ml / min (e.g. 15ml / min, 20ml / min, 25ml / min), and the flow rate of the inert gas is 170-200ml / min (e.g. 170ml / min, 180ml / min, 190ml / min, 200ml / min). Further, before the thermal activation treatment, the flow rate of the inert gas can be 20-30ml / min (e.g. 20ml / min, 25ml / min, 30ml / min), and the inert gas introduction time can be 30min, thereby ensuring that the air in the reaction vessel is completely discharged. The reaction vessel for the thermal activation treatment can be a tubular furnace.
[0050] According to an embodiment of the present application, the temperature of the carbonization treatment is 600-1200°C; for example, the temperature of the carbonization treatment can be 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, or 1200°C.
[0051] Furthermore, the temperature can be increased to the carbonization treatment temperature at a heating rate of 5°C / min.
[0052] And / or, the carbonization treatment time is 2-6 hours; for example, the carbonization treatment time can be 2 hours, 3 hours, 4 hours, 5 hours, or 6 hours.
[0053] And / or, the carbonization treatment is performed under a single protective atmosphere, and the single protective atmosphere includes any one of nitrogen and argon.
[0054] The present application also provides a sodium ion battery negative electrode material, which is prepared by the preparation method of the sodium ion battery negative electrode material described above.
[0055] The present application also provides a sodium ion battery, which includes the sodium ion battery negative electrode material described above.
[0056] The present application also provides an electrical device, which includes the sodium ion battery described above.
[0057] It should be noted that “and / or” is used to indicate that one or both of the described situations may occur. For example, A and / or B includes (A and B) and (A or B).
[0058] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0059] Example 1
[0060] The preparation method of the negative electrode material of a sodium ion battery comprises the following steps:
[0061] Step S1: 10g of anthracite is crushed and passed through a 300-mesh sieve. After sieving, it is pickled with 100ml (2mol / L) HCl for 2h, then alkali-washed with 100ml (3mol / L) NaOH for 2h, then washed with deionized water until neutral for 6h. After drying, the anthracite is mixed with 6g sucrose and 35g molten salt (the molten salt is a mixture of KCl and LiCl, and the mass ratio of KCl to LiCl is 11:9) by a ball mill at a ball milling speed of 300 rpm for 6h to obtain a negative electrode material precursor.
[0062] Step S2: Evenly mix the negative electrode material precursor and sulfur powder (the mass ratio of sulfur powder to negative electrode material precursor is 1:30), and then place it in a tubular furnace with a mixed gas atmosphere. Before thermal activation treatment, first inject nitrogen into the tubular furnace for 30 minutes, and ensure that the flow rate is maintained at 20ml / min, so as to ensure that the air in the pipeline is completely removed. In the first 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 20ml / min, and the flow rate of nitrogen is controlled at 180ml / min; in the subsequent thermal activation process, the flow rate of ammonia is controlled at 50ml / min, and the flow rate of nitrogen is controlled within 140ml / min; in the last 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 20ml / min, and the flow rate of nitrogen is controlled at 190ml / min. After thermal activation treatment at a temperature of 480°C for 4h, the negative electrode material intermediate is obtained.
[0063] Step S3: calcining the negative electrode material intermediate to 1000° C. at a heating rate of 5° C. / min in a nitrogen atmosphere for carbonization treatment for 6 hours to obtain a negative electrode material for a sodium ion battery.
[0064] Example 2
[0065] The preparation method of the negative electrode material of a sodium ion battery comprises the following steps:
[0066] Step S1: 20g of coking coal was crushed and passed through a 300-mesh sieve. After sieving, it was pickled with 100ml (2mol / L) HCl for 3h, then alkali-washed with 100ml (3mol / L) NaOH for 3h, then washed with deionized water until neutral for 8h. After drying, the coking coal was mixed with 12g sucrose and 40g molten salt (molten salt is a mixture of KCl and LiCl, and the mass ratio of KCl to LiCl is 11:9) by a ball mill, and the ball milling speed was 300 rpm for 6h to obtain a negative electrode material precursor.
