13X molecular sieve with core-shell structure and preparation method thereof
By forming a nickel nanoparticle layer and a titanium silicon shell on the surface of the 13X molecular sieve to form a core-shell structure, the problem of insufficient performance of the existing 13X molecular sieve is solved, and its adsorption ability in olefin purification and catalytic cracking is improved.
Patent Information
- Application Number
- CN202410976176.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing 13X molecular sieve has poor performance and small surface area, making it difficult to meet the needs of large-scale industrial applications, especially in olefin purification and catalytic cracking, which is difficult to effectively remove oxygen-containing compound impurities.
Using a 13X molecular sieve preparation method with a core-shell structure, a nickel nanoparticle layer and a titanium silicon shell are formed on the surface of the 13X molecular sieve, a metal-carrier interaction is used to form a metal organic framework structure, which improves mechanical strength and thermal stability, and increases the Large specific surface area and pore volume.
It significantly improves the performance of the 13X molecular sieve, increases the specific surface area and pore volume, improves the adsorption capacity, and expands its application range in the field of shape-selective adsorption.
Smart Images

Figure BDA0004954577730000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of molecular sieve preparation, and in particular to a 13X molecular sieve with a core-shell structure and a preparation method thereof. Background Art
[0002] Molecular sieve is a kind of aluminosilicate material with uniform pore size, regular crystal structure, rich pore system, large specific surface area and good thermal stability. In particular, X-type molecular sieve has shown good performance in olefin purification and can effectively remove oxygen-containing compound impurities.
[0003] Adsorption separation is widely used in petroleum cracking and refinery catalytic cracking, mainly for removing oxygenated substances from hydrocarbons. In addition, the hydrocarbon products produced by indirect liquefaction of coal through Fischer-Tropsch synthesis have different carbon number distributions, and there are many types of oxygenated compounds in each carbon number product. Therefore, molecular sieves with uniform and orderly micropores, large specific surface area, large adsorption capacity and low adsorption heat are needed to meet the needs of adsorption separation. However, the 13X molecular sieve in the prior art has a small surface area and poor performance, which is difficult to meet the needs of large-scale industrial applications. Therefore, the improvement of molecular sieves has broad application prospects. Summary of the invention
[0004] The main purpose of the present invention is to provide a 13X molecular sieve with a core-shell structure and a preparation method thereof, so as to solve the problem that the 13X molecular sieve prepared by the preparation method of the prior art has poor performance.
[0005] In order to achieve the above-mentioned purpose, according to the first aspect of the present invention, there is provided a method for preparing a 13X molecular sieve with a core-shell structure, the method comprising: subjecting the 13X molecular sieve to a first immersion in a first solution and then filtering to obtain a first solid; subjecting the first solid to a second immersion in a second solution and then first calcining to obtain a 13X molecular sieve containing a nickel nanoparticle layer; mixing the 13X molecular sieve containing the nickel nanoparticle layer with a precursor solution, and sequentially incubating, drying and second calcining to obtain a 13X molecular sieve with a core-shell structure; wherein the precursor solution comprises a titanium silicon molecular sieve precursor solution.
[0006] Further, the first solution includes any one or more of the following aqueous solutions: 3-aminopropyltriethoxysilane, tetraethoxysilane or tetramethoxysilane; preferably, the first impregnation time is 6-15h; preferably, the concentration of the first solution is 0.05-0.2mol / L; preferably, the second solution includes any one or more of the following aqueous solutions: nickel nitrate and / or nickel sulfate; preferably, the second impregnation time is 12-48h; preferably, the concentration of the second solution is 0.01-0.2M. Preferably, the first calcination includes: performing the first calcination in a gas atmosphere; preferably, the gas atmosphere includes a hydrogen atmosphere; preferably, the temperature of the first calcination is 200-1000°C and the time is 1-8h.
[0007] Furthermore, the titanium silicon molecular sieve precursor solution includes: silicon dioxide, titanium dioxide, a template, a fluorine complex and water; preferably, the molar ratio of silicon dioxide to titanium dioxide is 1:(0.04-0.1); preferably, the molar ratio of silicon dioxide to the template is 1:(0.1-0.3); preferably, the molar ratio of silicon dioxide to the fluorine complex is 1:(0.04-0.1); preferably, the molar ratio of silicon dioxide to water is 1:(20-50); preferably, the template includes organic amines and / or quaternary ammonium salts; preferably, the fluorine complex includes any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate or ammonium fluoride.
[0008] Further, the incubation temperature is 100-500° C., and the time is 5-20 h; preferably, the drying temperature is 80-200° C., and the time is 5-20 h; preferably, the second calcination temperature is 300-600° C., and the time is 2-10 h.
[0009] Further, the preparation method of 13X molecular sieve includes: subjecting a gel system containing a silicon source and an aluminum source to a first crystallization treatment and a second crystallization treatment in sequence to obtain a crystallized product; mixing the crystallized product with a gel mother liquor, and subjecting the crystallized product to an aging treatment and a third crystallization treatment in sequence to obtain a 13X molecular sieve; preferably, the preparation method of 13X molecular sieve includes: S1) dispersing a silicon source in water to obtain a silicon source dispersion; dispersing an aluminum source in water to obtain an aluminum source dispersion; S2) mixing the silicon source dispersion with the aluminum source dispersion, and adjusting the pH to 8.5 to 12.5 after stirring to obtain a gel system; S3) subjecting the gel system to a first crystallization treatment and a third crystallization treatment in sequence The crystallization product is subjected to a second crystallization treatment to obtain a crystallized product; S4) the crystallized product and the gel mother liquor are subjected to an aging treatment and a third crystallization treatment in sequence to obtain a 13X molecular sieve; preferably, in S1), the mass concentration of the silicon source dispersion is 28-99wt%; preferably, the silicon source comprises one or more of silica sol, tetraethyl orthosilicate, coarse-pore silica gel, silicon powder, fly ash or white carbon black; preferably, the mass concentration of the aluminum source dispersion is 15-99wt%; preferably, the aluminum source comprises one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; preferably, in S2), the stirring temperature is 20-100°C and the time is 0.1-24h.
