Preparation method of hydrophobic deodorizing silicon dioxide

By reacting the alkylation reagent with the surface of silica, the surface hydrophobic and internal pore hydrophilic silica particles are prepared, and the deodorant is loaded in the pore, which solves the dispersion and deodorization of silica in the hydrophobic substrate. The performance problem has achieved a combination of hydrophobic and deodorizing properties and is suitable for the field of breathable membranes.

CN118908231AActive Publication Date: 2024-11-08FUJIAN HENGAN HLDG CO LTD +1

Patent Information

Application Number
CN202410956525.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

Smart Images

  • Figure CN118908231A_ABST
    Figure CN118908231A_ABST
Patent Text Reader

Abstract

The invention relates to the field of sanitary materials, provides a preparation method of hydrophobic deodorizing silicon dioxide, and solves the defects that silicon dioxide in the prior art is difficult to disperse in a hydrophobic base material and does not have deodorizing performance. Comprising the following steps: (1) preparing raw materials: taking fumed silica as a raw material; (2) adding an alkylating reagent into the fumed silica in the step (1) according to a mass ratio of the alkylating reagent to the fumed silica of (5-20): 100, reacting for 0.5-2 hours, and controlling the reaction temperature at 150-200 DEG C to obtain hydrophobic silica; and (3) adding ethanol and a deodorant solution into the hydrophobic silicon dioxide in the step (2) at normal temperature, stirring for 1-4 hours, drying, and filtering to obtain the hydrophobic deodorant silicon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sanitary materials, and in particular to a method for preparing hydrophobic and deodorizing silicon dioxide. Background Art

[0002] Porous silica particles have a wide range of applications in the fields of chemical industry, environmental protection, medical treatment, etc. due to their low density, high specific surface area, biocompatibility, and non-toxicity. In particular, they can be used to manufacture lightweight deodorizing breathable membranes. However, they contain a large amount of hydroxyl groups and are highly hydrophilic, making it difficult to evenly disperse in hydrophobic substrates such as polyethylene. In addition, they do not have deodorizing properties, which limits the further application of silica. Therefore, it is of great practical significance to modify silica to be hydrophobic and deodorizing and develop hydrophobic deodorizing silica.

[0003] Although there are some reports on hydrophobic materials and deodorizing materials, there are no reports on combining the two to prepare silica particles with both hydrophobic and deodorizing properties. For example, Chinese Patent No. 201680004464.7 discloses a method for preparing a hydrophobic silica aerogel and a hydrophobic silica aerogel prepared thereby, the method comprising the following steps: (1) preparing a water glass dispersion; (2) adding the water glass dispersion and a surface modifier solution to a reactor and simultaneously performing surface modification, gelation and solvent replacement to prepare a hydrophobic silica wet gel; and (3) drying the hydrophobic silica wet gel, wherein the method further comprises adding ammonium hydroxide during the reaction of step (2), wherein the water glass dispersion comprises a water glass solution and an inorganic acid, wherein after adding the entire amount of the surface modifier solution, ammonium hydroxide is added when the pH in the reactor reaches 5 to 10, and wherein the amount of ammonium hydroxide added is such that the molar ratio of the ammonium hydroxide to the surface modifier in the surface modifier solution is in the range of 0.5 to 25. The silica has hydrophobic properties but does not have deodorizing properties.

[0004] For another example, Chinese Patent No. 202010618202.8 discloses a method for surface modification of silica, including: cleaning the surface of a silica sample; continuously heating the silica sample at 490°C to 510°C for 30 to 35 minutes. Hydroxylation of the surface of the silica sample; placing the silica sample in an electrolytic cell containing 0.025% to 0.030% calcium chloride or magnesium chloride solution, and using 1.5V / cm to 1.7V / cm direct current to electrically stimulate the surface of the silica to cause the S iOS i bond to break and combine with H+ and OH- in water. Alkylation of the silica sample; placing the silica sample treated with hydroxylation by electrical excitation in a preferred KH560: benzene: methanol = 1: (9 to 11): (0.5 to 0.7) new silane coupling agent reaction solution to complete the alkylation reaction and obtain a surface-modified silica sample. After modifying the silica sample using the silica surface modification method provided by the present invention, the wetting angle of deionized water on the silica sample surface is significantly increased, and the hydrophobicity of the silica sample surface is greatly improved. However, the silica obtained using the modification method of the present invention does not have a deodorizing function.

