13X type molecular sieve and preparation method thereof

Through two-stage crystallization treatment and recycling of inorganic waste, the problems of low silicon source utilization and poor product dispersion in the preparation of 13X molecular sieve were solved, and the controllability and adsorption capacity of product size and morphology were improved.

CN118908239AActive Publication Date: 2024-11-08CHINA ENERGY GRP NINGXIA COAL IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410976175.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In the existing preparation method of 13X type molecular sieve, the silicon source utilization rate is low, the product size and morphology are not easy to control, and the product dispersion is poor.

Method used

The gel system containing silicon and aluminum sources is subjected to the first crystallization and the second crystallization treatment by adopting the two-stage crystallization treatment method, and the mother liquor after the treatment of inorganic waste is mixed with the crystallization product system and calcined Prepare 13X type molecular sieve by solid-liquid separation and other steps.

Benefits of technology

The utilization rate of silicon source is improved, the controllability of product size and morphology is achieved, the dispersion is enhanced, and the adsorption capacity and application prospect of molecular sieves are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954577620000101
    Figure BDA0004954577620000101
Patent Text Reader

Abstract

The invention provides a 13X type molecular sieve and a preparation method thereof. The method comprises the following steps: S1, sequentially carrying out first crystallization treatment and second crystallization treatment on a gel system containing a silicon source and an aluminum source to obtain a system containing a crystallization product; the temperature of the first crystallization treatment is 20-60 DEG C, the time of the first crystallization treatment is 4-24 hours, the temperature of the second crystallization treatment is at least 20 DEG C higher than the temperature of the first crystallization treatment, and the time of the second crystallization treatment is 6-48 hours; s2, roasting the mixed system of the inorganic waste and the flux to obtain a roasted product; reacting the roasted product with an acid aqueous solution, and carrying out first solid-liquid separation to obtain filter residues and first filtrate; reacting the filter residue with an aqueous alkali solution, and carrying out second solid-liquid separation to obtain a second filtrate; mixing the first filtrate with the second filtrate to obtain mother liquor; wherein the inorganic waste comprises an aluminum element, a silicon element and an oxygen element; and S3, mixing the crystallization product in the crystallization product-containing system with a mother solution, and carrying out aging and third crystallization treatment to obtain the 13X type molecular sieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inorganic material preparation, and in particular to a 13X molecular sieve and a preparation method thereof. Background Art

[0002] Molecular sieve is a type of aluminosilicate, which has the characteristics of uniform pore size, regular crystal structure, rich pore system, large specific surface area and good thermal stability. It is considered to be the preferred adsorbent material for removing oxygen-containing compounds in olefins. The pore size of FAU type (X, Y type) molecular sieve is about 0.74nm. Among them, X type molecular sieve can better remove oxygen-containing compound impurities in olefins, and there are many related studies. It has also been applied in industrial practice. When X type molecular sieve is used for olefin purification, its adsorption heat is high and usually requires pre-loading. However, some olefins will be adsorbed during the adsorption purification process.

[0003] The research and development of X-type molecular sieve adsorbents mainly focuses on the following three aspects: first, selective adsorption of oxygenated compounds, and as little adsorption of olefins as possible; second, effective reduction of adsorption heat; third, effective increase of adsorption capacity of adsorbents, adsorption purification depth, etc. The use of adsorption to separate substances has been widely used in petroleum cracking and refinery catalytic cracking. At present, the research on adsorption separation technology is mainly used to remove oxygenated compounds from C4 and above hydrocarbons by adsorption; in addition, the hydrocarbon products produced by indirect liquefaction of coal through Fischer-Tropsch synthesis have different carbon number distributions, and the oxygenated compounds in each carbon number product are of various types, their molecular weight and molecular structure vary greatly, and the pore size and composition of commonly used molecular sieves are also different. Therefore, there is no adsorbent suitable for separating oxygenated compounds from Fischer-Tropsch products with all carbon number distributions. Therefore, adsorbents with uniform and ordered micropores, large specific surface area, large adsorption capacity and low adsorption heat have broad application prospects in the field of adsorption separation.

[0004] The existing document (publication number CN103523796A) proposes a method for preparing a submicron X-type molecular sieve, which uses silica sol as a silicon source to prepare a crystallization directing agent; uses water glass, sodium aluminate or aluminum hydroxide, and sodium hydroxide to prepare a molecular mother liquor, and after adding the directing agent to the mother liquor, it is aged for a certain period of time, and then a weakly polar water-soluble dispersant is added, stirred evenly, and hydrothermally crystallized in a closed container with the assistance of microwaves to obtain a submicron X-type molecular sieve.

[0005] However, the existing preparation method of 13X molecular sieve still has the problems of low silicon source utilization, difficult to control product size and morphology, and poor product dispersibility.

[0006] Therefore, it is of great significance to study and develop a method for preparing 13X molecular sieves with high silicon source utilization, easy control of product size and morphology, and good product dispersibility. Summary of the invention

[0007] The main purpose of the present invention is to provide a 13X molecular sieve and a preparation method thereof, so as to solve the problems of low silicon source utilization, difficult control of product size and morphology, and poor product dispersibility in the preparation method of the 13X molecular sieve in the prior art.