[0010] Further, in S3), the temperature of the second crystallization treatment is 20 to 100°C higher than the temperature of the first crystallization treatment; preferably, the temperature of the first crystallization treatment is 20 to 60°C, and the time is 10 to 18 hours; preferably, the temperature of the second crystallization treatment is 80 to 120°C, and the time is 6 to 48 hours; preferably, the components in the crystallization product include silicon dioxide, aluminum oxide, sodium oxide and water; preferably, the molar ratio of silicon dioxide to aluminum oxide is 0.01 to 2.5:1; preferably, the molar ratio of sodium oxide to silicon dioxide is 0.01 to 4.0:1; preferably, the molar ratio of water to silicon dioxide is 1.0 to 40.0:1.
[0011] Further, in S4), the preparation method of the gel mother liquor comprises: subjecting the mixed system of inorganic waste and flux to a third calcination to obtain a third calcination product; mixing the third calcination product with an acid solution, and obtaining a filter residue and a first filtrate after a first solid-liquid separation; mixing the filter residue with an alkaline solution, and obtaining a second filtrate after a second solid-liquid separation; mixing the first filtrate with the second filtrate to obtain a gel mother liquor; preferably, the inorganic waste comprises one or more of waste ZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst or waste VOC adsorbent; preferably, the temperature of the aging treatment is 20 to 100°C, and the time is 0.1 to 24h; preferably, the temperature of the third crystallization treatment is 60 to 105°C, and the time is 0.1 to 36h; preferably, the mass ratio of the crystallization product to the gel mother liquor is 5 to 20:100.
[0012] Furthermore, the mass ratio of inorganic waste to flux is 1:0.5-1:5; preferably, the temperature of the third roasting is 550-800°C and the time is 60-120min; preferably, the mass concentration of the acid solution is 10%-35%; preferably, the flux comprises sodium carbonate and / or sodium sulfate; preferably, the acid in the acid solution is a monobasic acid, more preferably hydrochloric acid and / or nitric acid; preferably, the alkali in the alkali solution comprises sodium hydroxide and / or potassium hydroxide; preferably, the mass ratio of the filter residue, the alkali and the water is is 0.1-100:40-60:50-400; preferably, the mass ratio of the first filtrate to the second filtrate is 1:(2.5-5.5); preferably, the components in the gel mother liquor include silicon dioxide, aluminum oxide, sodium oxide and water; preferably, the molar ratio of silicon dioxide to aluminum oxide is (0.5-6.0):1; preferably, the molar ratio of sodium oxide to silicon dioxide is (0.5-6.0):1; preferably, the molar ratio of water to silicon dioxide is (10-100):1.
[0013] Furthermore, the silicon-aluminum ratio of the 13X molecular sieve with a core-shell structure is 2.4-3.1, and the pore volume is 0.37-0.58 cm 3 / g, specific surface area is 850~1000m 2 / g.
[0014] In order to achieve the above object, according to a second aspect of the present invention, a method for preparing any one of the above 13X molecular sieves with a core-shell structure is provided to obtain a 13X molecular sieve with a core-shell structure, wherein the silicon-aluminum ratio of the 13X molecular sieve with a core-shell structure is 2.4 to 3.1, and the pore volume is 0.37 to 0.58 cm 3 / g, specific surface area is 850~1000m 2 / g.
[0015] By applying the technical scheme of the present invention, a first solid obtained by impregnating and filtering a 13X molecular sieve with a first solution is impregnated in a second solution, and a first calcination is performed after the reaction is complete to obtain a 13X molecular sieve containing a nickel nanoparticle layer; the 13X molecular sieve containing the nickel nanoparticle layer is mixed with a titanium silicon molecular sieve precursor solution and the mixture is heated, dried and calcined in sequence to obtain a 13X molecular sieve having both a nickel nanoparticle layer and a titanium silicon shell. The core-shell structure has a larger surface area, thereby improving the performance of the 13X molecular sieve in the prior art. DETAILED DESCRIPTION
[0016] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0017] As mentioned in the background technology, the size and morphology of the 13X molecular sieve prepared in the prior art are difficult to control, and the dispersibility is poor. Therefore, in the present application, the inventor attempts to develop a new method for preparing a 13X molecular sieve with a core-shell structure, and thus proposes a series of protection schemes of the present application.
[0018] In a first typical embodiment of the present application, a method for preparing a 13X molecular sieve with a core-shell structure is provided, the preparation method comprising: subjecting the 13X molecular sieve to a first immersion in a first solution and then filtering to obtain a first solid; subjecting the first solid to a second immersion in a second solution and then first calcining to obtain a 13X molecular sieve containing a nickel nanoparticle layer; mixing the 13X molecular sieve containing the nickel nanoparticle layer with a precursor solution, and sequentially incubating, drying and second calcining to obtain a 13X molecular sieve with a core-shell structure; wherein the precursor solution comprises a titanium silicon molecular sieve precursor solution.
[0019] In the prior art, the performance of the molecular sieve is improved by adding a core-shell structure outside the molecular sieve, usually by adding an outer shell without changing the properties of the molecular sieve. The nickel nanoparticle layer has good dispersion stability, and the titanium silicon outer shell has the characteristics of good pore penetration. However, it is difficult to cross-link the nickel nanoparticle layer and the titanium silicon outer shell in the prior art, and it is impossible to obtain a core-shell structure that is compatible with the advantages of the two outer layers (shells).