[0005] The difficulty lies in how to develop silica particles with hydrophobic surface and hydrophilic interior. If the hydrophobicity of silica is too high and the pores are also hydrophobic, it will greatly affect the loading of the deodorant. Therefore, in the field of breathable membranes, it is of great practical significance to develop silica particles with hydrophobic surface, so that they have a certain compatibility with the polyethylene matrix; and the internal pores of the hydrophilic particles can load the deodorant, resulting in excellent deodorizing performance. Summary of the invention

[0006] Therefore, in view of the above problems, the present invention provides a method for preparing hydrophobic deodorizing silica to solve the defects of the prior art that silica is difficult to disperse in a hydrophobic substrate and has no deodorizing performance.

[0007] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing hydrophobic deodorizing silica, comprising the following preparation steps:

[0008] (1) Prepare raw materials: use fumed silica as raw material;

[0009] (2) adding an alkylating agent to the fumed silica described in step (1), wherein the mass ratio of the alkylating agent to the fumed silica is 5-20:100, reacting for 0.5-2h, and controlling the reaction temperature at 150-200°C to obtain hydrophobic silica;

[0010] (3) Adding ethanol and the deodorant solution to the hydrophobic silica in step (2) at room temperature, stirring for 1-4 hours, drying, filtering, and obtaining hydrophobic deodorizing silica.

[0011] Furthermore: the fumed silica used in step (1) is nanoscale.

[0012] Furthermore: the alkylating agent in step (2) is any one of hexamethyldisilazane, trimethoxyoctadecylsilane, dimethyldichlorosilane and trimethylchlorosilane.

[0013] Furthermore: the deodorant described in step (3) is a plant deodorant containing any one of arginine, glycine, alanine, and amino acid cations, and the solid content of the deodorant is 30-35wt%.

[0014] Furthermore: the mass ratio of the deodorant solution, ethanol and hydrophobic silica in step (3) is 1-5:1:1.

[0015] A hydrophobic deodorizing silica particle is prepared by adopting the above-mentioned method for preparing the hydrophobic deodorizing silica.

[0016] By adopting the above technical solution, the beneficial effects of the present invention are:

[0017] 1. The present invention controls the amount of alkylating agent used to modify the porous silica particles to have a hydrophobic surface and hydrophilic internal pores, and then loads a deodorant inside the pores of the particles, so that the prepared silica particles have hydrophobic and deodorizing properties.

[0018] 2. The present invention utilizes an alkylating agent to react with hydroxyl groups on the surface of silica, and controls the degree of alkylation in the reaction to prepare silica particles with hydrophobic surface and hydrophilic internal pores. The plant deodorant is then loaded into the hydrophilic internal pores of the porous silica particles by utilizing the hydrogen bonding between the functional groups such as carboxyl and amino groups of the plant deodorant and the hydroxyl groups in the internal pores of the porous silica particles, so that the surface hydrophobic silica particles have deodorizing properties. Such materials can be used in the manufacture of lightweight deodorizing breathable membranes in the fields of sanitary materials and the like.

[0019] 3. The mechanism of surface modification of silicon dioxide is based on the fact that the silanol groups on its surface can react with organic silanes, alcohols and other substances. The Si(CH3)3 group in the alkylating agent reacts with the OH group on the surface of SiO2, so that the highly active Si(CH3)3 on the alkylating agent is bonded to the surface of SiO2, thereby achieving hydrophobic modification of the surface of nano-SiO2. The reaction equation for the reaction between the silanol groups on the surface of SiO2 and the alkylating agent is:

[0020]

[0021] The plant deodorant molecules enter the pores of the porous alkylated silica particles, and the functional groups such as carboxyl, amino, and hydroxyl in the plant deodorant react with the hydroxyl groups inside the alkylated silica particles through hydrogen bonds and are adsorbed on the internal surface of the pores of the alkylated silica particles.

[0022] 4. The present invention controls the mass ratio of the alkylating agent to the fumed silica and the reaction time so that the hydrophobic groups preferentially occupy the surface of the silica particles. The mass ratio of the alkylating agent to the fumed silica is controlled at 5-20:100, so that the surface of the silica particles can be made hydrophobic and the internal pores can be made hydrophilic. After the alkylation is completed, the deodorant is added. Since the silica particles are porous structures, the internal pores are connected to the outside, so the deodorant can enter the inside. Since the external pores are pre-occupied by the hydrophobic groups, there will be no deodorant in the external pores, and the deodorant can be smoothly distributed in the internal channels of the silica particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 : (a) Water drop contact angle diagram of alkylated silica particles, (b) Water drop contact angle diagram of deodorant-loaded alkylated silica particles;

[0024] Figure 2 It is a high-resolution TEM photo and EDS spectrum of alkylated silica particles;

[0025] Figure 3 This is a high-resolution TEM photo and EDS spectrum of deodorizing alkylated silica particles. DETAILED DESCRIPTION

[0026] The method of the present invention is further described in detail below in conjunction with the embodiments. It should be particularly noted that the protection scope of the present invention should include but is not limited to the technical content disclosed in this embodiment.

