Method for synthesizing micron-sized anhydrous magnesium carbonate crystal by one-step method
The one-step hydrothermal method is used to convert magnesium hydrogenate into anhydrous magnesium carbonate crystals, which solves the problems of high cost and complex processes in the existing technology, and realizes the efficient and environmentally friendly production of anhydrous magnesium carbonate, and prepares high-value-added non-existent Hydromagnesium carbonate crystals have good dispersion and particle size uniformity, and are suitable for industrial applications.
Patent Information
- Application Number
- CN202410975419.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing synthesis methods of anhydrous magnesium carbonate have problems such as high cost, complex process flow, high energy consumption, unsatisfactory product morphology, uneven particle size and waste liquid pollution, making it difficult to achieve large-scale industrial production.
A one-step hydrothermal method is used to convert natural magnesium hydrocarbonate into micron-scale anhydrous magnesium carbonate crystals. A mixture of deionized water and anhydrous ethanol is used as a solvent to prepare a 2-hydroxybenzoic acid solution and react with magnesium hydrocarbonate to carry out water. After heat treatment, it is cooled and dried naturally to obtain anhydrous magnesium carbonate crystals with uniform particle size and regular morphology, and are reused using waste liquid.
It has achieved simplification of the process flow, reduced production costs, and zero emission of waste liquid. It has prepared high added value anhydrous magnesium carbonate crystals, which have good dispersion and particle size uniformity, meet the requirements of green chemistry, and has large-scale industrialization. potential.
Smart Images

Figure CN118908252A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing and waste liquid recycling, and specifically relates to a one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals. Background Art
[0002] So far, my country's proven reserves of brucite ore exceed 25 million tons, ranking among the top in the world. The grade of brucite ore is high, mainly fibrous brucite, and less blocky brucite. Among them, the brucite mine in Liaoning Province has high ore quality, is easy to mine, and is large in scale. The brucite in Kuandian, Liaoning Province basically reaches its theoretical content. my country's brucite research started late, and it was mainly exported, or it was simply crushed and used to produce refractory and thermal insulation materials with low added value. In recent years, some mining companies have begun to use it to produce magnesium hydroxide flame retardants, but the scale is small, the energy consumption is high, and the processing technology is at a general level. In addition, the main problem in the application of brucite flame retardants is that the surface polarity of brucite is strong and its compatibility with high molecular polymers is poor, resulting in a decrease in polymer processing performance and mechanical properties. As a result, a large amount of brucite has not been effectively utilized, resulting in a waste of brucite resources. Therefore, high-value, high-quality and efficient utilization of my country's abundant brucite resources is of great significance to the national economic development.
[0003] Anhydrous magnesium carbonate (MgCO3) is a single crystal of magnesium carbonate salt. It exists in the form of dolomite in nature. It has the characteristics of low price, non-toxicity, and good biocompatibility. It is an important multifunctional inorganic chemical material.
[0004] Anhydrous magnesium carbonate has been the subject of research due to its wide application and research value. Because of its wide visible light emission region, it has broad application prospects in the field of optics. In the field of geochemistry, the crystallization study of anhydrous magnesium carbonate helps to understand the structural evolution of magnesite. With the development of materials science, anhydrous magnesium carbonate crystals with regular morphology can be used as a template for material synthesis. In addition, anhydrous magnesium carbonate crystals can also be used as a precursor to prepare high-purity magnesium oxide, which is used in adsorption, catalysis, antibacterial and other fields.