[0020] The present application can form a nickel nanoparticle intermediate layer and a titanium silicon molecular sieve shell on the surface of the 13X molecular sieve in sequence through the first impregnation treatment and the second impregnation treatment to form a core-shell gradient structure, which helps to improve the mechanical strength and thermal stability of the 13X molecular sieve. In this process, the structure of the 13X molecular sieve is optimized so that the resulting core-shell structure 13X molecular sieve has a certain range of parameters such as specific surface area and porosity. The present application interacts the nickel nanoparticles of the titanium silicon molecular sieve precursor solution with the nickel nanoparticles of the nickel nanolayer on the surface of the 13X molecular sieve, and forms a metal organic framework (MOF) and other structures through the metal-support interaction reaction, thereby forming a new core-shell structure on the surface of the 13X molecular sieve. The 13X molecular sieve with a core-shell structure in the present application has the advantages of good dispersion stability of the nickel nanoparticle layer, and also has the advantages of large pore volume and good pore penetration of the titanium silicon shell. It can also give full play to the performance of the 13X molecular sieve to form a multi-level pore molecular sieve material with controllable micro-mesopores, specific surface area and large pore volume, and can further improve the adsorption capacity of this type of molecular sieve, thereby giving it a wider range of applications in the field of shape-selective adsorption.
[0021] In a preferred embodiment, the first solution includes an aqueous solution of any one or more of the following: 3-aminopropyltriethoxysilane, tetraethoxysilane or tetramethoxysilane; preferably, the first immersion time is 6-15h, including but not limited to 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15h; preferably, the concentration of the first solution is 0.05-0.2 mol / L, including but not limited to 0.05, 0.06, 0.07, 0.08, 0.09, 0 .1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19 or 0.2 mol / L; preferably, the second solution comprises any one or more of the following aqueous solutions: nickel nitrate and / or nickel sulfate; preferably, the second immersion time is 12-48h, including but not limited to 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28 , 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47 or 48h; preferably, the concentration of the second solution is 0.01-0.2M, including but not limited to 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0. 16, 0.17, 0.18, 0.19, 0.2M; preferably, the first calcination includes: performing the first calcination in a gas atmosphere; preferably, the gas atmosphere includes a hydrogen atmosphere; preferably, the temperature of the first calcination is 200-1000°C, including but not limited to 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C or 1000°C, and the time is 1-8h, including but not limited to 1, 2, 3, 4, 5, 6, 7 or 8h. In the first calcination, the nickel compound attached to the surface of the 13X molecular sieve is decomposed at high temperature to form nickel oxide, and hydrogen reduces the nickel oxide to nickel nanoparticles. Controlling the temperature and time of the first calcination within the above range helps to improve the efficiency of forming nickel nanoparticles on the surface of the 13X molecular sieve.
[0022] In a preferred embodiment, the titanium silicon molecular sieve precursor solution comprises: silicon dioxide, titanium dioxide, a template, a fluorine complex and water; preferably, the molar ratio of silicon dioxide to titanium dioxide is 1:(0.04-0.1), including but not limited to 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.0, 1:0.09 or 1:0.1; preferably, the molar ratio of silicon dioxide to the template is 1:(0.1-0.3), including but not limited to 1:0.1, 1:0.2 or 1:0.3; preferably, silicon dioxide The molar ratio of silicon dioxide to water is 1:(20-50), including but not limited to 1:20, 1:25, 1:30, 1:40 or 1:50; preferably, the template comprises an organic amine and / or a quaternary ammonium salt; preferably, the fluorine complex comprises any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate or ammonium fluoride.
[0023] The present application uses a first solution containing silicon element to perform a first impregnation on 13X molecular sieve, obtains a first solid, and then performs a second impregnation with a second solution containing nickel element, and performs a first roasting, and the nickel nanoparticle layer finally obtained contains silicon element. The nickel nanoparticle layer reacts and crosslinks with the components in the titanium silicon molecular sieve precursor solution, and can form a titanium silicon shell outside the nickel nanoparticle layer, and finally obtains a 13X molecular sieve with a nickel nanoparticle layer and a titanium silicon shell. The present application helps to control the quality of the nickel nanoparticle layer by controlling the time of the first impregnation treatment, the time of the second impregnation treatment, the concentration of the first solution and the concentration of the second solution within the above range, improves the wetting effect of the first solution and the second solution on the 13X molecular sieve, and the crosslinking degree of the nickel nanoparticle layer and the titanium silicon shell, while not changing the performance of the 13X molecular sieve itself, and synergistically exerts the advantages of these two core-shell structures. Compared with the 13X molecular sieve without a core-shell structure, the molecular sieve with this core-shell structure has better dispersion stability, stronger pore penetration, and larger pore volume and specific surface area.
[0024] In a preferred embodiment, the incubation temperature is 100-500°C, including but not limited to 100°C, 200°C, 300°C, 400°C or 500°C, and the time is 5-20h, including but not limited to 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20h; preferably, the drying temperature is 80-200°C, including but not limited to 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C , 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, for 5-20h, including but not limited to 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20h; preferably, the temperature of the second calcination is 300-600°C, including but not limited to 300°C, 400°C, 500°C or 600°C, for 2-10h, including but not limited to 2, 3, 4, 5, 6, 7, 8, 9 or 10h. By controlling the temperature and time of the second calcination, the peptide silicon composite shell can be better cross-linked with the nickel nanoparticle layer, the efficiency of the reaction is improved, and a nickel nanoparticle layer-peptide silicon composite shell with a moderate degree of cross-linking is obtained, which is conducive to the formation of a 13X molecular sieve that can have the advantages of both shells and has improved comprehensive performance.
[0025] In a preferred embodiment, the preparation method of 13X molecular sieve includes: subjecting a gel system containing a silicon source and an aluminum source to a first crystallization treatment and a second crystallization treatment in sequence to obtain a crystallized product; mixing the crystallized product with a gel mother liquor, and subjecting the system to an aging treatment and a third crystallization treatment in sequence to obtain a 13X molecular sieve.
