Nickel oxide nanoparticles and preparation method thereof

By using gelatin and polyvinylpyrrolidone additives to prepare nickel oxide nanoparticles, the problem of difficult control of particle size and shape in the prior art is solved, and nickel oxide nanoparticles with uniform particle size and good dispersion are achieved, meeting the needs of various applications .

CN118908310APending Publication Date: 2024-11-08CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957061.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing nickel oxide nanoparticle preparation methods are difficult to control the particle size and shape, resulting in uneven particle size and poor dispersion, affecting its catalytic and energy storage performance.

Method used

Gelatin and polyvinylpyrrolidone were used as additives to prepare alkaline nickel carbonate precursors, and calcined at 650-700°C to obtain nickel oxide nanoparticles, and the particle size and morphology were controlled by regulating the synthesis conditions.

Benefits of technology

The nickel oxide nanoparticles have achieved uniform particle size and good dispersion, meet different application needs, and have shown wide application prospects in the fields of catalysis, battery materials and biomedical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908310A_ABST
    Figure CN118908310A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of nickel oxide nanoparticles. The preparation method comprises the following steps: preparing a gelatin aqueous solution; adding metal nickel salt into the gelatin aqueous solution to obtain a mixed solution A; polyvinylpyrrolidone is adopted as a surfactant and added into the mixed solution A, and a mixed solution B is obtained; adding a proper amount of ammonia water into the mixed solution B, and carrying out precipitation reaction for generating nickel hydroxide to obtain a mixture C; adding a proper amount of carbonate solution into the mixture C, and carrying out precipitation reaction for generating basic nickel carbonate to obtain a mixture D; heating and evaporating the mixture D to dryness, and carrying out solid-liquid separation to obtain dry gel of basic nickel carbonate; washing, drying and grinding to obtain a basic nickel carbonate precursor; and calcining the basic nickel carbonate precursor to obtain the nickel oxide nanoparticles. According to the preparation method of the nickel oxide nano-particles, gelatin and polyvinylpyrrolidone are adopted as auxiliaries to prepare the basic nickel carbonate precursor, the basic nickel carbonate precursor is further decomposed at high temperature to obtain the nickel oxide nano-particles, the nickel oxide nano-particles have the advantages of being good in dispersity and stability, the particle size and morphology of the nickel oxide nano-particles can be adjusted and controlled, and different application requirements can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano materials, and in particular to nickel oxide nano particles and a preparation method thereof. Background Art

[0002] Nickel oxide (NiO) powder is an important industrial raw material. It has excellent catalytic, electrochemical and magnetic properties and shows great application potential in the fields of electronic devices, catalysis, power systems and environmental protection. However, nickel oxide of different sizes has different properties. The particle size, shape and synthesis route of nickel oxide are crucial to its electrical, optical and magnetic properties. The preparation method of nickel oxide nanoparticles with uniform size and good dispersion has attracted wide attention.

[0003] Conventional nickel oxide preparation methods, such as hydrothermal method, solvothermal method, precipitation method, chemical vapor deposition method, etc., have certain limitations in the preparation of nickel oxide nanoparticles. First, the size and shape of the prepared particles are difficult to control; second, nickel oxide nanoparticles agglomerate during the preparation process, resulting in poor dispersion. Studies have found that the size uniformity and dispersion of nickel oxide nanoparticles have an important influence on their performance. Uniform particle size and good dispersion can make them exhibit superior catalytic and energy storage properties.

[0004] In the prior art, the methods for preparing nickel oxide include: preparing nickel oxide particles by calcining NiCl2-(NH4)CO3 and ethanol with air to obtain a precipitate, or preparing nickel oxide particles by annealing a precipitate obtained by adding Ni(OH)2 to an HNO3 solution. Although these methods reduce the size of the oxide precursor by adding an organic solvent and a surfactant, it is still difficult to avoid the agglomeration of nanoparticles in the subsequent calcination process to synthesize nickel oxide.

