Method for separating rubidium and cesium from high-salt mother liquor

By mixing high-salt mother liquor with magnesium chloride and sodium phosphate and stirring, the problem of difficulty in separating rubidium cesium in high-salt solutions in the prior art was solved, efficient separation of rubidium cesium and purity was achieved, and separation cost was reduced.

CN118908246AInactive Publication Date: 2024-11-08UNIV OF SCI & TECH BEIJING
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411027281.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has problems such as high cost of extractant, low adsorbent capacity and inapplicable to high-salt solutions when separating rubidium cesium from high-salt solutions, making it difficult to effectively separate rubidium cesium.

Method used

By mixing high-salt mother liquor with magnesium chloride and sodium phosphate, stirring and reaction, solid-liquid separation is performed to obtain a rubidium-containing cesium precipitate, and the reaction is carried out after adjusting the pH value to achieve separation of rubidium and cesium.

Benefits of technology

Efficient separation of rubidium cesium from high-salt mother liquor is achieved, which improves the precipitation rate and separation purity of rubidium cesium and reduces separation cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of nonferrous metallurgy, in particular to a method for separating rubidium and cesium from high-salt mother liquor. Comprising the following steps: mixing a high-salt mother solution with magnesium chloride to obtain a magnesium-containing solution; mixing the high-salt mother liquor with sodium phosphate to obtain a phosphate radical-containing solution; mixing the magnesium-containing solution with the phosphate radical-containing solution, and stirring for reaction to obtain a stirred reactant; carrying out solid-liquid separation on the stirred reactant to obtain rubidium and cesium-containing precipitates; and mixing the rubidium and cesium-containing precipitate with water, adjusting the pH value to be strongly alkaline, then carrying out a reaction to obtain a reactant, and carrying out solid-liquid separation to obtain a solution containing rubidium and cesium, thereby realizing separation of rubidium and cesium from the high-salt mother liquor. By adopting the method provided by the invention, rubidium and cesium can be efficiently separated from the high-salt mother liquor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonferrous metal metallurgy, in particular to a method for separating rubidium and cesium from a high-salt mother liquor. Background Art

[0002] Rubidium and cesium, two rare and expensive alkali metal elements, are key raw materials for energy transformation and high-tech energy transformation, and are widely used in new materials, new energy, biomedicine, aerospace and other fields.

[0003] As a rare metal, rubidium and cesium have a relatively high abundance in the earth's crust, but they are extremely dispersed and mostly associated with other alkali metal elements. Whether in solid minerals such as lepidolite and cesium garnet, or in salt lake brine, there are almost no independent deposits. During the extraction of metallic lithium, rubidium and cesium will enter the solution. After the metallic lithium is recovered, rubidium and cesium will exist in the post-extraction solution, but at this time, the presence of a large amount of potassium and sodium ions makes the extraction more difficult.

[0004] There are currently three main methods for extracting rubidium and cesium from solutions: precipitation, extraction and adsorption. The most commonly used extractant for the extraction method is t-BAMBP, but the extraction method has poor operating environment, high price of the extractant and certain toxicity. More importantly, the extractant emulsifies when treating high-salt solutions, which greatly increases the extraction cost. The adsorption method is mainly divided into inorganic adsorbents, organic adsorbents and biological adsorbents. Inorganic adsorbents are the most commonly used, including metal ferrocyanide, clay minerals, carbon-based materials, heteropoly acids and other materials; but the adsorption method has the disadvantages of low adsorption capacity and low mechanical strength, and is more suitable for treating low-concentration rubidium and cesium solutions. The precipitation method is more suitable for treating high-concentration rubidium and cesium solutions. Commonly used precipitants include vanadium salts, metal ferrocyanide, polyhalides and heteropoly acids.