[0026] Preferably, the preparation method of 13X molecular sieve comprises: S1) dispersing a silicon source in water to obtain a silicon source dispersion; dispersing an aluminum source in water to obtain an aluminum source dispersion; S2) mixing the silicon source dispersion with the aluminum source dispersion, and adjusting the pH to 8.5 to 12.5 after stirring, including but not limited to 8.5, 9, 9.5, 10, 10, 5, 11, 11.5, 12 or 12.5, to obtain a gel system; S3) sequentially performing a first crystallization treatment and a second crystallization treatment on the gel system to obtain a crystallized product; S4) subjecting the crystallized product and the gel mother liquor to an aging treatment and a third crystallization treatment in sequence to obtain a 13X molecular sieve; preferably, in S1), the mass concentration of the silicon source dispersion is 28 to 99 wt%, including but not limited to 28, 29, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 99 wt%; preferably, the silicon source comprises silica sol, tetraethyl orthosilicate, macroporous silica gel (type C silica gel), silicon powder, fly ash or white One or more of carbon black; preferably, the mass concentration of the aluminum source dispersion is 15 to 99wt%, including but not limited to 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 99wt%; preferably, the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; preferably Preferably, the first solvent and the second solvent include water; preferably, in S2), the stirring temperature is 20-100°C, including but not limited to 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, and the time is 0.1-24h, including but not limited to 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h.
[0027] Compared with the conventional method of obtaining a system containing a crystallization product by a single crystallization treatment, the above two-stage crystallization treatment of the gel system containing a silicon source and an aluminum source can effectively control the formation and growth of the crystal seeds. The first stage of the crystallization treatment is carried out under relatively low temperature and time conditions, which is conducive to the initial formation of the crystal seeds. The second stage of the crystallization treatment is carried out under higher temperature and time conditions, which is conducive to the further growth and improvement of the crystal seeds, and can improve the quality and controllability of the crystal seeds. Moreover, the mother liquor obtained by treating the inorganic waste containing the above specific elements is mixed with the system containing the crystallization product to prepare the 13X molecular sieve, which can improve the recovery rate of the inorganic waste and improve its utilization value. In the above method, the pH is adjusted to 8.5-12.5 after stirring, and the gel system obtained is beneficial to improving the crystallinity and purity of the crystallized product by adding the aluminum source dispersion into the silicon source dispersion, compared with pouring the aluminum source dispersion into the silicon source dispersion. At the same time, adjusting the pH within the above range is beneficial to accelerating the crystallization rate of the subsequent two-stage crystallization treatment, shortening the crystallization time, and facilitating the subsequent formation of the molecular sieve of the specific crystal form of the present application.
[0028] The preparation method of 13X molecular sieve in the present application utilizes recycled silicon-rich and aluminum-rich extracts to replace part of the raw materials, accurately controls the pH value, and performs segmented crystallization, adds an appropriate amount of seed solution, and uses other raw materials to replace part of the aluminum-rich liquid and silicon-rich liquid, effectively controlling the growth rate and final size of the crystal, and can prepare a 13X molecular sieve with a smooth crystal surface without impurities.
[0029] In a preferred embodiment, in S3), the temperature of the second crystallization treatment is 20-100°C higher than the temperature of the first crystallization treatment; preferably, the temperature of the first crystallization treatment is 20-60°C, including but not limited to 20°C, 30°C, 40°C, 50°C or 60°C, and the time is 4-24h, including but not limited to 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h. 4h; preferably, the temperature of the second crystallization treatment is 80-120°C, including but not limited to 80, 90, 100, 110 or 120°C, and the time is 6-48h, including but not limited to 6, 7, 8, 9, 10, 11, 12, 24, 36 or 48h; preferably, the components in the crystallization product include silicon dioxide, aluminum oxide, sodium oxide and water; preferably, the molar ratio of silicon dioxide to aluminum oxide is 0.01-2.5:1, including but not limited to 0.01: 1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 1:1, 1.5:1, 2:1 or 2.5:1; preferably, the molar ratio of sodium oxide to silicon dioxide is 0.01 to 4.0:1, including but not limited to 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1 , 0.08:1, 0.09:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1 or 4:1; preferably, the molar ratio of water to silicon dioxide is 1.0 to 40.0:1, including but not limited to 1:1, 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1 or 40:1.
[0030] In the present application, the temperature difference between the first crystallization treatment and the second crystallization treatment can make the adjustment of the silicon-aluminum ratio of the molecular sieve more flexible, which is conducive to the subsequent formation of a 13X type molecular sieve with controllable morphology and size and a wide silicon-aluminum ratio, thereby improving the comprehensive performance of the molecular sieve.
[0031] In a preferred embodiment, in S4), the preparation method of the gel mother liquor comprises: performing a third roasting on a mixed system of inorganic waste and flux to obtain a third roasting product; mixing the third roasting product with an acid solution, and obtaining a filter residue and a first filtrate after a first solid-liquid separation; mixing the filter residue with an alkaline solution, and obtaining a second filtrate after a second solid-liquid separation; mixing the first filtrate with the second filtrate to obtain a gel mother liquor; preferably, the inorganic waste comprises waste ZSM-5 molecular sieve catalyst, waste MTO catalyst, powder One or more of coal ash, waste FCC catalyst or waste VOC adsorbent; preferably, the aging temperature is 20-100°C, including but not limited to 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, and the time is 0.1-24h, including but not limited to 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23 or 24h; the aging process is carried out under stirring; preferably, the third crystallization treatment includes a crystallization temperature of 60 to 105°C, including but not limited to 60°C, 70°C, 80°C, 90°C, 100°C, 101°C, 102°C, 103°C, 104°C or 105°C, and a time of 0.1 to 36h, including but not limited to 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 2 0, 21, 22, 23 or 24h; preferably, the mass ratio of the crystallization product to the gel mother liquor is 5 to 20:100, including but not limited to 5:100, 6:100, 6:100, 6:100, 7:100, 8:100, 9:100, 10:100, 11:100, 12:100, 13:100, 14:100, 15:100, 16:100, 17:100, 18:100, 19:100 or 20:100.