[0005] Therefore, how to use a simple and efficient synthesis method to obtain nickel oxide nanoparticles with uniform particle size and good dispersion remains a challenge. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing nickel oxide nanoparticles, using gelatin and polyvinyl pyrrolidone as auxiliary agents to prepare a basic nickel carbonate precursor, and then further calcining to obtain nickel oxide nanoparticles. The prepared product has the characteristics of uniform particle size and good dispersibility, and by adjusting the synthesis conditions, the particle size can be controlled to meet different application requirements.

[0007] The technical solution of the present invention is as follows:

[0008] A method for preparing nickel oxide nanoparticles comprises the following steps:

[0009] Step S1, taking an appropriate amount of gelatin to prepare a gelatin aqueous solution with a mass concentration of 4.76-9.09%;

[0010] Specifically, the mass concentration of the gelatin aqueous solution may be 4.76%, 5%, 5.5%, 6%, 7%, 8% or 9.09%, or other values ​​within the range;

[0011] Step S2, using nickel nitrate hexahydrate Ni(NO3)2·6H2O as a metal nickel source, adding the metal nickel salt to a gelatin aqueous solution, stirring, and obtaining a mixed solution A, wherein the mass ratio of nickel nitrate hexahydrate to gelatin is 1:1-2; specifically, the mass ratio of nickel nitrate hexahydrate to gelatin can be 1:1, 1:1.5 or 1:2, or other values ​​within this range;

[0012] Step S3, using polyvinyl pyrrolidone as a surfactant, adding it to the mixed solution A, stirring, and obtaining a mixed solution B, wherein the mass ratio of polyvinyl pyrrolidone to gelatin is 1:1-1.5; specifically, the mass ratio of polyvinyl pyrrolidone to gelatin can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, or other values ​​within the range;

[0013] Step S4, adding an appropriate amount of aqueous ammonia to the mixed solution B to perform a precipitation reaction to generate nickel hydroxide, thereby obtaining a mixture C;

[0014] Step S5, adding an appropriate amount of carbonate solution to the mixture C to perform a precipitation reaction to generate basic nickel carbonate, thereby obtaining a mixture D;

[0015] Step S6, heating and evaporating the mixture D to perform solid-liquid separation to obtain a xerogel of basic nickel carbonate;

[0016] Step S7, washing, drying, and grinding to obtain a basic nickel carbonate precursor;

[0017] Step S8, calcining the basic nickel carbonate precursor at 650-700°C to obtain nickel oxide nanoparticles; specifically, the calcination temperature can be 650°C, 660°C, 670°C, 680°C, 690°C or 700°C, or other values ​​within this range.

[0018] Further, in step S4, the concentration of ammonia water is 7-10%, and the volume ratio of ammonia water to mixed solution B is 1:0.2-0.5. Specifically, the concentration of ammonia water can be 7%, 8%, 9% or 10%, or other values ​​within the range; the volume ratio of ammonia water to mixed solution B is 1:0.2, 1:0.3, 1:0.4 or 1:0.5, or other values ​​within the range.

[0019] Further, in step S5, the concentration of carbonate ions in the carbonate solution is 1-1.5M, and the volume ratio of the carbonate solution to the mixture C is 1:0.5-1.5. Specifically, the concentration of carbonate ions in the carbonate solution is 1M, 1.2M or 1.5M, or other values ​​within the range; the volume ratio of the carbonate solution to the mixture C is 1:0.5, 1:0.8, 1:1, 1:1.2 or 1:1.5, or other values ​​within the range.

[0020] Furthermore, the carbonate is at least one of sodium carbonate, ammonium carbonate and ammonium bicarbonate.

[0021] Further, in step S6, the heating temperature is 80-110° C. Specifically, the mixture is first heated to 80° C. and stirred for 6 hours to form a gel state, and then the temperature is continued to be raised to 110° C. to evaporate the solution to separate the solid and liquid, and stirred for 2 hours to obtain a dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O.

[0022] Furthermore, in step S7, deionized water or a mixture of deionized water and ethanol is used as a washing dispersion, and washing is performed by suction filtration or centrifugal separation.

[0023] Further, in step S8, the heating rate is 2-5°C / min; specifically, the heating rate may be 2°C / min, 3°C / min, 4°C / min or 5°C / min, or other values ​​within the range.