[0005] At present, the main methods for synthesizing anhydrous magnesium carbonate include carbonization, solid-phase reaction, precipitation crystallization and hydrothermal method. Among them, carbonization, solid-phase reaction and precipitation crystallization are difficult to obtain ideal anhydrous magnesium carbonate. Although the hydrothermal method can overcome the shortcomings of the above methods, it is very easy to generate basic magnesium carbonate. It is difficult to obtain a single-phase anhydrous magnesium carbonate. The use of additives will affect the purity of the product. In addition, most of the above methods use chemical reagents as raw materials, with high synthesis costs and contain Cl - 、SO4 2- 、NO3 2-Waste liquids such as magnesium carbonate are easy to pollute the environment and are difficult to produce on a large scale. Some researchers have successfully prepared anhydrous magnesium carbonate crystals using forsterite, magnesite, and dolomite as raw materials, but the process is complex, energy-intensive, and time-consuming. Overall, the morphology of the anhydrous magnesium carbonate products currently prepared is not ideal, and most of the products have the disadvantages of being too large in particle size, unevenly distributed, and poorly dispersed. Summary of the invention
[0006] In view of the deficiencies of the prior art, the present invention provides a one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals. The method uses natural brucite ore as raw material and adopts a hydrothermal method to synthesize anhydrous magnesium carbonate crystals in one step, which has the advantages of simple process flow, low production cost, uniform particle size distribution, good dispersibility and regular morphology of the prepared anhydrous magnesium carbonate; the obtained waste liquid can be reused to prepare high-value-added anhydrous magnesium carbonate crystals, achieving zero waste liquid discharge and meeting the requirements of green chemistry.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0009] (1) using a mixed solution of deionized water and anhydrous ethanol as a solvent to prepare a 2-hydroxybenzoic acid solution, adding brucite to the solution, stirring and mixing to obtain a mixed slurry;
[0010] (2) placing the mixed slurry under hydrothermal conditions to react, and after the reaction is completed, naturally cooling to room temperature, performing solid-liquid separation, and obtaining solid and waste liquid;
[0011] (3) drying the solid obtained in step (2) to obtain anhydrous magnesium carbonate crystals;
[0012] or
[0013] After collecting the waste liquid obtained by solid-liquid separation in step (2), brucite and 2-hydroxybenzoic acid are added in a certain proportion, and the mixture is stirred and reacted under hydrothermal conditions. After the reaction is completed, the mixture is naturally cooled to room temperature and solid-liquid separation is performed. After the obtained solid is dried, anhydrous magnesium carbonate crystals are obtained.
[0014] in:
[0015] In the step (1), the volume ratio of deionized water to anhydrous ethanol is (1-2):1, and the concentration of the obtained 2-hydroxybenzoic acid is 0.1-0.5 mol / L.
[0016] In the step (1), the particle size of brucite is 100 to 500 meshes.
[0017] In the step (1), the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in brucite is (1-3):1.
[0018] In the step (2), the hydrothermal temperature of the reaction between 2-hydroxybenzoic acid and brucite is 130-240° C., the hydrothermal time is 3-15 h, and the stirring rate is 100-600 r / min.
[0019] In the step (3), the drying temperature is 80 to 140° C. and the drying time is 6 to 24 hours.
[0020] In the step (3), the size of the anhydrous magnesium carbonate crystals is 2 to 10 μm, and the average particle size is 5 to 15 μm.
[0021] In the step (3), the molar ratio of the supplemented 2-hydroxybenzoic acid to the magnesium hydroxide in the brucite is (0.5-1):1, excluding 1:1.
[0022] In the step (3), the amount of brucite added is the same as the amount of brucite added in the step (1), based on the concentration of magnesium hydroxide.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention directly uses brucite as raw material, which has abundant sources and low costs and can replace magnesium salt chemical reagents.
[0025] 2. The present invention realizes the one-step conversion of natural minerals into high-value-added anhydrous magnesium carbonate, and the waste liquid can be reused. The process is simple, the cycle is short, and it is environmentally friendly, and has the potential for large-scale industrialization.
[0026] 3. The product synthesized by the present invention is a pure phase anhydrous magnesium carbonate crystal with good dispersion, uniform particle size and complete crystal morphology. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 XRD patterns of anhydrous magnesium carbonate crystals prepared in Examples 1-3 and 6-7 of the present invention;
[0028] Figure 2 Particle size distribution diagram of anhydrous magnesium carbonate crystals prepared in Examples 1-3 and 6-7 of the present invention;
[0029] Figure 3 SEM image of anhydrous magnesium carbonate prepared in Example 1 of the present invention; the upper right is a high-magnification SEM image;
[0030] Figure 4 SEM image of anhydrous magnesium carbonate prepared in Example 2 of the present invention; the upper right is a high-magnification SEM image;
[0031] Figure 5SEM image of anhydrous magnesium carbonate prepared in Example 3 of the present invention; the upper right is a high-magnification SEM image;
[0032] Figure 6 SEM image of anhydrous magnesium carbonate prepared in Example 6 of the present invention; the upper right is a high-magnification SEM image;
[0033] Figure 7 SEM image of anhydrous magnesium carbonate prepared in Example 7 of the present invention; the upper right image is a high-magnification SEM image. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work all fall within the scope of protection of the present invention.
[0035] The following provides a specific embodiment of a one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to the present invention.