[0008] In order to achieve the above-mentioned purpose, the present invention provides a preparation method of 13X type molecular sieve on the one hand, and the preparation method comprises: step S1, performing a first crystallization treatment and a second crystallization treatment on a gel system containing a silicon source and an aluminum source in sequence to obtain a crystallized product system; wherein, the temperature of the first crystallization treatment is 20-60°C, the time is 4-24h, and the temperature of the second crystallization treatment is at least 20°C higher than the temperature of the first crystallization treatment, and the time is 6-48h; step S2, roasting a mixed system of inorganic waste and flux to obtain a roasted product; reacting the roasted product with an acid aqueous solution, and obtaining a filter residue and a first filtrate after a first solid-liquid separation; reacting the filter residue with an alkaline aqueous solution, and obtaining a second filtrate after a second solid-liquid separation; mixing the first filtrate with the second filtrate to obtain a mother liquor; wherein the inorganic waste comprises aluminum element, silicon element and oxygen element; step S3, mixing the crystallized product in the crystallized product system with the mother liquor, and obtaining a 13X type molecular sieve after aging and a third crystallization treatment in sequence.

[0009] Furthermore, the temperature of the second crystallization treatment is 20-100° C. higher than the temperature of the first crystallization treatment; preferably, the temperature of the second crystallization treatment is 80-120° C., and the time is 6-48 hours.

[0010] Further, the inorganic waste includes 10.5-38.5wt% aluminum, 8.4-37.3wt% silicon and 43.6-52.1wt% oxygen and the balance is other elements; preferably, the inorganic waste is selected from one or more of the group consisting of waste ZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst and waste VOC adsorbent.

[0011] Further, the preparation method of the gel system in step S1 includes: step S11, mixing a silicon source with a first solvent to obtain a silicon source dispersion; preferably, the mass concentration of the silicon source dispersion is 28 to 99 wt%; step S12, mixing an aluminum source with a second solvent to obtain an aluminum source dispersion; preferably, the mass concentration of the aluminum source dispersion is 15 to 99 wt%; step S13, mixing the silicon source dispersion with the aluminum source dispersion, and adjusting the pH to 8.5 to 12.5 after stirring to obtain a gel system; preferably, step S13 The method comprises: adding an aluminum source dispersion liquid dropwise to a silicon source dispersion liquid, and adjusting the pH value to 11.9-12.1 after stirring to obtain a gel system; preferably, the stirring temperature is 20-100° C., and the stirring time is 0.1-24 hours; preferably, the silicon source is selected from one or more of the group consisting of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash and white carbon black; preferably, the aluminum source is selected from one or more of the group consisting of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; preferably, the first solvent and the second solvent are selected from water.

[0012] Further, the crystallization product system includes SiO2 and Al2O3, and preferably the molar ratio of SiO2 to Al2O3 is (0.01-2.5):1; preferably, the crystallization product system also includes Na2O and H2O, and preferably the molar ratio of Na2O to SiO2 is (0.01-4.0):1; the molar ratio of H2O to SiO2 is (1.0-40.0):1.

[0013] Furthermore, the weight ratio of the inorganic waste to the flux is 1:(0.5 to 1:5).

[0014] Furthermore, the calcination temperature is 550-800° C. and the calcination time is 60-120 min.

[0015] Furthermore, the mass concentration of the acid aqueous solution is 10 to 35%.

[0016] Furthermore, the weight ratio of the filter residue, the alkaline compound in the alkali aqueous solution and the water in the alkali aqueous solution is (2-100):(40-60):(50-400); preferably, the flux is sodium carbonate; preferably, the acidic compound in the acid aqueous solution is a monobasic acid, and more preferably, the acidic compound in the acid aqueous solution is selected from nitric acid and / or hydrochloric acid; preferably, the alkaline compound in the alkali aqueous solution is selected from NaOH and / or KOH.

[0017] Furthermore, the mother liquor obtained in step S2 includes SiO2 and Al2O3, and preferably the molar ratio of SiO2 to Al2O3 is (0.5-6.0):1; preferably, the mother liquor also includes Na2O and H2O, and preferably the molar ratio of Na2O to SiO2 is (0.5-6.0):1; the molar ratio of H2O to SiO2 is (10-100):1.

[0018] Furthermore, the weight ratio of the crystallized product to the mother liquor in the crystallized product-containing system is (5-20):100.

[0019] Furthermore, the weight ratio of the first filtrate to the second filtrate is 1:(2.5-5.5).

[0020] Furthermore, in step S3, the aging temperature is 20 to 100° C., and the aging time is 0.1 to 24 hours.

[0021] Furthermore, the temperature of the third crystallization treatment is 60-150° C., and the time is 0.1-36 h; preferably, the temperature of the third crystallization treatment is 90-120° C., and the time is 18-30 h.

[0022] In order to achieve the above object, another aspect of the present invention further provides a 13X molecular sieve prepared by the preparation method of the 13X molecular sieve provided in the present application, wherein the silicon-aluminum ratio of the 13X molecular sieve is 2.2-2.9, and the pore volume is 0.35-0.5 cm 3 / g, specific surface area is 800~950m 2 / g.