[0024] The present invention also provides a dispersible nickel oxide nanoparticle, which is prepared by the above method.

[0025] Compared with the prior art, the nickel oxide nanoparticles and the preparation method thereof provided by the present invention have the following beneficial effects:

[0026] 1. The method for preparing nickel oxide nanoparticles provided by the present invention uses gelatin and polyvinyl pyrrolidone as auxiliary agents to prepare a basic nickel carbonate precursor, and then further calcines to obtain nickel oxide nanoparticles. Polyvinyl pyrrolidone, as a surfactant, has the effect of reducing the size of basic nickel carbonate particles, and gelatin, as a porous template, prevents the agglomeration of nickel oxide nanoparticles during the calcination process. Therefore, the prepared product has the characteristics of uniform particle size and good dispersibility. By adjusting the synthesis conditions, the particle size can be controlled to meet different application requirements.

[0027] 2. In the preparation method of nickel oxide nanoparticles provided by the present invention, gelatin and polyvinyl pyrrolidone can interact with basic nickel carbonate particles and nickel oxide nanoparticles generated by conversion of basic nickel carbonate through surface groups to control the growth rate and crystal morphology of the nanoparticles, thereby achieving precise control of the size and morphology of the nanoparticles, so that the nickel oxide nanoparticles meet the needs of different application fields.

[0028] 3. The method for preparing nickel oxide nanoparticles provided by the present invention is to add a carbonate solution to a nickel hydroxide reactant to generate basic nickel carbonate, and then calcine the basic nickel carbonate gel to obtain nickel oxide nanoparticles. Compared with the calcination of nickel hydroxide in the prior art, the production of flakes can be reduced, the particles are more dispersed, and the particle size is more uniform.

[0029] Fourth, the preparation method of nickel oxide nanoparticles provided by the present invention achieves high dispersibility of nickel oxide nanoparticles, making them have broad application prospects. For example: in the field of catalysts, nickel oxide nanoparticles can be used as active components of high-efficiency catalysts to promote various chemical reactions; in the field of battery materials, nickel oxide nanoparticles can be used to prepare high-performance lithium-ion batteries and supercapacitors; in the field of sensors, nickel oxide nanoparticles can be used to prepare highly sensitive and highly selective gas sensors and biosensors; in addition, since gelatin and polyvinyl pyrrolidone have good biocompatibility, the prepared highly dispersible nickel oxide nanoparticles can also be used in the biomedical field, such as drug delivery, bioimaging and tissue engineering. The method of the present invention has a simple preparation process and is suitable for large-scale preparation and industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. The drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 is a crystal phase structure diagram of NiO prepared in Example 1 of the present invention;

[0032] Figure 2 is a surface microscopic morphology of NiO prepared in Example 1 of the present invention;

[0033] Figure 3 is a crystal phase structure diagram of NiO prepared in Example 2 of the present invention;

[0034] Figure 4 is a surface microscopic morphology of NiO prepared in Example 2 of the present invention;

[0035] Figure 5is a crystal phase structure diagram of NiO prepared in Example 3 of the present invention;

[0036] Figure 6 is a surface microscopic morphology of NiO prepared in Example 3 of the present invention;

[0037] Figure 7 is a surface microscopic morphology of NiO prepared in Example 4 of the present invention;

[0038] Figure 8 is a surface microscopic morphology of NiO prepared in Example 5 of the present invention;

[0039] Fig. 9 is a surface microscopic morphology of NiO prepared in Example 6 of the present invention;

[0040] Fig.10 This is a surface microscopic morphology of NiO prepared in Example 7 of the present invention. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention and to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are further described below.