[0032] The temperature and time of the third crystallization treatment include but are not limited to the above ranges. Limiting it within the above ranges is beneficial to improving the crystal purity of the prepared molecular sieve, reducing impurity components, and also beneficial to increasing the adsorption sites of the prepared 13X molecular sieve, increasing its internal pore volume, thereby improving its adsorption performance, and enabling a better formation of a core-shell structure of a nickel nanoparticle layer and a peptide silicon shell on its surface. The above-mentioned inorganic waste materials include but are not limited to one or more of ZSM-5 molecular sieve catalysts, waste MTO catalysts, fly ash, waste FCC catalysts or waste VOC adsorbents, and can also be one or more of other waste molecular sieve adsorbents or waste catalysts.
[0033] In a preferred embodiment, the mass ratio of inorganic waste to flux is 1:0.5-1:5, including but not limited to: 0.5, 1:1, 1:1.5; preferably, the temperature of the third roasting is 550-800°C, including but not limited to 550°C, 560°C, 570°C, 580°C, 600°C, 700°C or 800°C, and the time is 60-120min, including but not limited to 60, 70, 80, 90, 100, 110 or 120min; preferably, the mass concentration of the acid aqueous solution is 10%-35%, including but not limited to 10, 15, 20, 25, 30 or 35%; preferably, the flux comprises sodium carbonate and / or sodium sulfate; preferably, the acid in the acid solution is a monobasic acid, more preferably hydrochloric acid and / or nitric acid; preferably, the alkali in the alkali solution comprises sodium hydroxide and / or potassium hydroxide; preferably, the mass ratio of the filter residue, the alkali and the water is 0.1-100:40-60:50-400; Preferably, the mass ratio of the first filtrate to the second filtrate is 1:(2.5-5.5), including but not limited to 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 or 1:5.5; preferably, the components in the gel mother liquor include silicon dioxide, aluminum oxide, sodium oxide and water; preferably, the molar ratio of silicon dioxide to aluminum oxide is (0.5-6.0):1, including but not limited to 0.5:1, 1:1, 2:1, 3:1, 4:1 , 5:1 or 6:1; preferably, the molar ratio of sodium oxide to silicon dioxide is (0.5-6.0):1, including but not limited to 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1 or 6:1; preferably, the molar ratio of water to silicon dioxide is (10-100):1, including but not limited to 10:1, 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1 or 100:1.
[0034] In a preferred embodiment, the silicon-aluminum ratio of the 13X molecular sieve with a core-shell structure is 2.4-3.1, and the pore volume is 0.37-0.58 cm 3 / g, specific surface area is 850~1000m 2 / g.
[0035] In a second typical embodiment of the present application, a 13X molecular sieve with a core-shell structure is prepared by any one of the above-mentioned methods for preparing a 13X molecular sieve with a core-shell structure, wherein the silicon-aluminum ratio of the 13X molecular sieve with a core-shell structure is 2.4 to 3.1, and the pore volume is 0.37 to 0.58 cm 3 / g, specific surface area is 850~1000m 2 / g.
[0036] The 13X molecular sieve with a core-shell structure in the present application has a large specific surface area, contains more adsorption sites, and has better adsorption performance. In the molecular sieve of the present application, by introducing a nickel nanoparticle layer and a titanium silicon shell, a mesoporous channel is introduced, the pore volume inside the molecular sieve crystal is increased, and the flow and diffusion performance of the guest molecules inside the molecular sieve is improved, and the morphology is evenly dispersed and has regular nanoparticles. And the 13X molecular sieve prepared by the preparation method of the above-mentioned 13X molecular sieve also has a high silicon-aluminum ratio, a high silicon source utilization rate, and has better selectivity for cross-linking with the two shells. It can be regulated according to different adsorption molecules, thereby significantly reducing the carbon deposition rate of the molecular sieve to improve the diffusion performance of the adsorbent.
[0037] The beneficial effects of the present application will be further explained in detail below in conjunction with specific embodiments.
[0038] Example 1
[0039] A method for preparing a 13X molecular sieve having a core-shell structure comprises the following steps:
[0040] (1) 21.0 g of silica sol was dissolved in 36.0 g of deionized water, and pretreated in a sealed reactor at 25° C. for 1 h to obtain a silicon source dispersion;
[0041] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water and stir at 25° C. for 1 h to obtain an aluminum source dispersion;
[0042] The aluminum source dispersion was added dropwise to the silicon source dispersion, and the mixture was stirred at 60° C. for 8 h to obtain a gel solution;
[0043] Dissolve 6.74 g of NaOH in 36 g of deionized water to obtain a NaOH aqueous solution, add the NaOH aqueous solution to the gel solution, adjust the pH value to 12.2, and obtain a gel system containing a silicon source and an aluminum source;
[0044] The above gel system was transferred to a hydrothermal reactor and subjected to two-stage temperature-controlled crystallization (i.e., the first crystallization treatment and the second crystallization treatment): the temperature of the first crystallization treatment was 40°C and the time was 12 h; the temperature of the second crystallization treatment was 95°C and the time was 24 h.
[0045] A crystallized product (white) was obtained;
[0046] In the crystallized product, the molar ratio of SiO2 to Al2O3 is 1.5:1, the molar ratio of Na2O to SiO2 is 1.6:1, and the molar ratio of H2O to SiO2 is 32:1.
[0047] (2) The above-mentioned 10 g, 200 mesh waste ZSM-5 molecular sieve catalyst was mixed with 8 g Na2CO3 and calcined at 650°C for 120 min to obtain a third calcined product; then the third calcined product was dissolved and filtered using a nitric acid solution with a mass fraction of 25% to obtain a filter residue; the specific components of the above-mentioned waste ZSM-5 molecular sieve are shown in Table 1.