[0023] By applying the technical solution of the present invention, compared with the conventional method of obtaining a crystallization product system by a single crystallization treatment, the above two-stage crystallization treatment of the gel system containing silicon source and aluminum source can effectively control the formation and growth of crystal seeds. The first stage of crystallization treatment is carried out under relatively low temperature and time conditions, which is conducive to the initial formation of crystal seeds. The second stage of crystallization treatment is carried out under higher temperature and time conditions, which is conducive to the further growth and improvement of crystal seeds, thereby improving the quality and controllability of crystal seeds. Moreover, the mother liquor obtained by treating the inorganic waste containing the above specific elements is mixed with the crystallization product system to prepare the 13X molecular sieve, which can improve the recovery rate of inorganic waste and improve its utilization value.

[0024] Compared with other ranges, the two-stage crystallization treatment of the gel system under the above-mentioned specific conditions (the temperature and time of the first crystallization treatment and the second crystallization treatment are within the above-mentioned range of the present application) is beneficial to more effectively control the growth rate and final size of the crystals, to improve the crystallinity and purity of the crystallization product, to the subsequent formation of a 13X molecular sieve with controllable morphology and size and a relatively wide silicon-aluminum ratio, and to improve its dispersibility.

[0025] Compared with the 13X molecular sieve prepared by the traditional method, the 13X molecular sieve prepared by the above-mentioned preparation method of the present application has better adsorption capacity and has a good application prospect in the field of shape-selective adsorption. DETAILED DESCRIPTION

[0026] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0027] As described in the background art, the existing preparation method of 13X molecular sieve has the problems of low silicon source utilization, difficult to control product size and morphology, and poor product dispersibility. In order to solve the above technical problems, the first aspect of the present application provides a preparation method of 13X type molecular sieve, which comprises: step S1, sequentially performing a first crystallization treatment and a second crystallization treatment on a gel system containing a silicon source and an aluminum source to obtain a system containing a crystallized product; wherein the temperature of the first crystallization treatment is 20 to 60°C, and the time is 4 to 24 hours, and the temperature of the second crystallization treatment is at least 20°C higher than the temperature of the first crystallization treatment, and the time is 6 to 48 hours; step S2, roasting a mixed system of inorganic waste and flux to obtain a roasted product; reacting the roasted product with an acid aqueous solution, and obtaining a filter residue and a first filtrate after a first solid-liquid separation; reacting the filter residue with an alkaline aqueous solution, and obtaining a second filtrate after a second solid-liquid separation; mixing the first filtrate with the second filtrate to obtain a mother liquor; wherein the inorganic waste comprises aluminum, silicon and oxygen; step S3, mixing the crystallized product in the crystallized product system with the mother liquor, and sequentially performing aging and a third crystallization treatment to obtain a 13X type molecular sieve.

[0028] Compared with the conventional method of obtaining a system containing a crystallized product by a single crystallization treatment, the above two-stage crystallization treatment of the gel system containing a silicon source and an aluminum source can effectively control the formation and growth of the crystal seeds. The first stage of crystallization treatment is carried out under relatively low temperature and time conditions, which is conducive to the initial formation of the crystal seeds. The second stage of crystallization treatment is carried out under higher temperature and time conditions, which is conducive to the further growth and improvement of the crystal seeds, thereby improving the quality and controllability of the crystal seeds. Moreover, the mother liquor obtained by treating the inorganic waste containing the above specific elements is mixed with the system containing the crystallized product to prepare the 13X molecular sieve, which can improve the recovery rate of the inorganic waste and improve its utilization value.

[0029] Compared with other ranges, the two-stage crystallization treatment of the gel system under the above-mentioned specific conditions (the temperature and time of the first crystallization treatment and the second crystallization treatment are within the above-mentioned range of the present application) is beneficial to more effectively control the growth rate and final size of the crystals, to improve the crystallinity and purity of the crystallization product, to the subsequent formation of a 13X molecular sieve with controllable morphology and size and a relatively wide silicon-aluminum ratio, and to improve its dispersibility.

[0030] Compared with the 13X molecular sieve prepared by the traditional method, the 13X molecular sieve prepared by the above-mentioned preparation method of the present application has better adsorption capacity and has a good application prospect in the field of shape-selective adsorption.

[0031] In a preferred embodiment, the temperature of the second crystallization treatment is 20 to 100° C. higher than the temperature of the first crystallization treatment. Compared with other ranges, limiting the temperature difference of the two crystallization treatments within the above range is conducive to making the adjustment of the silicon-aluminum ratio more flexible, facilitating the preparation of molecular sieves with different silicon-aluminum ratios as required, and facilitating the subsequent formation of a 13X molecular sieve with controllable morphology and size and a wide silicon-aluminum ratio, thereby facilitating the improvement of the comprehensive performance of the molecular sieve.

[0032] In a preferred embodiment, the temperature of the second crystallization treatment is 80-120°C and the time is 6-48 hours. Compared with other ranges, limiting the temperature and time of the second crystallization treatment within the above range is conducive to further improving the utilization rate of the silicon source, and is conducive to further forming a 13X molecular sieve with controllable morphology and size and a wide silicon-aluminum ratio, and is also conducive to further improving its dispersibility.