[0067] Step S2: Evenly mix the negative electrode material precursor and sulfur powder (the mass ratio of sulfur powder to negative electrode material precursor is 1:30), and then place it in a tubular furnace with a mixed gas atmosphere. Before thermal activation treatment, first inject nitrogen into the tubular furnace for 30 minutes, and ensure that the flow rate is maintained at 25ml / min, so as to ensure that the air in the pipeline is completely removed. In the first 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 25ml / min, and the flow rate of nitrogen is controlled at 170ml / min; in the subsequent thermal activation process, the flow rate of ammonia is controlled at 40ml / min, and the flow rate of nitrogen is controlled at 150ml / min; in the last 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 20ml / min, and the flow rate of nitrogen is controlled at 180ml / min. After thermal activation treatment at a temperature of 400°C for 5 hours, the negative electrode material intermediate is obtained.
[0068] Step S3: calcining the negative electrode material intermediate to 1100° C. at a heating rate of 5° C. / min under a nitrogen atmosphere for carbonization for 6 hours to obtain a negative electrode material for a sodium ion battery.
[0069] Example 3
[0070] The preparation method of the negative electrode material of a sodium ion battery comprises the following steps:
[0071] Step S1: 20g of lignite was crushed and passed through a 300-mesh sieve. After sieving, it was pickled with 100ml (2mol / L) HCl for 3h, then alkali-washed with 100ml (3mol / L) NaOH for 3h, then washed with deionized water until neutral for 8h. After drying, lignite was mixed with 10g sucrose and 38g molten salt (molten salt was a mixture of KCl and LiCl, with a mass ratio of KCl to LiCl of 11:9) in a ball mill at a ball milling speed of 300 rpm for 6h to obtain a negative electrode material precursor.
[0072] Step S2: Evenly mix the negative electrode material precursor and sulfur powder (the mass ratio of sulfur powder to negative electrode material precursor is 1:30), and then place it in a tubular furnace with a mixed gas atmosphere. Before thermal activation treatment, first inject nitrogen into the tubular furnace for 30 minutes, and ensure that the flow rate is maintained at 25ml / min, so as to ensure that the air in the pipeline is completely removed. In the first 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 30ml / min, and the flow rate of nitrogen is controlled at 180ml / min; in the subsequent thermal activation process, the flow rate of ammonia is controlled at 45ml / min, and the flow rate of nitrogen is controlled at 160ml / min; in the last 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 20ml / min, and the flow rate of nitrogen is controlled at 170ml / min. After thermal activation treatment at a temperature of 450°C for 4.5h, the negative electrode material intermediate is obtained.
[0073] Step S3: calcining the negative electrode material intermediate to 1200° C. at a heating rate of 5° C. / min under a nitrogen atmosphere for carbonization for 6 hours to obtain a negative electrode material for a sodium ion battery.
[0074] Comparative Example 1
[0075] The negative electrode material for a sodium ion battery was prepared by referring to the method of Example 1, except that no thermal activation treatment step was performed before the carbonization treatment. The specific steps of Comparative Example 1 are:
[0076] Step S1: 10g of anthracite is crushed and passed through a 300-mesh sieve. After sieving, it is pickled with 100ml (2mol / L) HCl for 2h, then alkali-washed with 100ml (3mol / L) NaOH for 2h, then washed with deionized water until neutral for 6h. After drying, the anthracite is mixed with 6g sucrose and 35g molten salt (the molten salt is a mixture of KCl and LiCl, and the mass ratio of KCl to LiCl is 11:9) by a ball mill at a ball milling speed of 300 rpm for 6h to obtain a negative electrode material precursor.
[0077] Step S2: calcining the negative electrode material precursor to 1000° C. at a heating rate of 5° C. / min in a nitrogen atmosphere for carbonization treatment for 6 hours to obtain a negative electrode material for a sodium ion battery.
[0078] Comparative Example 2
[0079] The negative electrode material of the sodium ion battery was prepared by referring to the method of Example 2, except that no molten salt was added. The specific steps of Comparative Example 2 are:
[0080] Step S1: 20g of coking coal is crushed and passed through a 300-mesh sieve. After sieving, it is acid-washed with 100ml (2mol / L) HCl for 3h, then alkaline-washed with 100ml (3mol / L) NaOH for 3h, then washed with deionized water until neutral for 8h. After drying, the coking coal and 12g of sucrose are evenly mixed in a ball mill at a ball milling speed of 300 rpm for 6h to obtain a negative electrode material precursor.