[0027] Embodiment 1

[0028] A method for preparing hydrophobic deodorizing silica comprises the following preparation steps:

[0029] (1) adding 12 mL of hexamethyldisilazane to 100 g of porous silica particles and reacting at 180° C. for 30 min to obtain hexamethyldisilazane-modified silica particles;

[0030] (2) 100 g of hexamethyldisilazane-modified silica particles and 100 g of ethanol were added to 100 mL of a plant deodorant solution containing arginine with a solid content of 30 wt.%, stirred for 1 h, filtered, washed, and dried to obtain hydrophobic deodorizing silica particles.

[0031] Embodiment 2

[0032] A method for preparing hydrophobic deodorizing silica comprises the following preparation steps:

[0033] (1) 20 mL of trimethoxyoctadecylsilane was added to 100 g of porous silica particles and reacted at 200° C. for 30 min to obtain trimethoxyoctadecylsilane-modified silica particles.

[0034] (2) 100 g of trimethoxyoctadecylsilane-modified silica particles and 100 g of ethanol were added to 500 mL of a plant deodorant solution containing glycine with a solid content of 30 wt.%, stirred for 1 h, filtered, washed, and dried to obtain hydrophobic deodorizing silica particles.

[0035] Embodiment 3

[0036] A method for preparing hydrophobic deodorizing silica comprises the following preparation steps:

[0037] (1) 8 mL of dimethyldichlorosilane was added to 100 g of porous silica particles and reacted at 150° C. for 30 min to obtain hexamethyldisilazane-modified silica particles.

[0038] (2) 100 g of dimethyldichlorosilane-modified silica particles and 100 g of ethanol were added to 300 mL of a plant deodorant solution containing alanine with a solid content of 30 wt.%, stirred for 1 h, filtered, washed, and dried to obtain hydrophobic deodorizing silica particles.

[0039] Embodiment 4

[0040] A method for preparing hydrophobic deodorizing silica comprises the following preparation steps:

[0041] (1) 15 mL of trimethylsilyl chloride was added to 100 g of porous silica particles and reacted at 185° C. for 30 min to obtain trimethylsilyl chloride-modified silica particles.

[0042] (2) 100 g of trimethylchlorosilane-modified silica particles and 100 g of ethanol were added to 200 mL of a plant deodorant solution containing arginine with a solid content of 30 wt.%, stirred for 1 h, filtered, washed, and dried to obtain hydrophobic deodorizing silica particles.

[0043] Main performance test

[0044] The hydrophobic and deodorizing silica particles prepared by the present invention have the important feature that the material has both hydrophobic and deodorizing properties, so the hydrophobic and deodorizing properties are tested.

[0045] refer to Figures 1 to 3The modified deodorizing silica particles in all the examples have hydrophobic properties and deodorizing properties. The hydrophobic silica particles and the hydrophobic deodorizing silica particles were respectively glued to a glass plate for water drop shape analysis. Figure 1 As shown. Pure silica particles have strong hydrophilicity. When water drops on the surface of the particles, the water drops are immediately absorbed by the particles, showing a contact angle of 0°. The contact angle of the hydrophobically modified silica particles is 139.5°, indicating that they have good hydrophobicity. The contact angle of the hydrophobic deodorizing silica particles after further deodorizing modification is 134.2°, indicating that the deodorizing modified particles are still very hydrophobic, and the deodorant treatment has little effect on their hydrophobicity.

[0046] According to the method of GB / T 33610.2-2017, the deodorization performance of hydrophobic deodorizing silica particles was analyzed using a detection tube. The reduction rate of ammonia concentration by hydrophobic deodorizing silica particles reached 98.8%, which has a good deodorization effect. This type of material can be used in the manufacture of breathable membranes in the medical field.