[0005] Chinese Patent 201710615317.X proposes a method for separating and extracting rubidium and cesium from coal, using iodine chloride to generate a precipitate containing rubidium and cesium, and then combining t-BAMBP extraction to obtain high-purity rubidium chloride and cesium chloride. Chinese Patent 201811063100.3 proposes a method for separating rubidium and cesium from associated sodium and potassium by using the property of aluminum sulfate to form insoluble rubidium and cesium alum with rubidium and cesium. Chinese Patent 202110474179.4 proposes a method for extracting rubidium and cesium from complex underground brine, using the SnCl4 precipitation method to separate rubidium and cesium by forming an insoluble chloride rubidium and cesium complex salt. Patent application 202011340808.6 proposes a method for preparing metal ferrocyanide adsorbent particles for the extraction of liquid rubidium and cesium resources, using transition metal ferrocyanide as an adsorbent to extract rubidium and cesium. The main problems of ferrocyanide in the process of recovering rubidium and cesium are small particles, poor crystallinity, low strength, etc., which makes it difficult to separate solids and liquids. Chinese patent 202010712906.1 proposes a method for extracting cesium and rubidium from lithium mica, and the mixed alum of rubidium and cesium is roasted at high temperature to obtain a sulfate solution enriched in rubidium and cesium, and then multi-stage extraction is performed to obtain cesium sulfate and rubidium sulfate with a purity of more than 98%, and the total recovery rate of cesium and rubidium is more than 80%; 201910583379.6 proposes a rubidium and cesium precipitation and separation system in aqueous solution and its application method. The rubidium and cesium are reacted with phosphotungstic acid and other precipitants to form a precipitate, and then the particles are separated by froth flotation.

[0006] In summary, the problem of separating rubidium and cesium by adsorption is that the capacity of the adsorbent is small; the organic extraction method is not suitable for rubidium and cesium in high-salt solutions. In view of the problems existing in the prior art, the present invention proposes a method for separating rubidium and cesium from high-salt mother liquor, in order to solve the shortcomings of the prior art. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a method for separating rubidium and cesium from a high-salt mother liquor, thereby achieving separation of rubidium and cesium from a high-salt mother liquor.

[0008] In order to achieve the above object, the present invention provides the following technical solutions:

[0009] The present invention provides a method for separating rubidium and cesium from a high-salt mother liquor, comprising the following steps:

[0010] 1) mixing a high-salt mother liquor with magnesium chloride to obtain a magnesium-containing solution;

[0011] mixing the high salt mother liquor with sodium phosphate to obtain a phosphate-containing solution;

[0012] The high salt mother liquor contains rubidium ions and cesium ions;

[0013] 2) mixing the magnesium-containing solution obtained in step 1) with the phosphate-containing solution, stirring and reacting to obtain a stirred reactant;

[0014] 3) separating the stirred reaction product obtained in step 2) into solid and liquid to obtain a precipitate containing rubidium and cesium;

[0015] 4) Mixing the rubidium-cesium precipitate obtained in step 3) with water, adjusting the pH value to above 12.0, and reacting to obtain a reactant. After solid-liquid separation, the obtained solution contains rubidium and cesium, thereby achieving separation of rubidium and cesium from the high-salt mother liquor.

[0016] Preferably, in the step 1), the concentration of sodium ions in the high-salt mother liquor is 117.9 g / L, the concentration of potassium ions is 91.47 g / L, the concentration of rubidium ions is 6.99 g / L, the concentration of cesium ions is 8.59 g / L, the concentration of calcium ions is 1.97 g / L, the concentration of chloride ions is 158.65 g / L, and the concentration of bromide ions is 18.89 g / L.

[0017] Preferably, the mass ratio of the volume of the high-salt mother liquor in step 1) to magnesium chloride is 25-50 mL: 1.46-2.91 g.

[0018] Preferably, the mass ratio of the volume of the high-salt mother liquor in step 1) to the sodium phosphate is 25-50 mL: 1.18-2.54 g.

[0019] Preferably, the stirring reaction conditions in step 2) include: a rotation speed of 600 rpm and a time of 30 min;

[0020] The volume ratio of the magnesium-containing solution to the phosphate-containing solution is 1:1.

[0021] Preferably, after the solid-liquid separation in step 3), the obtained solid is dried to obtain a precipitate containing rubidium and cesium;

[0022] The drying conditions include: temperature of 105° C. and time of 120 min.

[0023] Preferably, the mass ratio of the rubidium-cesium precipitate to water in step 4) is 1:2-3.

[0024] Preferably, the reaction conditions of step 4) include: a rotation speed of 600 rpm and a reaction time of 2 h.