[0081] Step S2: Evenly mix the negative electrode material precursor and sulfur powder (the mass ratio of sulfur powder to negative electrode material precursor is 1:30), and then place it in a tubular furnace with a mixed gas atmosphere. Before thermal activation treatment, first inject nitrogen into the tubular furnace for 30 minutes, and ensure that the flow rate is maintained at 25ml / min, so as to ensure that the air in the pipeline is completely removed. In the first 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 25ml / min, and the flow rate of nitrogen is controlled at 170ml / min; in the subsequent thermal activation process, the flow rate of ammonia is controlled at 40ml / min, and the flow rate of nitrogen is controlled at 150ml / min; in the last 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 20ml / min, and the flow rate of nitrogen is controlled at 180ml / min. After thermal activation treatment at a temperature of 400°C for 5 hours, the negative electrode material intermediate is obtained.
[0082] Step S3: calcining the negative electrode material intermediate to 1100° C. at a heating rate of 5° C. / min under a nitrogen atmosphere for carbonization for 6 hours to obtain a negative electrode material for a sodium ion battery.
[0083] Comparative Example 3
[0084] The sodium ion battery negative electrode material was prepared by referring to the method of Example 3. The difference from Example 3 is that no biomass-based material is added, and only coal-based material is used as the carbon source. The specific steps of Comparative Example 3 are:
[0085] Step S1: 20g of lignite was crushed and passed through a 300-mesh sieve. After sieving, it was pickled with 100ml (2mol / L) HCl for 3h, then alkali-washed with 100ml (3mol / L) NaOH for 3h, then washed with deionized water until neutral for 8h. After drying, the lignite was mixed with 38g of molten salt (the molten salt was a mixture of KCl and LiCl, and the mass ratio of KCl to LiCl was 11:9) by a ball mill, the ball milling speed was 300 rpm, and the ball milling was performed for 6h to obtain a negative electrode material precursor.
[0086] Step S2: Evenly mix the negative electrode material precursor and sulfur powder (the mass ratio of sulfur powder to negative electrode material precursor is 1:30), and then place it in a tubular furnace with a mixed gas atmosphere. Before thermal activation treatment, first inject nitrogen into the tubular furnace for 30 minutes, and ensure that the flow rate is maintained at 25ml / min, so as to ensure that the air in the pipeline is completely removed. In the first 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 30ml / min, and the flow rate of nitrogen is controlled at 180ml / min; in the subsequent thermal activation process, the flow rate of ammonia is controlled at 45ml / min, and the flow rate of nitrogen is controlled at 160ml / min; in the last 30 minutes of thermal activation treatment, the flow rate of ammonia is controlled at 20ml / min, and the flow rate of nitrogen is controlled at 170ml / min. After thermal activation treatment at a temperature of 450°C for 4.5h, the negative electrode material intermediate is obtained.
[0087] Step S3: calcining the negative electrode material intermediate to 1200° C. at a heating rate of 5° C. / min under a nitrogen atmosphere for carbonization for 6 hours to obtain a negative electrode material for a sodium ion battery.
[0088] The performance of the sodium ion battery negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-3 was tested.
[0089] (1) SEM test
[0090] The sodium ion battery negative electrode material prepared in Example 1 was subjected to SEM testing, and the test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the negative electrode material of the sodium ion battery exhibits a granular morphology, and its particle size D50 is between 5-10 μm.
[0091] (2) Physical and chemical properties
[0092] The specific surface area, tap density, particle size distribution, interlayer spacing (D002) and moisture content of the sodium ion battery negative electrode materials of Examples 1-3 and Comparative Examples 1-3 were measured in detail. The test method was carried out in accordance with the standard GBT-41704-2022 "Graphite negative electrode materials for sodium ion batteries". The specific test results are shown in Table 1.