[0048] Take 10g of the filter residue and mix it with 6g of NaOH and 40g of water; mix the silicon-rich liquid and the aluminum-rich liquid in a weight ratio of 4:1 to obtain a gel mother liquid;
[0049] The molar ratio of SiO2 to Al2O3 in the gel mother solution is 3.5:1, the molar ratio of Na2O to SiO2 is 2.8:1, and the molar ratio of H2O to SiO2 is 80:1.
[0050] Table 1
[0051] <![CDATA[Fe2O3 / wt%]]> <![CDATA[Al2O3 / wt%]]> <![CDATA[SiO2 / wt%]]> <![CDATA[SO3 / wt%]]> CaO / wt% Spent ZSM-5 molecular sieve catalyst 0.050 19.84 79.64 0.31 0.18
[0052] (3) Take 25 g of the crystallized product obtained in step (1) and add it to the gel mother liquor prepared in step (2), age it at 60°C for 12 h, and place it in a hydrothermal reactor for a third crystallization treatment, wherein the temperature of the third crystallization treatment is 98°C and the time is 24 h; filter and wash until the pH is 7, and dry it at 90°C to obtain a 13X molecular sieve.
[0053] (4) The 13X molecular sieve was placed in 500 mL of a 0.2 mol / L 3-aminopropyltriethoxysilane (APTES) aqueous solution (first solution) for a first immersion for 8 hours. The 13X molecular sieve (first solid) after the first immersion was then immersed in a 0.1 M nickel nitrate solution (second solution), and the pH was adjusted to 9 with sodium hydroxide. After immersion for 24 hours, the 13X molecular sieve was first calcined at 500° C. for 2 hours in a hydrogen atmosphere to form a nano-nickel particle deposition layer on the outside, thereby obtaining a 13X molecular sieve containing a nickel nano-particle layer.
[0054] (5) Mix according to the molar ratio of SiO2: TiO2: organic amine: sodium hexafluorophosphate: water = 1: (0.04): (0.1): (0.03): (20) to obtain a titanium silicon molecular sieve precursor solution. Add the 13X molecular sieve containing the nickel nanoparticle layer to the titanium silicon molecular sieve precursor solution, mix thoroughly, and transfer the mixed solution to a reactor. Perform a hydrothermal reaction at 150°C for 12 hours to form a titanium silicon composite shell (incubation). After the reaction is completed, filter and wash with deionized water, then dry at 110°C for 12 hours, and finally perform a second calcination at 450°C for 4 hours to obtain a 13X molecular sieve with a core-shell structure.
[0055] Example 2
[0056] The difference from Example 1 is that: (1) 1 g of silicon powder is dissolved in 18.0 g of deionized water, and pretreated in a closed reactor at 25° C. for 1 h to obtain a silicon source dispersion;
[0057] Dissolve 12 g of aluminum nitrate in 18 g of deionized water and stir at 25° C. for 1 h to obtain an aluminum source dispersion;
[0058] The aluminum source dispersion liquid was added dropwise to the silicon source dispersion liquid, and stirring was continued at 50° C. for 6 hours to obtain a gel solution;
[0059] Dissolve 2 g of NaOH in 36 g of deionized water to obtain a NaOH aqueous solution, add the NaOH aqueous solution to the gel solution, adjust the pH value to 11.8, and obtain a gel system containing a silicon source and an aluminum source;
[0060] The gel system was transferred to a hydrothermal reactor and subjected to two stages of temperature-controlled crystallization (i.e., the first crystallization treatment and the second crystallization treatment): the temperature of the first crystallization treatment was 40°C and the time was 14h; the temperature of the second crystallization treatment was 100°C and the time was 18h. A crystallized product (light yellow) was obtained;
[0061] In the crystallization product, the molar ratio of SiO2 to Al2O3 is 0.6:1, the molar ratio of Na2O to SiO2 is 3:1, and the molar ratio of H2O to SiO2 is 20:1.
[0062] (2), (3), (4) and (5) are consistent with the steps in Example 1.
[0063] Example 3
[0064] The difference from Example 1 is:
[0065] (1) 14.65 g of ethyl orthosilicate and 36 g of deionized water were mixed in a mass ratio of 1:1, and pretreated in a sealed reactor at 25° C. for 1 hour to obtain a silicon source dispersion;
[0066] 12 g of aluminum nitrate was dissolved in 18.0 g of deionized water, and stirred at 35° C. for 1 hour to obtain an aluminum source dispersion.
[0067] The aluminum source dispersion liquid was gradually added dropwise to the silicon source dispersion liquid, and the mixture was mixed and stirred at 20° C. for 0.1 hour to prepare a gel solution;
[0068] Dissolve 0.56 g of NaOH in 6 g of deionized water to obtain a NaOH aqueous solution, add the NaOH aqueous solution to the gel solution, adjust the pH value to 8.5, and obtain a gel system containing a silicon source and an aluminum source;
[0069] The gel system was transferred to a hydrothermal reactor and subjected to two-stage temperature-controlled crystallization (i.e., the first crystallization treatment and the second crystallization treatment): the first crystallization temperature was 20°C and the time was 4 hours; the second crystallization treatment temperature was 80°C and the time was 6 hours, and finally a white solid 13X molecular sieve was obtained.
[0070] Steps (2) to (5) are the same as those in Example 1.
[0071] Example 4
[0072] The difference from Example 1 is that: (1) 0.17 g of silicon powder is dissolved in 6 g of deionized water, and pretreated in a closed reactor at 25° C. for 1 h to obtain a silicon source dispersion;
[0073] Dissolve 12 g of aluminum nitrate in 18 g of deionized water and stir at 35° C. for 1 h to obtain an aluminum source dispersion;
[0074] The aluminum source dispersion liquid was added dropwise to the silicon source dispersion liquid, and the mixture was stirred at 100° C. for 24 hours to obtain a gel solution;
[0075] Dissolve 0.9 g of NaOH in 6 g of deionized water to obtain a NaOH aqueous solution, add the NaOH aqueous solution to the gel solution, adjust the pH value to 12.5, and obtain a gel system containing a silicon source and an aluminum source;
[0076] The gel system was transferred to a hydrothermal reactor and subjected to two stages of temperature-controlled crystallization (i.e., the first crystallization treatment and the second crystallization treatment): the temperature of the first crystallization treatment was 60°C for 24 hours; the temperature of the second crystallization treatment was 120°C for 48 hours. A crystallized product (light yellow) was obtained;
[0077] In the crystallized product, the molar ratio of SiO2 to Al2O3 is 0.1:1, the molar ratio of Na2O to SiO2 is 4:1, and the molar ratio of H2O to SiO2 is 1:1.