[0036] Example 1
[0037] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0038] (1) using a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1 as a solvent, preparing a 0.25 mol / L 2-hydroxybenzoic acid solution, adding brucite with a particle size of 200 meshes to the solution, wherein the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in the brucite is 2:1, and mixing by magnetic stirring to obtain a mixed slurry;
[0039] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 180° C., a hydrothermal time of 12 h, and a stirring rate of 400 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0040] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0041] The XRD spectrum of anhydrous magnesium carbonate crystals prepared by the method provided in this embodiment is as follows: Figure 1 The particle size distribution diagram is shown in Figure 2 As shown in the SEM images Figure 3 As shown, the obtained product is a pure phase rhombic anhydrous magnesium carbonate crystal with a length of 2 to 6 μm, a width of 1 to 5 μm and an average particle size of 9 μm.
[0042] Example 2
[0043] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0044] (1) using a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1 as a solvent, preparing a 0.20 mol / L 2-hydroxybenzoic acid solution, adding brucite with a particle size of 200 meshes to the solution, wherein the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in the brucite is 1.5:1, and mixing by magnetic stirring to obtain a mixed slurry;
[0045] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 180° C., a hydrothermal time of 12 h, and a stirring rate of 600 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0046] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0047] The XRD spectrum of anhydrous magnesium carbonate crystals prepared by the method provided in this embodiment is as follows: Figure 1 The particle size distribution diagram is shown in Figure 2 As shown in the SEM images Figure 4 As shown, the obtained product is a pure phase rhombohedral anhydrous magnesium carbonate crystal with a diameter of 2 to 4 μm and an average particle size of 6 μm.
[0048] Example 3
[0049] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0050] (1) using a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1 as a solvent, preparing a 0.25 mol / L 2-hydroxybenzoic acid solution, adding brucite with a particle size of 200 meshes to the solution, wherein the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in the brucite is 2:1, and mixing by magnetic stirring to obtain a mixed slurry;
[0051] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 180° C., a hydrothermal time of 9 h, and a stirring rate of 300 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0052] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0053] The XRD spectrum of anhydrous magnesium carbonate crystals prepared by the method provided in this embodiment is as follows: Figure 1 The particle size distribution diagram is shown in Figure 2 As shown in the SEM images Figure 5As shown, the obtained product is a pure phase rhombohedral anhydrous magnesium carbonate crystal with a diameter of 2 to 5 μm and an average particle size of 9 μm.
[0054] Example 4
[0055] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0056] (1) using a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1 as a solvent, preparing a 0.4 mol / L 2-hydroxybenzoic acid solution, adding brucite with a particle size of 200 meshes to the solution, wherein the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in the brucite is 1.5:1, and mixing by magnetic stirring to obtain a mixed slurry;
[0057] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 210° C., a hydrothermal time of 8 h, and a stirring rate of 100 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0058] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0059] Example 5
[0060] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0061] (1) using a mixture of deionized water and anhydrous ethanol in a volume ratio of 1:1 as a solvent, preparing a 0.1 mol / L 2-hydroxybenzoic acid solution, adding brucite with a particle size of 200 meshes to the solution, wherein the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in the brucite is 1:1, and mixing by magnetic stirring to obtain a mixed slurry;
[0062] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 160° C., a hydrothermal time of 11 h, and a stirring rate of 200 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0063] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0064] Example 6
[0065] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0066] (1) collecting the waste liquid obtained in Example 1, adding 2-hydroxybenzoic acid and brucite at a molar ratio of 2-hydroxybenzoic acid to brucite of 2:3 until the concentration of magnesium hydroxide in the brucite is the same as that added in Example 1, and mixing by magnetic stirring to obtain a mixed slurry;
[0067] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 180° C., a hydrothermal time of 12 h, and a stirring rate of 400 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0068] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0069] The XRD spectrum of anhydrous magnesium carbonate crystals prepared by the method provided in this embodiment is as follows: Figure 1 The particle size distribution diagram is shown in Figure 2 As shown in the SEM images Figure 6 As shown, the obtained product is a pure phase prismatic anhydrous magnesium carbonate crystal with a length of about 9 μm, a width of about 5 μm and an average particle size of 9 μm.