[0033] In order to further improve the recycling rate of inorganic waste, preferably, the inorganic waste includes 10.5-38.5 wt% aluminum, 8.4-37.3 wt% silicon, 43.6-52.1 wt% oxygen and the balance other elements.

[0034] Inorganic waste materials in the present application include but are not limited to one or more of the group consisting of waste ZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst and waste VOC adsorbent. Using the above types of inorganic waste materials is conducive to improving their recyclable value.

[0035] In a preferred embodiment, the preparation method of the gel system in step S1 includes: step S11, mixing a silicon source with a first solvent to obtain a silicon source dispersion; preferably, the mass concentration of the silicon source dispersion is 28-99wt%; step S12, mixing an aluminum source with a second solvent to obtain an aluminum source dispersion; preferably, the mass concentration of the aluminum source dispersion is 15-99wt%; step S13, mixing the silicon source dispersion with the aluminum source dispersion, and adjusting the pH to 8.5-12.5 after stirring to obtain a gel system. The preparation method of the gel system is used to facilitate the formation of seed crystals after the subsequent two-stage crystallization treatment, which is beneficial to accelerate the growth of seed crystals, thereby obtaining a system containing a crystallization product, which is beneficial to the subsequent formation of a molecular sieve of a specific crystal form of the present application.

[0036] In order to improve the uniformity of the gel system and facilitate the subsequent two-stage crystallization treatment, preferably, the stirring temperature is 20 to 100° C. and the stirring time is 0.1 to 24 h.

[0037] In a preferred embodiment, step S13 includes: adding the aluminum source dispersion dropwise to the silicon source dispersion, and adjusting the pH to 11.9 to 12.1 after stirring to obtain a gel system. Compared with pouring the aluminum source dispersion into the silicon source dispersion, adding the aluminum source dispersion dropwise to the silicon source dispersion is beneficial to improving the crystallinity and purity of the crystallized product, and adjusting the pH within the above range is beneficial to accelerating the crystallization rate of the subsequent two-stage crystallization treatment, shortening the crystallization time, and facilitating the subsequent formation of the molecular sieve of the specific crystal form of the present application.

[0038] The silicon source and aluminum source in the present application can be any of the commonly used ones in the art. In a preferred embodiment, the silicon source includes but is not limited to one or more of the group consisting of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash and white carbon black; the aluminum source includes but is not limited to one or more of the group consisting of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate.

[0039] In the present application, the first solvent and the second solvent may be commonly used in the art. In a preferred embodiment, the first solvent and the second solvent include but are not limited to water.

[0040] In a preferred embodiment, the crystallization product system includes SiO2 and Al2O3, and the molar ratio of SiO2 to Al2O3 is preferably (0.01-2.5): 1. Compared with other ranges, limiting the molar ratio of SiO2 to Al2O3 in the crystallization product system to the above range is conducive to the subsequent formation of a specific crystal form of 13X molecular sieve.

[0041] In a preferred embodiment, the crystallization product system further comprises Na2O and H2O, and preferably the molar ratio of Na2O to SiO2 is (0.01-4.0):1; the molar ratio of H2O to SiO2 is (1.0-40.0):1. Compared with other ranges, limiting the molar ratio of Na2O to SiO2 and the molar ratio of H2O to SiO2 in the crystallization product system to the above ranges is conducive to the subsequent formation of a specific crystal form of 13X molecular sieve.

[0042] In a preferred embodiment, the weight ratio of inorganic waste to flux is 1:(0.5-1:5). The weight ratio of inorganic waste to flux includes but is not limited to the above range, and limiting it within the above range is conducive to improving the processability of inorganic waste, thereby facilitating the utilization of Al, Si and O elements therein, and further facilitating the improvement of its recycling rate.

[0043] In a preferred embodiment, the calcination temperature is 550-800°C and the time is 60-120 minutes. The calcination temperature and time include but are not limited to the above ranges, and limiting them within the above ranges is conducive to improving the leaching rate of Al and Si elements, thereby facilitating the increase of the Al content in the first filtrate and the Si content in the second filtrate, and further facilitating better performance of the mother liquor.

[0044] In a preferred embodiment, the mass concentration of the acid aqueous solution is 10-35%. Compared with other ranges, limiting the mass concentration of the acid aqueous solution within the above range is conducive to increasing the leaching rate of the Al element, thereby increasing the Al element content in the first filtrate, and further facilitating better performance of the mother liquor.

[0045] In order to further improve the leaching rate of Al element, preferably, the acidic compound in the acid aqueous solution is a monobasic acid, and more preferably, the acidic compound in the acid aqueous solution includes but is not limited to nitric acid and / or hydrochloric acid.

[0046] In a preferred embodiment, the weight ratio of the filter residue, the alkaline compound in the alkali aqueous solution, and the water in the alkali aqueous solution is (2-100): (40-60): (50-400). Compared with other ranges, limiting the weight ratio of the filter residue, the alkaline compound in the alkali aqueous solution, and the water in the alkali aqueous solution to the above range is conducive to improving the leaching rate of the Si element, thereby helping to improve the utilization rate of the filter residue and the Si element content in the second filtrate, and further helping to better play the role of the mother liquor.

[0047] In order to further improve the leaching rate of Si element, preferably, the alkaline compound in the alkaline aqueous solution includes but is not limited to NaOH and / or KOH.