[0042] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0043] Example 1

[0044] In this embodiment, gelatin is used alone as a template size limiting agent to prepare nickel oxide, including the following steps:

[0045] Step S1, using gelatin as an organic macromolecular template and size limiting agent. Add 1g of gelatin to 20mL of deionized water and stir thoroughly to accelerate dissolution; then place the gelatin solution on a magnetic heating stirrer, heat to 50°C, and continue stirring until the gelatin is completely dissolved and the solution becomes transparent;

[0046] Step S2, using nickel nitrate hexahydrate Ni(NO3)2·6H2O as a metal nickel source, adding 1 g of nickel nitrate hexahydrate Ni(NO3)2·6H2O into the gelatin solution, and continuing to stir until dissolved;

[0047] Step S3, preparing 7% dilute ammonia water as an alkali source, dripping the dilute ammonia water dropwise into the mixed solution of step S2, adjusting the pH to 8, so as to perform a precipitation reaction to generate nickel hydroxide Ni(OH)2; the chemical reaction formula of this step is as follows:

[0048] Ni(NO3)2+2NH4OH→Ni(OH)2↓+2NH4NO3

[0049] Step S4, preparing a carbonate solution with a carbonate ion concentration of 1.5 M, adding 100 mL of the carbonate solution to the solution of step S3, and mixing them to perform a precipitation reaction to generate basic nickel carbonate NiCO3·2Ni(OH)2·4H2O;

[0050] Step S5, heating the mixture of step S4 to 80° C., continuing to stir for 6 hours to form a gel state, then continuing to heat to 110° C. to evaporate the solution to separate the solid and liquid, stirring for 2 hours, to obtain a dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O;

[0051] Step S6, washing the dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O by alternating centrifugation with water and ethanol to remove excess PVP and organic matter, and then drying it in an oven at 60°C, taking out the dried precipitate and grinding it in a mortar for 30 minutes, adding a small amount of ethanol during the process to make the powder obtained after grinding more uniformly dispersed, and obtaining a basic nickel carbonate (NiCO3·2Ni(OH)2·4H2O) precursor;

[0052] Step S7, calcining the prepared basic nickel carbonate precursor in a muffle furnace at 700°C for 2h (heating rate 5°C / min) to obtain nickel oxide particles. The chemical reaction formula of this step is as follows:

[0053] NiCO3·2Ni(OH)2·4H2O→3NiO+6H2O+CO2

[0054] Please refer to Figure 1 and Figure 2 ,in Figure 1 is a crystal phase structure diagram of NiO prepared in Example 1 of the present invention; Figure 2 : is a surface microscopic morphology of NiO prepared in Example 1 of the present invention. Figure 1 It can be seen that the prepared NiO material has the same diffraction peak position as the PDF card 75-0197 of the standard NiO material, indicating that a pure phase NiO material has been obtained. The surface micromorphology of the NiO material was studied by scanning electron microscopy (SEM). Figure 2As shown, it can be seen that the NiO material is a particle with a size of about 100 nm. Due to the lack of the surfactant regulation effect of PVP, the prepared nanoparticles are larger in size and unevenly distributed.

[0055] Example 2

[0056] In this embodiment, polyvinyl pyrrolidone (PVP) is used alone as a surfactant to prepare NiO, comprising the following steps:

[0057] Step S1, using nickel nitrate hexahydrate Ni(NO3)2·6H2O as a metallic nickel source, adding 1 g of nickel nitrate hexahydrate Ni(NO3)2·6H2O into 20 mL of deionized water, and stirring until dissolved;

[0058] Step S2, using PVP as a surfactant, adding 1 g of polyvinyl pyrrolidone (PVP) to the solution of step S1, and stirring thoroughly until dissolved;

[0059] Step S3, preparing 7% dilute ammonia water as an alkali source, dripping the dilute ammonia water dropwise into the mixed solution of step S2, adjusting the pH to 8, so as to perform a precipitation reaction to generate nickel hydroxide Ni(OH)2; the chemical reaction formula of this step is as follows:

[0060] Ni(NO3)2+2NH4OH→Ni(OH)2↓+2NH4NO3

[0061] Step S4, preparing a carbonate solution with a carbonate ion concentration of 1.5 M, adding 100 mL of the carbonate solution to the solution of step S3, and mixing them to perform a precipitation reaction to generate basic nickel carbonate NiCO3·2Ni(OH)2·4H2O;

[0062] Step S5, heating the mixture of step S4 to 80° C., continuing to stir for 6 hours to form a gel state, then continuing to heat to 110° C. to evaporate the solution to separate the solid and liquid, stirring for 2 hours, to obtain a dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O;