[0025] Beneficial effects of the present invention:

[0026] The method provided by the invention can efficiently separate rubidium and cesium from high-salt mother liquor. DETAILED DESCRIPTION

[0027] The present invention provides a method for separating rubidium and cesium from a high-salt mother liquor, comprising the following steps:

[0028] 1) mixing a high-salt mother liquor with magnesium chloride to obtain a magnesium-containing solution;

[0029] mixing the high salt mother liquor with sodium phosphate to obtain a phosphate-containing solution;

[0030] The high salt mother liquor contains rubidium ions and cesium ions;

[0031] 2) mixing the magnesium-containing solution obtained in step 1) with the phosphate-containing solution, stirring and reacting to obtain a stirred reactant;

[0032] 3) separating the stirred reaction product obtained in step 2) into solid and liquid to obtain a precipitate containing rubidium and cesium;

[0033] 4) Mixing the rubidium-cesium precipitate obtained in step 3) with water, adjusting the pH value to above 12.0, and reacting to obtain a reactant. After solid-liquid separation, the obtained solution contains rubidium and cesium, thereby achieving separation of rubidium and cesium from the high-salt mother liquor.

[0034] The invention mixes a high-salt mother liquor with magnesium chloride to obtain a magnesium-containing solution; mixes the high-salt mother liquor with sodium phosphate to obtain a phosphate-containing solution; and the high-salt mother liquor contains rubidium ions and cesium ions.

[0035] In the present invention, the concentration of sodium ions in the high-salt mother liquor is preferably 117.9 g / L, the concentration of potassium ions is preferably 91.47 g / L, the concentration of rubidium ions is preferably 6.99 g / L, the concentration of cesium ions is preferably 8.59 g / L, the concentration of calcium ions is preferably 1.97 g / L, the concentration of chloride ions is preferably 158.65 g / L, and the concentration of bromide ions is preferably 18.89 g / L. It should be pointed out that the method and content of the present invention are developed based on this high-salt mother liquor, but the content of the invention is not limited to the high-salt mother liquor of the components shown in the table, and is applicable to other types of liquids containing rubidium and cesium.

[0036] In the present invention, the mass ratio of the volume of the high salt mother liquor to the magnesium chloride is preferably 25-50 mL: 1.46-2.91 g. In the present invention, the magnesium chloride is preferably magnesium chloride hexahydrate. In the present invention, the mass ratio of the volume of the high salt mother liquor to the sodium phosphate is preferably 25-50 mL: 1.18-2.54 g.

[0037] The present invention mixes the obtained magnesium-containing solution with the phosphate-containing solution, and stirs the reaction to obtain a stirred reactant. In the present invention, the conditions of the stirring reaction preferably include: a rotation speed of 600 rpm and a time of 30 min. In the present invention, the volume ratio of the magnesium-containing solution to the phosphate-containing solution is preferably 1:1. In the present invention, the reaction formula of the stirring reaction is as follows:

[0038] Cs + / Rb + +Mg2+ +PO4 3- =(Cs / Rb)MgPO4↓.

[0039] The present invention separates the stirred reactant into solid and liquid to obtain a precipitate containing rubidium and cesium. In the present invention, after the solid-liquid separation, the obtained solid is preferably dried to obtain a precipitate containing rubidium and cesium. In the present invention, the drying conditions preferably include: a temperature of 105° C. and a time of 120 min. The present invention does not specifically limit the solid-liquid separation, and those skilled in the art can use conventional methods.

[0040] The method comprises mixing the obtained rubidium-cesium-containing precipitate with water, adjusting the pH value to be above 12.0, and then reacting to obtain a reactant. After solid-liquid separation, the obtained solution contains rubidium and cesium, thereby realizing separation of rubidium and cesium from a high-salt mother liquor.

[0041] In the present invention, the mass ratio of the rubidium-cesium precipitate to water is preferably 1:2-3. In the present invention, the reaction conditions preferably include: a rotation speed of 600 rpm and a time of 2 hours. In the present invention, the chemical reaction formula of the reaction is as follows:

[0042] (Cs / Rb)MgPO4+2OH-=Cs + / Rb + +PO4 3- +Mg(OH)2.

[0043] In order to further illustrate the present invention, the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0044] The mother liquor used in the embodiment of the present invention is a high-salt mother liquor, and its specific composition is shown in Table 1. It should be pointed out that the method and content of the present invention are developed based on this mother liquor, but the content of the invention is not limited to the mother liquor with the composition shown in the table, and is applicable to other types of liquids containing rubidium and cesium.