[0048] In order to improve the processability of inorganic waste and facilitate its processing and reuse, preferably, the flux is sodium carbonate.

[0049] In a preferred embodiment, the mother liquor obtained in step S2 includes SiO2 and Al2O3, and preferably the molar ratio of SiO2 to Al2O3 is (0.5-6.0): 1. Compared with other ranges, limiting the molar ratio of SiO2 to Al2O3 in the mother liquor to the above range is conducive to the subsequent formation of a specific crystal form of 13X molecular sieve.

[0050] In a preferred embodiment, the mother liquor further comprises Na2O and H2O, preferably the molar ratio of Na2O to SiO2 is (0.5-6.0):1; the molar ratio of H2O to SiO2 is (10-100):1. Compared with other ranges, limiting the molar ratio of Na2O to SiO2 and the molar ratio of H2O to SiO2 in the mother liquor to the above range is conducive to the subsequent formation of a specific crystal form of 13X molecular sieve.

[0051] In a preferred embodiment, the weight ratio of the crystallized product to the mother liquor in the crystallized product-containing system is (5-20): 100. The weight ratio of the crystallized product to the mother liquor includes but is not limited to the above range, and limiting it within the above range is beneficial to improving the utilization rate of silicon source, aluminum source and inorganic waste, facilitating subsequent aging and third crystallization treatment, and is beneficial to forming a specific crystal form of 13X molecular sieve.

[0052] In a preferred embodiment, in step S3, the aging temperature is 20-100° C. and the aging time is 0.1-24 hours. The aging temperature and time include but are not limited to the above ranges, and limiting them within the above ranges facilitates the subsequent third crystallization treatment, and is also beneficial to increase the adsorption sites of the prepared 13X molecular sieve and increase its internal pore volume.

[0053] In a preferred embodiment, in step S3, the temperature of the third crystallization treatment is 60-150°C, and the time is 0.1-36h; preferably, the temperature of the third crystallization treatment is 90-120°C, and the time is 18-30h. The temperature and time of the third crystallization treatment include but are not limited to the above ranges. Limiting it within the above range is beneficial to improving the crystal purity of the obtained molecular sieve, reducing impurity components, and also beneficial to increasing the adsorption sites of the obtained 13X molecular sieve, increasing its internal pore volume, thereby improving its adsorption performance and broadening its application in the field of shape-selective adsorption.

[0054] The second aspect of the present application also provides a 13X molecular sieve prepared by a method for preparing a 13X molecular sieve, wherein the 13X molecular sieve has a silicon-aluminum ratio of 2.2 to 2.9 and a pore volume of 0.35 to 0.5 cm 3 / g, specific surface area is 800~950m 2 The 13X molecular sieve provided in the present application has a higher silicon-aluminum ratio, a larger pore volume and specific surface area, and also has a better adsorption capacity, and has a good application prospect in the field of shape-selective adsorption.

[0055] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0056] Example 1

[0057] A method for preparing a 13X molecular sieve comprises the following steps:

[0058] (1) 21.0 g of silica sol (mass fraction of 30%) was dissolved in 36.0 g of deionized water, and pretreated in a sealed reactor at 25° C. for 1 h to obtain a silicon source dispersion; 24 g of aluminum sulfate was dissolved in 18.0 g of deionized water, and stirred at 25° C. for 1 h to obtain an aluminum source dispersion; the aluminum source dispersion was slowly added dropwise to the silicon source dispersion, and the addition was completed in 0.8 h, and the stirring was continued at 60° C. for 8 h to obtain a mixed system; 6.74 g of sodium hydroxide was dissolved in 36 g of deionized water, and the mixture was obtained. to a NaOH aqueous solution, and adding the NaOH aqueous solution to the mixed system until the pH value is 12 to obtain a gel system; placing it in a hydrothermal reactor and performing two-stage temperature-controlled crystallization, the first stage crystallization temperature is 40°C, the time is 12h, the second stage crystallization temperature is 95°C, the time is 24h, and a crystallization product system is obtained (wherein the molar ratio of each component is: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1);

[0059] (2) preparing a waste ZSM-5 molecular sieve catalyst having the composition shown in Table 1 as an inorganic waste;

[0060] Table 1

[0061] <![CDATA[Fe2O3 / wt%]]> <![CDATA[Al2O3 / wt%]]> <![CDATA[SiO2 / wt%]]> <![CDATA[SO3 / wt%]]> CaO / wt% Spent ZSM-5 molecular sieve catalyst 0.050 19.84 79.64 0.31 0.18

[0062] The above 10g, 200-mesh waste ZSM-5 molecular sieve catalyst was mixed with 8g Na2CO3, and calcined at 650°C for 120min to obtain a calcined product; then the calcined product was dissolved and filtered with a nitric acid solution with a mass fraction of 25% to obtain an aluminum-rich liquid (i.e., the first filtrate) with an Al element content of 1.2 mol / L and a residue; 10g of the above residue was mixed with 6g NaOH and 40g water, and filtered to obtain a silicon-rich liquid (i.e., the second filtrate) with an Si element content of 2 mol / L; the silicon-rich liquid and the aluminum-rich liquid were mixed at a weight ratio of 4:1 to obtain a mother liquor; the molar ratio of SiO2 to Al2O3 in the mother liquor was 3.5:1, the molar ratio of Na2O to SiO2 was 2.8:1, and the molar ratio of H2O to the SiO2 was 80:1;

[0063] (3) Take 25 g of the crystallized product obtained in step (1) and add it to the mother liquor obtained in step (2), age it at 60°C for 12 hours, and place it in a hydrothermal reactor for a third crystallization treatment, wherein the temperature of the third crystallization treatment is 98°C and the time is 24 hours; filter and wash until the pH is 7, and dry it at 90°C to obtain a 13X molecular sieve.