[0070] Example 7
[0071] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0072] (1) collecting the waste liquid obtained in Example 2, adding 2-hydroxybenzoic acid and brucite at a molar ratio of 2-hydroxybenzoic acid to brucite of 5:6 until the concentration of magnesium hydroxide in the brucite is the same as that added in Example 2, and mixing by magnetic stirring to obtain a mixed slurry;
[0073] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 180° C., a hydrothermal time of 12 h, and a stirring rate of 600 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0074] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0075] The XRD spectrum of anhydrous magnesium carbonate crystals prepared by the method provided in this embodiment is as follows: Figure 1 The particle size distribution diagram is shown in Figure 2 As shown in the SEM images Figure 7 As shown, the obtained product is a pure phase rhombohedral anhydrous magnesium carbonate crystal with a diameter of 3 to 5 μm and an average particle size of 9 μm.
[0076] Example 8
[0077] A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, specifically comprising the following steps:
[0078] (1) collecting the waste liquid obtained in Example 3, adding 2-hydroxybenzoic acid and brucite at a molar ratio of 2-hydroxybenzoic acid to brucite of 4:7 until the concentration of magnesium hydroxide in the brucite is the same as that added in Example 3, and mixing by magnetic stirring to obtain a mixed slurry;
[0079] (2) The mixed slurry was transferred to a high-pressure reactor for reaction at a hydrothermal temperature of 180° C., a hydrothermal time of 9 h, and a stirring rate of 300 r / min. After the reaction was completed, the mixture was naturally cooled to room temperature and solid-liquid separation was performed;
[0080] (3) Drying the solid obtained in step (2) in an oven at 100° C. for 10 h to obtain anhydrous magnesium carbonate crystals.
[0081] As can be seen from the above embodiments, in the process of preparing anhydrous magnesium carbonate crystals, the present invention can directly convert natural brucite into pure phase anhydrous magnesium carbonate crystals by a one-step hydrothermal method, and the waste liquid generated can be reused to improve the comprehensive utilization rate of resources. The present invention not only has a simple process flow, low production cost, and no by-product pollution, but also has great industrialization potential, and the obtained anhydrous magnesium carbonate particles have good dispersibility, uniform particle size distribution, and regular morphology, and can be used as a high-quality powder filler, and is widely used in the fields of reinforcement and flame retardant of composite materials and optoelectronic materials.
[0082] The above embodiments are used to describe the implementation of the present invention in detail. However, the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals, characterized in that: The specific steps include: (1) using a mixed solution of deionized water and anhydrous ethanol as a solvent to prepare a 2-hydroxybenzoic acid solution, adding brucite to the solution, stirring and mixing to obtain a mixed slurry; (2) placing the mixed slurry under hydrothermal conditions to react, and after the reaction is completed, naturally cooling to room temperature, performing solid-liquid separation, and obtaining solid and waste liquid; (3) drying the solid obtained in step (2) to obtain anhydrous magnesium carbonate crystals; or After collecting the waste liquid obtained by solid-liquid separation in step (2), brucite and 2-hydroxybenzoic acid are added in a certain proportion, and the mixture is stirred and reacted under hydrothermal conditions. After the reaction is completed, the mixture is naturally cooled to room temperature and solid-liquid separation is performed. After the obtained solid is dried, anhydrous magnesium carbonate crystals are obtained.
2. The method for synthesizing micron-sized anhydrous magnesium carbonate crystals in a one-step process according to claim 1, wherein: In the step (1), the volume ratio of deionized water to anhydrous ethanol is (1-2):1, and the concentration of the obtained 2-hydroxybenzoic acid is 0.1-0.5 mol / L.
3. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (1), the particle size of brucite is 100 to 500 meshes.
4. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (1), the molar ratio of 2-hydroxybenzoic acid in the solution to magnesium hydroxide in brucite is (1-3):
1.
5. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (2), the hydrothermal temperature of the reaction between 2-hydroxybenzoic acid and brucite is 130-240° C., the hydrothermal time is 3-15 h, and the stirring rate is 100-600 r / min.
6. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (3), the drying temperature is 80 to 140° C. and the drying time is 6 to 24 hours.
7. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (3), the size of the anhydrous magnesium carbonate crystals is 2 to 10 μm, and the average particle size is 5 to 15 μm.
8. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (3), the molar ratio of the supplemented 2-hydroxybenzoic acid to the magnesium hydroxide in the brucite is (0.5-1):1, excluding 1:
1.
9. A one-step method for synthesizing micron-sized anhydrous magnesium carbonate crystals according to claim 1, characterized in that: In the step (3), the amount of brucite added is the same as the amount of brucite added in the step (1), based on the concentration of magnesium hydroxide.