[0047] Embodiment 5

[0048] A composition of a lightweight breathable base film for sanitary products, comprising the following raw materials in parts by weight: 5 parts by weight of the hydrophobic deodorizing silica of Example 1, 3 parts of an antibacterial agent, and 100 parts by weight of a polyolefin resin, wherein the hydrophobic deodorizing silica is prepared by using an alkylating agent, a deodorizing agent, and an antibacterial agent to modify silica, wherein the deodorizing agent is a plant deodorant containing arginine with a solid content of 30 wt%, and the antibacterial agent is chitosan;

[0049] The hydrophobic deodorizing silica is prepared by the following steps: (1) preparing raw materials: using fumed silica as raw material; (2) adding hexamethyldisilazane to the fumed silica described in step (1), wherein the mass ratio of hexamethyldisilazane to the fumed silica is 5:100, reacting for 0.5 h, and controlling the reaction temperature at 150° C. to obtain hydrophobic silica; (3) adding ethanol, a plant deodorant containing arginine with a solid content of 30 wt % and chitosan to the hydrophobic silica in step (2) at room temperature, stirring for 1 h, centrifugally filtering and drying, and controlling the moisture content to be within 400 ppm to obtain hydrophobic deodorizing silica.

[0050] The mass ratio of arginine, chitosan, ethanol and hydrophobic silica is 0.2:0.1:50:20.

[0051] The silica particle size is 18 nm, the average adsorption pore size is 0.24 nm, and the specific surface area is 215 m 2 / g.

[0052] Embodiment 6

[0053] A method for preparing a lightweight deodorant and breathable base film for sanitary products comprises the following preparation steps: (1) mixing the composition of the lightweight breathable base film for sanitary products of Example 5 with a processing aid, wherein the processing aid is specifically nano titanium dioxide, calcium carbonate, a titanate coupling agent, and polyethylene wax, and the amount of the processing aid is 2wt% of the polyolefin resin, that is, the processing aid is 2 parts by weight, more specifically, 0.5 parts by weight of titanium dioxide, 0.6 parts by weight of calcium carbonate, 0.4 parts by weight of a titanate coupling agent, and 0.5 parts by weight of polyethylene wax, and stirring evenly to obtain a mixture; (2) feeding the mixture into a screw extruder, and subjecting it to melt extrusion and cooling; (3) subjecting it to four-stage stretching by a stretching mechanism, and the stretching ratios are 1.3, 1.5, 1.7, and 1.6 respectively; and (4) further subjecting it to shaping and cooling to prepare a lightweight deodorant and breathable base film.

[0054] Embodiment 7

[0055] A deodorizing disposable sanitary product comprises a liquid permeable surface layer, an absorbent body and a liquid impermeable bottom layer which are sequentially stacked from top to bottom, wherein the absorbent body is formed by mixing a deodorizing material, fluff pulp and a high molecular weight water-absorbent resin in a weight ratio of 1:20:2, the liquid impermeable bottom layer is formed by a hydrophobic deodorizing breathable membrane and a hydrophobic non-woven fabric composited on the bottom of the hydrophobic deodorizing breathable membrane, the hydrophobic deodorizing breathable membrane is formed by 5 parts by weight of hydrophobic deodorizing silica, 100 parts by weight of a polyolefin resin and 3 parts by weight of a processing aid, and the deodorizing material is deodorizing silica loaded with an aromatic material.

[0056] The preparation method of the deodorizing silica loaded with aromatic materials is as follows: silica particles with a pore size of 10 nm are selected as raw materials, aromatic essential oil is added, stirred to allow the aromatic essential oil to be fully absorbed by the silica, and then an acrylic acid aqueous adhesive is added, and stirred again to obtain the deodorizing silica loaded with aromatic materials. The silica: aromatic essential oil: acrylic acid aqueous adhesive = 1:0.1:0.05, calculated by mass ratio.

[0057] The solid content of the plant deodorant is 30wt%, the mass ratio of the plant deodorant, ethanol and hydrophobic silica is 0.2:50:20, the silica particle size is 18nm, the average adsorption pore size is 0.24nm, and the specific surface area is 215m 2 / g.

[0058] The preparation method of the hydrophobic deodorizing silica is prepared by adopting the preparation method of the hydrophobic deodorizing silica in Example 1.