[0064] Example 2

[0065] Step (1) is the same as in Example 1.

[0066] The difference from Example 1 is that: waste 13X adsorbent with the composition shown in Table 2 is prepared instead of waste ZSM-5 molecular sieve catalyst as inorganic waste;

[0067] Table 2

[0068] <![CDATA[Fe2O3 / wt%]]> <![CDATA[Al2O3 / wt%]]> <![CDATA[SiO2 / wt%]]> <![CDATA[K2O / wt%]]> CaO / wt% Waste 13X adsorbent 0.020 72.36 18.0 0.024 0.042

[0069] (2) 12 g of the above-mentioned 200-mesh waste 13X adsorbent was mixed with 10 g of Na2CO3 and calcined at 650°C for 120 min to obtain a calcined product; the calcined product was then dissolved and filtered with a 15% by mass nitric acid solution to obtain an aluminum-rich liquid (i.e., the first filtrate) and a residue having an Al element content of 1.5 mol / L; 15 g of the above-mentioned residue was mixed with 6 g of NaOH and 40 g of water, and filtered to obtain a silicon-rich liquid (i.e., the second filtrate) having an Si element content of 0.8 mol / L; the silicon-rich liquid and the aluminum-rich liquid were mixed at a weight ratio of 3.5:1 to obtain a mother liquor; the molar ratio of SiO2 to Al2O3 in the mother liquor was 1.8:1, the molar ratio of Na2O to SiO2 was 4.5:1, and the molar ratio of H2O to the SiO2 was 50:1;

[0070] (3) Take 15 g of the crystallized product obtained in step (1) and add it to the mother liquor obtained in step (2), age it at 60°C for 12 h, and place it in a hydrothermal reactor for a third crystallization treatment, wherein the temperature of the third crystallization treatment is 95°C and the time is 24 h; filter and wash until the pH is 7, and dry it at 90°C to obtain a 13X molecular sieve.

[0071] Example 3

[0072] Step (1) is the same as in Example 1.

[0073] The difference from Example 1 is that a mixture of the waste 13X adsorbent shown in Table 1 and the waste ZSM-5 molecular sieve catalyst described in Table 2 is used as the inorganic waste material;

[0074] The above-mentioned 5g, 200-mesh waste ZSM-5 molecular sieve catalyst and 6g, 200-mesh waste 13X adsorbent and 15g Na2CO3 were mixed, and calcined at 650°C for 120min to obtain a calcined product; then the calcined product was dissolved and filtered with a nitric acid solution with a mass fraction of 15% to obtain an aluminum-rich liquid (i.e., the first filtrate) with an Al element content of 1.2 mol / L and a residue; 15g of the above-mentioned residue was mixed with 8g NaOH and 45g water, and after filtering, a silicon-rich liquid (i.e., the second filtrate) with an Si element content of 2 mol / L was obtained; the silicon-rich liquid with a weight ratio of 5.5:1 was mixed with the aluminum-rich liquid to obtain a mother liquor; the molar ratio of SiO2 to Al2O3 in the mother liquor was 0.5:1, the molar ratio of Na2O to SiO2 was 6:1, and the molar ratio of H2O to the SiO2 was 10:1;

[0075] (3) Take 20 g of the crystallized product obtained in step (1) and add it to the mother liquor obtained in step (2), age it at 60°C for 12 hours, and place it in a hydrothermal reactor for a third crystallization treatment, wherein the temperature of the third crystallization treatment is 105°C and the time is 20 hours; filter and wash until the pH is 7, and dry it at 90°C to obtain a 13X molecular sieve.

[0076] Example 4

[0077] Step (1) is the same as in Example 1.

[0078] The difference from Example 1 is that: in step (2), the weight ratio of the silicon-rich liquid to the aluminum-rich liquid is 2.5:1; in step (3), 30 g of the crystallized product obtained in step (1) is added to the mother liquor obtained in step (2), aged at 70°C for 152 hours, and placed in a hydrothermal reactor for a third crystallization treatment, wherein the temperature of the third crystallization treatment is 115°C and the time is 16 hours; the pH after filtration and washing is 7, and the 13X molecular sieve is obtained by drying at 90°C.

[0079] Example 5

[0080] The difference from Example 1 is that in step (1), the temperature of the first crystallization treatment is 20°C, and the temperature of the second crystallization treatment is 40°C.

[0081] Example 6

[0082] The difference from Example 1 is that in step (1), the temperature of the first crystallization treatment is 60°C, and the temperature of the second crystallization treatment is 80°C.