[0078] (2), (3), (4) and (5) are consistent with the steps in Example 1.
[0079] Example 5
[0080] Steps (1) to (4) and (5) in this embodiment are consistent with those in Example 1;
[0081] (4) is different from Example 1 in that the first impregnation time is 15 h, the solution concentration is 0.04 mol / L; the second impregnation time is 48 h, the solution concentration is 0.01 M; and the first calcination is at 1000°C for 1 h.
[0082] Example 6
[0083] Steps (1) to (3) and (5) in this embodiment are consistent with those in Embodiment 1;
[0084] (4) is different from Example 1 in that the first impregnation time is 6 h, the solution concentration is 0.2 mol / L; the second impregnation time is 12 h, the solution concentration is 0.2 M; and the first calcination is at 200°C for 8 h.
[0085] Example 7
[0086] Steps (1) to (4) and (5) in this embodiment are consistent with those in Example 1;
[0087] (5) is different from Example 1 in that the molar ratio of SiO2:TiO2:organic amine:sodium hexafluorophosphate:water is 1:0.04:0.1:0.04:20.
[0088] Example 8
[0089] Steps (1) to (4) in this embodiment are consistent with those in Embodiment 1;
[0090] (5) is different from Example 1 in that the molar ratio of SiO2:TiO2:organic amine:sodium hexafluorophosphate:water is 1:0.1:0.3:0.1:50.
[0091] Example 9
[0092] Steps (1) to (4) in this embodiment are consistent with those in Embodiment 1;
[0093] (5), the incubation temperature is 100°C and the time is 20 h; the second calcination temperature is 300°C and the time is 10 h.
[0094] Example 10
[0095] Steps (1) to (4) in this embodiment are consistent with those in Embodiment 1;
[0096] (5), the incubation temperature is 500°C and the time is 5 h; the second calcination temperature is 600°C and the time is 2 h.
[0097] Comparative Example 1
[0098] In this comparative example, steps (1) to (3) and (5) are consistent with those in Example 1;
[0099] (4) is different from Example 1 in that after obtaining the 13X molecular sieve, the first impregnation is not performed in the first solution, and the second impregnation is performed directly in nickel nitrate. The subsequent steps are consistent with the other steps of step (4) of Example 1 to obtain the 13X molecular sieve.
[0100] Comparative Example 2
[0101] In this comparative example, steps (1) to (3) and (5) are consistent with those in Example 1;
[0102] This comparative example does not include step (4). After completing step (3), step (5) is directly performed to obtain 13X molecular sieve.
[0103] Comparative Example 3
[0104] Steps (1) to (4) in this embodiment are consistent with those in Embodiment 1;
[0105] This comparative example does not include step (5) and obtains 13X molecular sieve.
[0106] Table 2 shows the BET surface area, pore volume, BJH adsorption average pore diameter and silicon source conversion rate of the molecular sieves prepared in Examples 1-10 and Comparative Examples 1-3 of the present application. Micropores refer to pores with a pore diameter of less than 2 nm, and mesopores refer to pores with a diameter of 2 to 50 nm.
[0107] Table 2
[0108]
[0109] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0110] The 13X molecular sieve with a nickel nanoparticle layer and a titanium silicon shell prepared by the preparation method of the present application has improved specific surface area, pore volume and pore capacity performance compared with the 13X molecular sieve without a core-shell structure prepared in the prior art. Finally, a 13X molecular sieve with a core-shell structure with a large surface area, controllable morphology and size, and better dispersibility is obtained.
[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a 13X molecular sieve having a core-shell structure, characterized in that: The preparation method comprises: The 13X molecular sieve is first impregnated in a first solution and then filtered to obtain a first solid; the first solid is second impregnated in a second solution and then first calcined to obtain a 13X molecular sieve containing a nickel nanoparticle layer; The 13X molecular sieve containing the nickel nanoparticle layer is mixed with a precursor solution, and incubated, dried and calcined in sequence to obtain the 13X molecular sieve having a core-shell structure; Wherein, the precursor solution includes a titanium silicon molecular sieve precursor solution.
2. The preparation method according to claim 1, characterized in that: The first solution includes an aqueous solution of any one or more of the following: 3-aminopropyltriethoxysilane, tetraethoxysilane or tetramethoxysilane; Preferably, the first impregnation time is 6-15h; Preferably, the concentration of the first solution is 0.05-0.2 mol / L; Preferably, the second solution comprises an aqueous solution of any one or more of the following: nickel nitrate and / or nickel sulfate; Preferably, the second impregnation time is 12-48h; Preferably, the concentration of the second solution is 0.01-0.2M; Preferably, the first calcination comprises: performing the first calcination in a gas atmosphere; Preferably, the gas atmosphere comprises a hydrogen atmosphere; Preferably, the temperature of the first calcination is 200-1000° C., and the time is 1-8 hours.
3. The preparation method according to claim 1, characterized in that: The titanium silicon molecular sieve precursor solution comprises: silicon dioxide, titanium dioxide, a template agent, a fluorine complex and water; Preferably, the molar ratio of the silicon dioxide to the titanium dioxide is 1:(0.04-0.1); Preferably, the molar ratio of the silica to the template is 1:(0.1-0.3); Preferably, the molar ratio of the silicon dioxide to the fluorine complex is 1:(0.04-0.1); Preferably, the molar ratio of the silicon dioxide to the water is 1:(20-50); Preferably, the template comprises an organic amine and / or a quaternary ammonium salt; Preferably, the fluorine complex includes any one or more of sodium hexafluorophosphate, sodium hexafluoroacetylacetonate or ammonium fluoride.