[0045] Table 1 Component content of high salt mother liquor

[0046] Element <![CDATA[Na + ]]> <![CDATA[K + ]]> <![CDATA[Rb + ]]> <![CDATA[Cs + ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Cl - ]]> <![CDATA[Br - ]]> Concentration(g / L) 117.9 91.47 6.99 8.59 1.97 158.65 18.89

[0047] Example 1

[0048] Take two 25mL portions of high-salt mother liquor, add 1.56g of magnesium chloride hexahydrate and 1.34g of sodium phosphate respectively, stir until completely dissolved, then add the solution containing magnesium ions to the solution containing phosphate, and stir at a speed of 600r / min for 30min. After the reaction, filter with fast filter paper, and dry the solid precipitate in a 105℃ oven for 120min after deionization washing to obtain 1.97g of magnesium phosphate rubidium cesium precipitate. After testing, the concentrations of cesium and rubidium in the precipitated liquid are 0.39g / L and 1.07g / L respectively, and the precipitation rates of rubidium and cesium are calculated to be 95.41% and 84.66% respectively; in addition, magnesium phosphate rubidium cesium precipitate also contains 2.52% and 0.51% potassium ions and sodium ions, which are mass percentages.

[0049] The magnesium phosphate rubidium cesium solid was added to deionized water at a mass ratio of 1:2, and sodium hydroxide was added to adjust to 13.0, and stirred at a speed of 600r / min for 2h. After the reaction, it was filtered with a quick filter paper, and 0.15g of magnesium hydroxide solid was obtained after solid-liquid separation. The filtered solution was tested to be a rubidium-cesium solution with a content of approximately 81.2g / L cesium, 65.41g / L rubidium, 5.96g / L potassium, and 1.01g / L sodium.

[0050] Example 2

[0051] Take two 25mL portions of high-salt mother liquor, add 1.46g of magnesium chloride hexahydrate and 1.18g of sodium phosphate respectively, stir until completely dissolved, then add the solution containing magnesium ions to the solution containing phosphate, and stir at a speed of 600r / min for 30min. After the reaction, filter with fast filter paper, and dry the solid precipitate in a 105℃ oven for 120min after deionization washing to obtain 1.84g of magnesium phosphate rubidium cesium precipitate. After testing, the concentrations of cesium and rubidium in the precipitated liquid are 0.30g / L and 1.13g / L respectively, and the precipitation rates of rubidium and cesium are calculated to be 96.55% and 83.74% respectively; in addition, magnesium phosphate rubidium cesium precipitate also contains 3.01% and 0.79% potassium ions and sodium ions, which are mass percentages.

[0052] Add magnesium phosphate rubidium cesium solid to deionized water at a mass ratio of 1:2, and add sodium hydroxide to adjust to 14.0. Stir at a speed of 600r / min for 2h. After the reaction, filter with fast filter paper, and obtain 0.12g of magnesium hydroxide solid after solid-liquid separation. The filtered solution is about 80.69g / L of cesium, 68.55g / L of rubidium, 4.98g / L of potassium, and 1.59g / L of sodium.

[0053] Example 3

[0054] Take two 50mL portions of high-salt mother liquor, add 2.91g of magnesium chloride hexahydrate and 2.54g of sodium phosphate respectively, stir until completely dissolved, then add the solution containing magnesium ions to the solution containing phosphate, and stir at a speed of 600r / min for 30min. After the reaction, filter with fast filter paper, and dry the solid precipitate in a 105℃ oven for 120min after deionization washing to obtain 3.88g of magnesium phosphate rubidium cesium precipitate. After testing, the concentrations of cesium and rubidium in the precipitated liquid are 0.35g / L and 0.94g / L respectively, and the precipitation rates of rubidium and cesium are calculated to be 95.96% and 86.59% respectively; in addition, magnesium phosphate rubidium cesium precipitate also contains 3.01% and 0.79% potassium ions and sodium ions, which are mass percentages.

[0055] Add magnesium phosphate rubidium cesium solid to deionized water at a mass ratio of 1:3, and add sodium hydroxide to adjust to 14.0. Stir at a speed of 600r / min for 2h. After the reaction, filter with fast filter paper, and obtain 0.25g of magnesium hydroxide solid after solid-liquid separation. The filtered solution is about 94.52g / L of cesium, 74.19g / L of rubidium, 6.32g / L of potassium, and 3.88g / L of sodium.