[0083] Example 7

[0084] The difference from Example 1 is that the temperature of the third crystallization treatment in step (3) is 60° C. and the time is 36 hours.

[0085] Example 8

[0086] The difference from Example 1 is that the temperature of the third crystallization treatment in step (3) is 115° C. and the time is 0.1 h.

[0087] Example 9

[0088] The difference from Example 1 is that the temperature of the third crystallization treatment in step (3) is 150°C.

[0089] Comparative Example 1

[0090] The difference from Example 1 is that: step (1) does not adopt two-stage crystallization treatment, but adopts one-stage crystallization treatment to obtain a seed solution, wherein the temperature of one stage crystallization treatment is 40°C and the time is 12h; the temperature of the crystallization treatment in step (3) is 100°C.

[0091] Comparative Example 2

[0092] The difference from Example 1 is that: step (1) is omitted; in step (2), the weight ratio of silicon-rich liquid to aluminum-rich liquid is 9.5:1 to obtain a mother liquor; step (3) comprises: aging the mother liquor obtained in step (2) at 70°C for 15 hours, placing it in a hydrothermal reactor for crystallization treatment, wherein the crystallization temperature is 105°C and the crystallization time is 20 hours; the pH after filtration and washing is 7, and drying at 90°C to obtain a 13X molecular sieve.

[0093] Comparative Example 3

[0094] The difference from Example 1 is that: step (1) is completely different from Example 1, and no two-stage crystallization treatment is performed, and step (2) is completely different from Example 1, and no silicon-rich liquid and aluminum-rich liquid are used to prepare the mother liquor; specifically, Comparative Example 3 adopts the following method to prepare 13X molecular sieve: 12.5g of pseudo-boehmite is dissolved in 25.0g of deionized water, and stirred at 25°C for 1h to obtain an aluminum source dispersion, 100.0g of water glass (mass fraction is 28%) is dissolved in 18.0g of deionized water to obtain a silicon source dispersion; the silicon source dispersion is added dropwise to the aluminum source dispersion at a rate of 1mL / min, and stirring is continued at 45°C for 24h to obtain a mixed system; 20.2g of NaOH was dissolved in 15 g of deionized water and added to the mixed system, and the pH value was controlled to be maintained at 13.0 to obtain a system to be crystallized; the system to be crystallized was transferred to a hydrothermal reactor for temperature-controlled crystallization, the crystallization temperature was 100°C, and the time was 18 h; the reaction product was filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.

[0095] Comparative Example 4

[0096] The difference from Example 1 is that in step (1), the temperature of the first crystallization treatment is 70°C, and the temperature of the second crystallization treatment is 75°C.

[0097] Table 3 lists the BET surface area, pore volume, BJH adsorption average pore diameter and silicon source conversion rate of the molecular sieves prepared in the above examples and comparative examples of the present application. It should be noted that in Table 3, micropores refer to pores with a pore diameter of less than 2 nm, and mesopores refer to pores of 2 to 50 nm.

[0098] Table 3

[0099]

[0100] From the above description, it can be seen that the above-mentioned embodiments of the present invention achieve the following technical effects: Compared with the conventional method of obtaining a system containing a crystallization product by a one-stage crystallization treatment, the above-mentioned two-stage crystallization treatment of the gel system containing a silicon source and an aluminum source can effectively control the formation and growth of crystal seeds. The first stage of crystallization treatment is carried out under relatively low temperature and time conditions, which is conducive to the initial formation of crystal seeds. The second stage of crystallization treatment is carried out under higher temperature and time conditions, which is conducive to the further growth and improvement of the crystal seeds, thereby improving the quality and controllability of the crystal seeds. Moreover, the mother liquor obtained by treating the inorganic waste containing the above-mentioned specific elements is mixed with the system containing the crystallization product to prepare a 13X molecular sieve, which can improve the recovery rate of the inorganic waste and improve its utilization value.

[0101] Compared with other ranges, the two-stage crystallization treatment of the gel system under the above-mentioned specific conditions (the temperature and time of the first crystallization treatment and the second crystallization treatment are within the above-mentioned range of the present application) is beneficial to more effectively control the growth rate and final size of the crystals, to improve the crystallinity and purity of the crystallization product, to the subsequent formation of a 13X molecular sieve with controllable morphology and size and a relatively wide silicon-aluminum ratio, and to improve its dispersibility.

[0102] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a 13X molecular sieve, characterized in that: The preparation method comprises: Step S1, sequentially performing a first crystallization treatment and a second crystallization treatment on a gel system containing a silicon source and an aluminum source to obtain a crystallized product system; wherein the temperature of the first crystallization treatment is 20 to 60° C., and the time is 4 to 24 hours, and the temperature of the second crystallization treatment is at least 20° C. higher than the temperature of the first crystallization treatment, and the time is 6 to 48 hours; Step S2, roasting the mixed system of inorganic waste and flux to obtain a roasting product; reacting the roasting product with an acid aqueous solution to obtain a filter residue and a first filtrate after a first solid-liquid separation; reacting the filter residue with an alkaline aqueous solution to obtain a second filtrate after a second solid-liquid separation; mixing the first filtrate with the second filtrate to obtain a mother liquor; wherein the inorganic waste includes aluminum, silicon and oxygen; Step S3, mixing the crystallized product in the crystallized product-containing system with the mother liquor, and subjecting the mixture to aging and a third crystallization treatment to obtain the 13X molecular sieve.