[0093] Table 1 Physical and chemical properties of sodium ion battery negative electrode materials of Examples 1-3 and Comparative Examples 1-3
[0094] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Specific surface area (m 2 / g)]]> 6.899 6.291 6.163 6.011 4.014 5.652 <![CDATA[Tap density (g / cm 3 )]]> 0.74 0.66 0.653 0.701 0.602 0.613 Particle size distribution D10 (μm) 3.294 3.560 4.142 3.652 4.542 4.265 Particle size distribution D50 (μm) 5.561 6.262 7.325 6.363 7.681 7.580 Particle size distribution D90 (μm) 9.234 10.614 11.405 11.102 12.146 12.325 Interlayer distance D002(nm) 0.388 0.382 0.380 0.379 0.360 0.370 Moisture (%) 0.201 0.226 0.231 0.223 0.231 0.234
[0095] (3) Button battery test
[0096] First, the sodium ion battery negative electrode material prepared in Examples 1-3 and Comparative Examples 1-3 is prepared into a negative electrode sheet of a sodium ion battery. The specific method is: the sodium ion battery negative electrode material, SP, CNT, binder MAC-500, SBR, and H2O are mixed to prepare a slurry, wherein the mass ratio of the sodium ion battery negative electrode material to SP, CNT, binder MAC-500, SBR, and H2O is 100:1.5:7.5:2:2.95:84, and the slurry is coated on the current collector to finally prepare a negative electrode sheet. The sodium sheet is used as the counter electrode; the electrolyte is a NaClO4 solution, wherein the solvent of the electrolyte includes EC, DEC and FEC, the mass ratio of EC to DEC and FEC is 1:1:0.05, and the concentration of the electrolyte is 1.4 mol / L; the diaphragm is made of glass fiber. Finally, it is assembled into a button battery.
[0097] The electrochemical performance was tested on a blue battery test cabinet with a charge and discharge voltage range of 1.5-3.95V and a scan rate of 0.01v / ms.
[0098] The first discharge capacity and first efficiency of the button cell were tested according to the standard of GBT-41704-2022 "Graphite-based negative electrode materials for sodium ion batteries". Under the same conditions, the changes in the electrochemical properties of the negative electrode materials for sodium ion batteries prepared in Examples 1-3 and Comparative Examples 1-3 were compared. The test results are shown in Table 2.
[0099] Table 2 Electrochemical performance test results of sodium ion battery negative electrode materials of examples and comparative examples
[0100]
[0101] It can be seen from Table 1 and Table 2 that in the present invention, the discharge specific capacity and the first coulombic efficiency of the sodium ion battery negative electrode materials of Examples 1, 2, and 3 are better than those of Comparative Examples 1, 2, and 3. The reasons are as follows: first, the thermal activation treatment step increases the interlayer spacing of the carbon material, and the coal-based material and the biomass-based material undergo a strong cross-linking reaction to increase the sodium storage capacity of the sodium ion battery negative electrode material. The addition of molten salt makes the cross-linking reaction between the coal-based material and the biomass-based material more thorough, thereby increasing the specific capacity of the negative electrode material and improving the first coulombic efficiency.
[0102] (4) Cylindrical 18650 full battery test
[0103] The negative electrode materials of the sodium ion battery of Examples 1-3 and Comparative Examples 1-3 were homogenized and coated to prepare negative electrode sheets. 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 ]O2 was used as the positive electrode and NaClO4 solution (the solvent of the electrolyte included EC, DEC and FEC, the mass ratio of EC to DEC and FEC was 1:1:0.05, and the concentration of the electrolyte was 1.4 mol / L) was used as the electrolyte to prepare a 1.5Ah cylindrical battery.
[0104] Test cycle capacity retention rate: charge and discharge current 0.5C / 1C, voltage range 1.5-3.95V, cycle number 1000 times.
[0105] Test rate discharge performance: charge at 0.5C constant current to 3.95V, constant voltage to 0.01C cutoff, and then discharge at 15C rate to 1.5V, discharge capacity at 15C rate discharge / discharge capacity at 1C rate discharge = rate discharge performance (%).
[0106] Test rate charging performance: charge at a constant current of 15C to 3.95V, constant voltage to 0.01C cutoff, and then discharge at a rate of 1C to 1.5V, discharge capacity at a rate of 15C / discharge capacity at a rate of 1C = rate charging performance (%).
[0107] The test results are shown in Table 3.