[0056] Example 4

[0057] Take two 50mL portions of high-salt mother liquor, add 2.74g of magnesium chloride hexahydrate and 2.41g of sodium phosphate respectively, stir until completely dissolved, then add the solution containing magnesium ions to the solution containing phosphate, and stir at a speed of 600r / min for 30min. After the reaction, filter with fast filter paper, wash the solid precipitate with deionization, and dry it in a 105℃ oven for 120min to obtain 3.56g of magnesium phosphate rubidium cesium precipitate. After testing, the concentrations of cesium and rubidium in the precipitated liquid are 0.40g / L and 0.98g / L respectively, and the precipitation rates of rubidium and cesium are calculated to be 95.31% and 85.94% respectively; in addition, the magnesium phosphate rubidium cesium precipitate also contains 3.18% and 0.98% of potassium ions and sodium ions, which are the mass percentages.

[0058] The magnesium phosphate rubidium cesium solid was added to deionized water at a mass ratio of 1:3, and sodium hydroxide was added to adjust to 14.0. Stir at a speed of 600r / min for 2h. After the reaction, it was filtered with a quick filter paper, and 0.28g of magnesium hydroxide solid was obtained after solid-liquid separation. The filtered solution was tested to be a rubidium-cesium solution with a content of approximately 98.18g / L of cesium, 73.98g / L of rubidium, 7.81g / L of potassium, and 4.67g / L of sodium.

[0059] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for separating rubidium and cesium from a high-salt mother liquor, It is characterized in that The following steps are involved: 1) mixing a high-salt mother liquor with magnesium chloride to obtain a magnesium-containing solution; mixing the high salt mother liquor with sodium phosphate to obtain a phosphate-containing solution; The high salt mother liquor contains rubidium ions and cesium ions; 2) mixing the magnesium-containing solution obtained in step 1) with the phosphate-containing solution, stirring and reacting to obtain a stirred reactant; 3) separating the stirred reaction product obtained in step 2) into solid and liquid to obtain a precipitate containing rubidium and cesium; 4) Mixing the rubidium-cesium precipitate obtained in step 3) with water, adjusting the pH value to above 12.0, and reacting to obtain a reactant. After solid-liquid separation, the obtained solution contains rubidium and cesium, thereby achieving separation of rubidium and cesium from the high-salt mother liquor.

2. The method according to claim 1, It is characterized in that In the step 1), the concentration of sodium ions in the high-salt mother liquor is 117.9 g / L, the concentration of potassium ions is 91.47 g / L, the concentration of rubidium ions is 6.99 g / L, the concentration of cesium ions is 8.59 g / L, the concentration of calcium ions is 1.97 g / L, the concentration of chloride ions is 158.65 g / L, and the concentration of bromide ions is 18.89 g / L.

3. The method according to claim 1, It is characterized in that In the step 1), the mass ratio of the volume of the high-salt mother liquor to the magnesium chloride is 25-50 mL: 1.46-2.91 g.

4. The method according to claim 1, It is characterized in that In the step 1), the mass ratio of the volume of the high-salt mother liquor to the sodium phosphate is 25-50 mL: 1.18-2.54 g.

5. The method according to claim 1, It is characterized in that The stirring reaction conditions in step 2) include: a rotation speed of 600 rpm and a time of 30 min; The volume ratio of the magnesium-containing solution to the phosphate-containing solution is 1:

1.

6. The method according to claim 1, It is characterized in that After the solid-liquid separation in step 3), the obtained solid is dried to obtain a precipitate containing rubidium and cesium; The drying conditions include: temperature of 105° C. and time of 120 min.

7. The method according to claim 1, It is characterized in that In the step 4), the mass ratio of the rubidium-cesium precipitate to water is 1:2-3.

8. The method according to claim 1, It is characterized in that The reaction conditions of step 4) include: a rotation speed of 600 rpm and a reaction time of 2 hours.

Citation Information

Patent Citations

  • Method for extracting alkali metal from salt lake brine and seawater through membrane extraction-back extraction

    CN102312110A

  • Process for the complete separation of technically pure rubidium (and cesium) salts from those of the alkalis

    DE515851A

  • Method for removing cesium and strontium

    JP2013152218A