2. The method for preparing 13X molecular sieve according to claim 1, characterized in that: The temperature of the second crystallization treatment is 20 to 100° C. higher than the temperature of the first crystallization treatment; Preferably, the temperature of the second crystallization treatment is 80-120° C., and the time is 6-48 hours.

3. The method for preparing 13X molecular sieve according to claim 1, characterized in that: The inorganic waste material comprises 10.5-38.5wt% aluminum, 8.4-37.3wt% silicon, 43.6-52.1wt% oxygen and the remainder other elements; Preferably, the inorganic waste is selected from one or more of the group consisting of waste ZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst and waste VOC adsorbent.

4. The method for preparing a 13X molecular sieve according to any one of claims 1 to 3, characterized in that: The preparation method of the gel system in step S1 comprises: Step S11, mixing a silicon source with a first solvent to obtain a silicon source dispersion; preferably, the mass concentration of the silicon source dispersion is 28 to 99 wt %; Step S12, mixing the aluminum source with the second solvent to obtain an aluminum source dispersion liquid; preferably, the mass concentration of the aluminum source dispersion liquid is 15 to 99 wt %; Step S13, mixing the silicon source dispersion liquid and the aluminum source dispersion liquid, adjusting the pH to 8.5-12.5 after stirring, to obtain the gel system; Preferably, the step S13 comprises: adding the aluminum source dispersion liquid dropwise to the silicon source dispersion liquid, adjusting the pH to 11.9-12.1 after stirring, to obtain the gel system; Preferably, the stirring temperature is 20 to 100° C. and the stirring time is 0.1 to 24 h; Preferably, the silicon source is selected from one or more of the group consisting of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash and white carbon black; Preferably, the aluminum source is selected from one or more of the group consisting of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; Preferably, the first solvent and the second solvent are selected from water.

5. The method for preparing 13X molecular sieve according to claim 4, characterized in that: The crystallization product system includes SiO2 and Al2O3, and preferably the molar ratio of SiO2 to Al2O3 is (0.01-2.5):1; Preferably, the crystallization product system further comprises Na2O and H2O, and preferably, the molar ratio of the Na2O to the SiO2 is (0.01-4.0):1; the molar ratio of the H2O to the SiO2 is (1.0-40.0):

1.

6. The method for preparing a 13X molecular sieve according to any one of claims 1 to 5, characterized in that: The weight ratio of the inorganic waste to the flux is 1:(0.5-1:5); and / or, The calcination temperature is 550-800°C and the calcination time is 60-120 min; and / or, The mass concentration of the acid aqueous solution is 10 to 35%; and / or, The weight ratio of the filter residue, the alkaline compound in the alkaline aqueous solution and the water in the alkaline aqueous solution is (2-100):(40-60):(50-400); Preferably, the flux is sodium carbonate; Preferably, the acidic compound in the acid aqueous solution is a monoacid, and more preferably the acidic compound in the acid aqueous solution is selected from nitric acid and / or hydrochloric acid; Preferably, the alkaline compound in the aqueous alkaline solution is selected from NaOH and / or KOH.

7. The method for preparing 13X molecular sieve according to claim 6, characterized in that: The mother liquor obtained in step S2 comprises SiO2 and Al2O3, and preferably the molar ratio of SiO2 to Al2O3 is (0.5-6.0):1; Preferably, the mother liquor further comprises Na2O and H2O, and preferably the molar ratio of the Na2O to the SiO2 is (0.5-6.0):1; the molar ratio of the H2O to the SiO2 is (10-100):

1.

8. The method for preparing 13X molecular sieve according to claim 7, characterized in that: The weight ratio of the crystallized product in the crystallized product-containing system to the mother liquor is (5-20):100; and / or, The weight ratio of the first filtrate to the second filtrate is 1:(2.5-5.5).

9. The method for preparing 13X molecular sieve according to claim 7 or 8, characterized in that: In step S3, the aging temperature is 20-100° C. and the time is 0.1-24 h; and / or, The temperature of the third crystallization treatment is 60-150° C., and the time is 0.1-36 h; preferably, the temperature of the third crystallization treatment is 90-120° C., and the time is 18-30 h.

10. A 13X molecular sieve obtained by the method for preparing a 13X molecular sieve according to any one of claims 1 to 9, characterized in that: The 13X molecular sieve has a silicon-aluminum ratio of 2.2 to 2.9 and a pore volume of 0.35 to 0.5 cm 3 / g, specific surface area is 800~950m 2 / g.

Citation Information

Patent Citations

  • NaX zeolite molecular sieve and preparation method thereof

    CN104355317A

  • 13X zeolite molecular sieve, preparation method therefor and application of 13X zeolite molecular sieve

    CN106542542A

  • Preparation method for efficiently synthesizing 13X-type molecular sieve from calcined kaolin by microwave-assisted hydrothermal method

    CN108726533A

  • 13X molecular sieve synthesis method and 13X molecular sieve

    CN115838180A

  • Coal gangue-based NaX type molecular sieve as well as preparation method and application thereof

    CN117509661A