[0059] Embodiment 8

[0060] A method for preparing a deodorizing disposable sanitary product, comprising the following preparation process:

[0061] (1) preparing a liquid-permeable surface layer;

[0062] (2) Preparation of absorbent: Deodorizing material, fluff pulp and high molecular weight water-absorbent resin are fed into a mold wheel mold cavity in a weight ratio of 1:200:2 for molding, and then demolded to obtain an absorbent; the deodorizing material is deodorizing silica loaded with aromatic material, and the preparation method of the deodorizing silica loaded with aromatic material is as follows: silica particles with a pore size of 10 nm are selected as raw materials, aromatic essential oil is added, stirred so that the aromatic essential oil is fully absorbed by silica, and then low-temperature water-based adhesive is added, and stirred again to obtain deodorizing silica loaded with aromatic material; the silica: aromatic essential oil: acrylic water-based adhesive = 1:0.1:0.05, calculated by mass ratio;

[0063] (3) Preparing a liquid-impermeable bottom layer: unwinding a hydrophobic nonwoven fabric, transferring it online, and compounding a hydrophobic deodorizing breathable film online on its surface, wherein the preparation method of the hydrophobic deodorizing breathable film comprises the following steps: a. mixing 50 parts by weight of hydrophobic deodorizing silica, 100 parts by weight of a polyolefin resin, and 3 parts by weight of a processing aid, stirring the mixture uniformly, and obtaining a mixture; b. feeding the mixture into a screw extruder, extruding the mixture through melt extrusion, and cooling the mixture; c. performing four-stage stretching through a stretching mechanism, and the stretching ratios are 1.3, 1.5, 1.7, and 1.6, respectively; d. performing shaping and cooling the mixture;

[0064] The preparation method of hydrophobic deodorizing silica adopts the preparation method of Example 1;

[0065] (4) The liquid-permeable surface layer, absorbent body and liquid-impermeable bottom layer transmitted online are compounded into one body, and then cut into pieces to obtain individual deodorizing disposable sanitary products.

[0066] Embodiment 9

[0067] A deodorizing adult diaper comprises a liquid-permeable surface layer, an absorbent and a liquid-impermeable bottom layer which are sequentially stacked from top to bottom, wherein the absorbent comprises 10 parts by weight of a polymer water-absorbent resin, 2 parts by weight of silicon dioxide, 5 parts by weight of a surfactant, 1 part by weight of an essential oil, 0.5 parts by weight of an acrylic acid aqueous adhesive and 900 parts by weight of fluff pulp, and the liquid-impermeable bottom layer comprises a hydrophobic deodorizing breathable film and a hydrophobic non-woven fabric composited on the bottom of the hydrophobic deodorizing breathable film, and the hydrophobic deodorizing breathable film comprises 5 parts by weight of hydrophobic deodorizing silicon dioxide, 100 parts by weight of a polyolefin resin and 3 parts by weight of a processing aid.

[0068] The preparation method of the hydrophobic deodorizing silica is as follows: (1) preparing raw materials: using fumed silica as raw material; (2) adding hexamethyldisilazane to the fumed silica described in step (1), wherein the mass ratio of the alkylating agent to the fumed silica is 5:100, reacting for 0.5 h, and controlling the reaction temperature at 150° C. to obtain hydrophobic deodorizing silica; (3) adding ethanol and a plant deodorant solution containing arginine to the hydrophobic silica in step (2) at room temperature, stirring for 1 h, centrifugally filtering and drying, and controlling the moisture content to be within 400 ppm to obtain hydrophobic deodorizing silica.

[0069] The solid content of the plant deodorant is 30wt%, the mass ratio of the plant deodorant, ethanol and hydrophobic silica is 0.2:50:20, the silica particle size is 18nm, the average adsorption pore size is 0.24nm, and the specific surface area is 215m 2 / g.

[0070] The preparation process of the absorbent is as follows: a. adding a surfactant to the essential oil for emulsification so that the essential oil is wrapped by the surfactant; b. mixing a high molecular weight water-absorbent resin and silicon dioxide with a pore size of 10 nm evenly, adding an acrylic acid aqueous adhesive to bond the high molecular weight water-absorbent resin and the silicon dioxide together; c. adding the essential oil emulsified in step a to the material in step b, mixing and stirring evenly to obtain a preform; d. feeding the preform and the fluff pulp into a mold wheel mold cavity according to a ratio for molding, and then demolding to obtain the absorbent.