[0108] Table 3 Performance test results of sodium ion battery negative electrode materials of the embodiments and comparative examples
[0109]
[0110] It can be seen from Table 3 that the cycle capacity retention rate and double charge and discharge performance of Examples 1, 2, and 3 are higher than those of Comparative Examples 1, 2, and 3. The reason for this is that the specific surface area of the carbon materials of Examples 1-3 is higher than that of Comparative Examples 1-3. After the electrolyte is injected, the materials of Examples 1-3 have stronger adsorption performance for the electrolyte, retaining more electrolyte in the cylindrical battery, so the cycle performance and double charge and discharge performance are better than those of the comparative example. In addition, the carbon layer spacing of the negative electrode material of the sodium ion battery in the embodiment is larger, which is conducive to the conduction of sodium ions.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing a negative electrode material for a sodium ion battery, characterized in that: include: Mixing a coal-based material with a biomass-based material and a molten salt to obtain a negative electrode material precursor, wherein the molten salt includes any one of an alkali metal halide and an alkaline earth metal halide; The negative electrode material precursor is mixed with a sulfur-containing activator and subjected to thermal activation treatment to obtain a negative electrode material intermediate; The negative electrode material intermediate is carbonized to obtain a negative electrode material for a sodium ion battery.
2. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The coal-based material includes at least one of coking coal, anthracite, and lignite; The biomass-based material includes sucrose; The sulfur-containing activator includes at least one of sulfur powder, sulfur-containing amino acid, mercaptan, thioether, carbon disulfide, and sulfate; And / or, the alkali metal halide includes at least one of KCl and LiCl; And / or, before mixing the coal-based material with the biomass-based material and the molten salt, the preparation method further comprises: sequentially acid-washing, alkali-washing and water-washing the coal-based material, and mixing the acid-washed, alkali-washed and water-washed coal-based material with the biomass-based material and the molten salt to obtain a negative electrode material precursor; And / or, the solution used for the acid washing includes an HCl solution, the concentration of the HCl solution is 2-5 mol / L, and the acid washing time is 1-3 h; the solution used for the alkali washing includes a NaOH solution, the concentration of the NaOH solution is 2-5 mol / L, and the alkali washing time is 1-3 h; the water washing time is 5-10 h.
3. The method for preparing a negative electrode material for a sodium ion battery according to claim 2, characterized in that: The weight ratio of the coal-based material to the biomass-based material and the molten salt is (10 20): (5-12): (30-45).
4. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The mass ratio of the sulfur-containing activator to the negative electrode material precursor is (1-1.5):(27-33).
5. The method for preparing a negative electrode material for a sodium ion battery according to claim 1, characterized in that: The temperature of the thermal activation treatment is 300-480°C; And / or, the thermal activation treatment time is 2-5h.
6. The method for preparing a negative electrode material for a sodium ion battery according to claim 5, characterized in that: The thermal activation treatment is carried out in a mixed atmosphere of ammonia and an inert gas, wherein the inert gas includes at least one of nitrogen and argon; And / or, before the thermal activation treatment, the inert gas is introduced into the reaction container; within the first 30 minutes of the thermal activation treatment, the flow rate of the ammonia is 20-30 ml / min, and the flow rate of the inert gas is controlled at 170-200 ml / min; in the subsequent thermal activation treatment, the flow rate of the ammonia is 40-60 ml / min, and the flow rate of the inert gas is 130-160 ml / min; in the last half hour of the thermal activation treatment, the flow rate of the ammonia is 15-25 ml / min, and the flow rate of the inert gas is 170-200 ml / min.
7. The method for preparing a negative electrode material for a sodium ion battery according to any one of claims 1 to 6, characterized in that: The temperature of the carbonization treatment is 600-1200°C; And / or, the carbonization treatment time is 2-6h; And / or, the carbonization treatment is performed under a single protective atmosphere, and the single protective atmosphere includes any one of nitrogen and argon.
8. A sodium ion battery negative electrode material, characterized in that: The sodium ion battery negative electrode material is prepared by the method for preparing the sodium ion battery negative electrode material according to any one of claims 1 to 7.
9. A sodium ion battery, characterized in that: The sodium ion battery comprises the sodium ion battery negative electrode material according to claim 8.
10. An electrical device, characterized in that: The electrical equipment comprises the sodium ion battery according to claim 9.
Citation Information
Patent Citations
Negative electrode material for sodium ion battery and preparation method thereof
CN107732240A
Coal-based carbonized sodium battery negative electrode material and preparation method thereof, and sodium ion battery containing coal-based carbonized sodium battery negative electrode material
CN116613300A
Preparation method of coal-based hard carbon negative electrode material as well as product and application of coal-based hard carbon negative electrode material
CN117945385A
Cited By
Coal-based carbon negative electrode material, preparation method thereof and sodium ion battery
CN119797324A