4. The preparation method according to claim 1, characterized in that: The incubation temperature is 100-500°C and the time is 5-20h; Preferably, the drying temperature is 80-200°C and the drying time is 5-20h; Preferably, the second calcination is carried out at a temperature of 300-600° C. and for a time of 2-10 h.
5. The preparation method according to claim 1, characterized in that: The preparation method of the 13X molecular sieve comprises: subjecting a gel system containing a silicon source and an aluminum source to a first crystallization treatment and a second crystallization treatment in sequence to obtain a crystallized product; The crystallized product is mixed with a gel mother solution, and subjected to an aging treatment and a third crystallization treatment in sequence to obtain the 13X molecular sieve; Preferably, the preparation method of the 13X molecular sieve comprises: S1) dispersing a silicon source in water to obtain a silicon source dispersion; dispersing an aluminum source in water to obtain an aluminum source dispersion; S2) mixing the silicon source dispersion liquid and the aluminum source dispersion liquid, and adjusting the pH to 8.5 to 12.5 after stirring to obtain the gel system; S3) subjecting the gel system to the first crystallization treatment and the second crystallization treatment in sequence to obtain the crystallized product; S4) subjecting the crystallized product and the gel mother solution to the aging treatment and the third crystallization treatment in sequence to obtain the 13X molecular sieve; Preferably, in said S1), the mass concentration of said silicon source dispersion is 28 to 99 wt %; Preferably, the silicon source includes one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash or white carbon black; Preferably, the mass concentration of the aluminum source dispersion is 15 to 99 wt %; Preferably, the aluminum source includes one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate or aluminum nitrate; Preferably, in S2), the stirring temperature is 20 to 100° C. and the stirring time is 0.1 to 24 h.
6. The preparation method according to claim 5, characterized in that: In said S3), the temperature of said second crystallization treatment is 20 to 100° C. higher than the temperature of said first crystallization treatment; Preferably, the temperature of the first crystallization treatment is 20-60°C and the time is 10-18h; Preferably, the temperature of the second crystallization treatment is 80-120°C and the time is 6-48h; Preferably, the components in the crystallized product include silicon dioxide, aluminum oxide, sodium oxide and water; Preferably, the molar ratio of silicon dioxide to aluminum oxide is 0.01 to 2.5:1; Preferably, the molar ratio of sodium oxide to silicon dioxide is 0.01 to 4.0:1; Preferably, the molar ratio of water to silicon dioxide is 1.0-40.0:
1.
7. The preparation method according to claim 5, characterized in that: In said S4), the preparation method of the gel mother solution comprises: performing a third roasting on a mixed system of inorganic waste and flux to obtain a third roasting product; The third calcined product is mixed with an acid solution, and a filter residue and a first filtrate are obtained after a first solid-liquid separation; The filter residue is mixed with an alkaline solution, and a second filtrate is obtained after a second solid-liquid separation; Mixing the first filtrate with the second filtrate to obtain the gel mother solution; Preferably, the inorganic waste includes one or more of waste ZSM-5 molecular sieve catalyst, waste MTO catalyst, fly ash, waste FCC catalyst or waste VOC adsorbent; Preferably, the aging treatment temperature is 20 to 100°C and the time is 0.1 to 24 hours; Preferably, the temperature of the third crystallization treatment is 60-105° C., and the time is 0.1-36 h; Preferably, the mass ratio of the crystallization product to the gel mother solution is 5-20:
100.
8. The preparation method according to claim 7, characterized in that: The mass ratio of the inorganic waste to the flux is 1:0.5-1:5; Preferably, the temperature of the third calcination is 550-800°C and the time is 60-120min; Preferably, the mass concentration of the acid solution is 10%-35%; Preferably, the flux comprises sodium carbonate and / or sodium sulfate; Preferably, the acid in the acid solution is a monoprotic acid, more preferably hydrochloric acid and / or nitric acid; Preferably, the alkali in the alkali solution comprises sodium hydroxide and / or potassium hydroxide; Preferably, the mass ratio of the filter residue, the alkali and water is 0.1-100:40-60:50-400; Preferably, the mass ratio of the first filtrate to the second filtrate is 1:(2.5-5.5); Preferably, the components in the gel mother solution include silicon dioxide, aluminum oxide, sodium oxide and water; Preferably, the molar ratio of silicon dioxide to aluminum oxide is (0.5-6.0):1; Preferably, the molar ratio of sodium oxide to silicon dioxide is (0.5-6.0):1; Preferably, the molar ratio of water to silicon dioxide is (10-100):
1.
9. The preparation method according to claim 1, characterized in that: The silicon-aluminum ratio of the 13X molecular sieve with a core-shell structure is 2.4-3.1, and the pore volume is 0.37-0.58 cm 3 / g, specific surface area is 850~1000m 2 / g.
10. A 13X molecular sieve with a core-shell structure prepared by the method for preparing a 13X molecular sieve with a core-shell structure according to any one of claims 1 to 9, characterized in that: The silicon-aluminum ratio of the 13X molecular sieve with a core-shell structure is 2.4-3.1, and the pore volume is 0.37-0.58 cm 3 / g, specific surface area is 850~1000m 2 / g.
Citation Information
Patent Citations
Titanium-silicon material with core-shell structure, preparation method of titanium-silicon material and method for producing epoxy compound through macromolecular olefin oxidation reaction
CN112742471A
MFI type core-shell structure molecular sieve and preparation method thereof, acoustic reinforcing material, loudspeaker and electronic equipment
CN116375047A
Preparation method for SSZ-52 molecular sieve
WO2024139860A1