[0071] Embodiment 10

[0072] A method for preparing a deodorized adult diaper, comprising the following preparation process:

[0073] (1) preparing a liquid-permeable surface layer;

[0074] (2) preparing an absorbent: a. adding a surfactant to the essential oil for emulsification so that the essential oil is wrapped by the surfactant; b. mixing a high molecular weight water-absorbing resin and silicon dioxide with a pore size of 10 nm, and adding an acrylic acid-based aqueous adhesive to bond the high molecular weight water-absorbing resin and the silicon dioxide together; c. adding the essential oil emulsified in step a to the material in step b, mixing and stirring to obtain a preform; d. feeding the preform and the fluff pulp into a mold wheel mold cavity according to a ratio for molding, and then demolding to obtain an absorbent;

[0075] (3) Preparing a liquid-impermeable bottom layer: unwinding a hydrophobic nonwoven fabric, transferring it online, and compounding a hydrophobic deodorizing breathable film online on its surface, wherein the preparation method of the hydrophobic deodorizing breathable film comprises the following steps: a. mixing 50 parts by weight of hydrophobic deodorizing silica, 100 parts by weight of a polyolefin resin, and 3 parts by weight of a processing aid, stirring the mixture uniformly, and obtaining a mixture; b. feeding the mixture into a screw extruder, extruding the mixture through melt extrusion, and cooling the mixture; c. performing four-stage stretching through a stretching mechanism, and the stretching ratios are 1.3, 1.5, 1.7, and 1.6, respectively; d. performing shaping and cooling the mixture;

[0076] The preparation method of hydrophobic deodorizing silica is as follows: a. preparing raw materials: using fumed silica as raw material; b. adding an alkylating agent to the fumed silica described in step (1), wherein the mass ratio of the alkylating agent to the fumed silica is 5-20:100, reacting for 1 hour, and controlling the reaction temperature at 150° C. to obtain hydrophobic deodorizing silica; c. adding ethanol and a deodorant solution to the hydrophobic silica in step (2) at room temperature, stirring for 2 hours, centrifugally filtering and drying, and controlling the moisture content to be within 400 ppm, to obtain hydrophobic deodorizing silica;

[0077] (4) The liquid-permeable surface layer, absorbent body and liquid-impermeable bottom layer transmitted online are compounded into one body, and then cut into pieces to obtain individual deodorizing disposable sanitary products.

[0078] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.

Claims

1. A method for preparing hydrophobic deodorizing silica, characterized in that: The method comprises the following preparation steps: (1) Prepare raw materials: use fumed silica as raw material; (2) adding an alkylating agent to the fumed silica described in step (1), wherein the mass ratio of the alkylating agent to the fumed silica is 5-20:100, reacting for 0.5-2h, and controlling the reaction temperature at 150-200°C to obtain hydrophobic silica; (3) Adding ethanol and the deodorant solution to the hydrophobic silica in step (2) at room temperature, stirring for 1-4 hours, drying, filtering, and obtaining hydrophobic deodorizing silica.

2. The method for preparing a hydrophobic deodorizing silica according to claim 1, characterized in that : The fumed silica used in step (1) is nanoscale.

3. A method for preparing a hydrophobic deodorizing silica according to claim 1, characterized in that: The alkylating agent in step (2) is any one of hexamethyldisilazane, trimethoxyoctadecylsilane, dimethyldichlorosilane and trimethylchlorosilane.

4. A method for preparing a hydrophobic deodorizing silica according to claim 1, characterized in that: The deodorant described in step (3) is a plant deodorant containing any one of arginine, glycine, alanine, and amino acid cations, and the solid content of the deodorant is 30-35wt%.

5. The method for preparing a hydrophobic deodorizing silica according to claim 1, characterized in that: The mass ratio of the deodorant solution, ethanol and hydrophobic silica in step (3) is 1-5:1:

1.

6. A hydrophobic deodorizing silica particle, characterized in that: The hydrophobic deodorizing silica is prepared by the preparation method of the hydrophobic deodorizing silica described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for preparing hydrophobic silica aerogel and hydrophobic silica aerogel prepared therefrom

    CN107108237A

  • Surface modification method for silicon dioxide

    CN111718603A

  • Cosmetic composition comprising imidopercarboxylic acid derivative and n-acylated amino acid ester

    CN101543465A

  • Water containing powder composition

    CN102686207A

  • Method of isolating lipids from a lipids containing biomass with aid of hydrophobic silica

    CN112166176A

Cited By

  • Composition of light breathable bottom film of hygienic product and preparation method of breathable bottom film

    CN118702977A

  • A composition for a lightweight breathable bottom film of hygiene products and a method for preparing the breathable bottom film.

    CN118702977B

  • Preparation method, production system and production method of hydrophobic nano silicon dioxide

    CN120887431A