[0063] Step S6, washing the dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O by alternating centrifugation with water and ethanol to remove excess PVP and organic matter, and then drying it in an oven at 60°C, taking out the dried precipitate and grinding it in a mortar for 30 minutes, adding a small amount of ethanol during the process to make the powder obtained after grinding more uniformly dispersed, and obtaining a basic nickel carbonate (NiCO3·2Ni(OH)2·4H2O) precursor;

[0064] Step S7, calcining the prepared basic nickel carbonate precursor in a muffle furnace at 700°C for 2h (heating rate 5°C / min) to obtain nickel oxide particles. The chemical reaction formula of this step is as follows:

[0065] NiCO3·2Ni(OH)2·4H2O→3NiO+6H2O+CO2

[0066] Please combine Figure 3 and Figure 4 ,in Figure 3 is a crystal phase structure diagram of NiO prepared in Example 2 of the present invention; Figure 4 : is a surface microscopic morphology of NiO prepared in Example 2 of the present invention. Figure 3 It can be seen that the prepared NiO material has the same diffraction peak position as the PDF card 75-0197 of the standard NiO material, indicating that a pure phase NiO material has been obtained. The surface micromorphology of the NiO material was studied by scanning electron microscopy (SEM). Figure 4 As shown, it can be seen that the NiO material is a particle with a size of about 200 nm. Due to the lack of the regulatory effect of gelatin, the prepared nanoparticles are agglomerated and have a larger size.

[0067] Example 3

[0068] In this embodiment, gelatin and polyvinyl pyrrolidone (PVP) are used as a size limiting agent and a surfactant to prepare nickel oxide, comprising the following steps:

[0069] Step S1, using gelatin as an organic macromolecular template and size limiting agent. Add 1g of gelatin to 20mL of deionized water and stir thoroughly to accelerate dissolution; then place the gelatin solution on a magnetic heating stirrer, heat to 50°C, and continue stirring until the gelatin is completely dissolved and the solution becomes transparent;

[0070] Step S2, using nickel nitrate hexahydrate Ni(NO3)2·6H2O as a metal nickel source, adding 1 g of nickel nitrate hexahydrate Ni(NO3)2·6H2O into the gelatin solution, and continuing to stir until dissolved;

[0071] Step S3, using polyvinyl pyrrolidone (PVP) as a surfactant, adding 1 g of polyvinyl pyrrolidone (PVP) to the mixed solution of step S2, and stirring thoroughly until dissolved;

[0072] Step S4, preparing 7% by mass dilute ammonia water as an alkali source, dripping the dilute ammonia water dropwise into the mixed solution of step S3, adjusting the pH to 8, so as to perform a precipitation reaction to generate nickel hydroxide Ni(OH)2; the chemical reaction formula of this step is as follows:

[0073] Ni(NO3)2+2NH4OH→Ni(OH)2↓+2NH4NO3

[0074] Step S5, preparing a carbonate solution with a carbonate ion concentration of 1.5 M, adding 100 mL of the carbonate solution to the solution of step S3, and mixing them to perform a precipitation reaction to generate basic nickel carbonate NiCO3·2Ni(OH)2·4H2O;

[0075] Step S6, heating the mixture of step S5 to 80° C., continuing to stir for 6 hours to form a gel state, then continuing to heat to 110° C. to evaporate the solution to separate the solid and liquid, stirring for 2 hours, to obtain a dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O;

[0076] Step S7, washing the dry gel of basic nickel carbonate NiCO3·2Ni(OH)2·4H2O by alternating centrifugation with water and ethanol to remove excess PVP and organic matter, and then drying it in an oven at 60°C, taking out the dried precipitate and grinding it in a mortar for 30 minutes, adding a small amount of ethanol during the process to make the powder obtained after grinding more uniformly dispersed, and obtaining a basic nickel carbonate (NiCO3·2Ni(OH)2·4H2O) precursor;

[0077] Step S8, calcining the prepared basic nickel carbonate precursor in a muffle furnace at 700°C for 2h (heating rate 5°C / min) to obtain nickel oxide particles. The chemical reaction formula of this step is as follows:

[0078] NiCO3·2Ni(OH)2·4H2O→3NiO+6H2O+CO2

[0079] Please refer to Figure 5 and Figure 6 ,in Figure 5 is a crystal phase structure diagram of NiO prepared in Example 3 of the present invention; Figure 6 : is a surface microscopic morphology of NiO prepared in Example 3 of the present invention. Figure 5 It can be seen that the diffraction peak positions of the NiO material prepared in this example correspond to those of the PDF card 75-0197 of the standard NiO material, indicating that a pure phase NiO material is obtained. The surface micromorphology of the NiO material is studied by scanning electron microscopy (SEM). Figure 6 As shown, it can be seen that the NiO material is a particle with a size of about 80 nm. Due to the size regulation of gelatin and the dispersion regulation of PVP, the size of the prepared nanoparticles is small, and the size distribution is uniform without agglomeration.

[0080] The metal elements and their contents in the NiO material of this embodiment were detected by inductively coupled plasma (ICP) technology. The results are shown in Table 1, and it can be seen that the prepared NiO nanoparticles have a high purity (99.4%) and are basically free of other impurities.

[0081] Table 1: NiO material composition test table of Example 3

[0082] element NiO Zn Al Ca Cd Cu content(%) 99.43821 0.3878 0.00289 0.102 0.001 0.0012 element K Na Fe Mg Pb Si content(%) 0.00048 0.024 0.00172 0.0072 0.00838 0.0236 element Zr Tl Cr content(%) 0.0012 0 0.00032

[0083] Embodiment 4-6

[0084] The preparation method of nickel oxide nanoparticles in this embodiment is basically the same as that in Example 3, except that:

[0085] The amount of gelatin added was 0.5 g, 0.25 g, and 2 g, respectively, and the corresponding mass concentrations of the gelatin aqueous solution were 2.44%, 1.23%, and 9.09%;

[0086] The amount of polyvinyl pyrrolidone added was 0.5 g, 0.25 g and 2 g, and the mass ratio of polyvinyl pyrrolidone to gelatin was 1:1;

[0087] The amount of nickel nitrate hexahydrate Ni(NO3)2·6H2O added as the nickel metal source remained unchanged, and the mass ratios of nickel nitrate hexahydrate to gelatin were 1:0.5, 1:0.25 and 1:2, respectively.

[0088] The other processes and parameters are the same as those of Example 3, and Examples 4-6 are obtained respectively. The other processes and parameters are not described in detail here.

[0089] See also Figure 7 , Figure 8 and Fig. 9 ,in Figure 7 is a surface microscopic morphology of NiO prepared in Example 4 of the present invention; Figure 8 is a surface microscopic morphology of NiO prepared in Example 5 of the present invention; Fig. 9 : is a surface microscopic morphology of NiO prepared in Example 6 of the present invention. Figure 7 It can be seen that when the concentration of gelatin and PVP is halved (0.5 g) and the mass ratio of nickel nitrate hexahydrate to gelatin is 1:0.5, the particle size distribution of the obtained NiO material is more uniform, but because the size restriction and dispersion effect of gelatin and PVP are halved, some particles grow further, and particles with an average size of about 100 nm are obtained. Figure 8It can be seen that when the amount of gelatin and PVP is further reduced (0.25 g), and the mass ratio of nickel nitrate hexahydrate to gelatin is 1:0.25, the growth restriction and dispersion effects of the nanoparticles are further weakened, and the obtained NiO nanoparticles have uneven particle sizes and a larger average particle size (about 200 nm). Fig. 9 It can be seen that when the amount of gelatin and PVP is doubled (2 g) and the mass ratio of nickel nitrate hexahydrate to gelatin is 1:2, the obtained NiO nanoparticles have good size dispersibility and uniform particle size distribution, which is different from the NiO particles obtained when the mass ratio of nickel nitrate hexahydrate to gelatin is 1:1 ( Figure 6 ) is not much different. Considering the economy and practicality, the present invention achieves the best effect when the mass ratio of nickel nitrate hexahydrate to gelatin is set to 1:1.

[0090] Example 7

[0091] In this embodiment, gelatin and polyvinyl pyrrolidone (PVP) are used as a size limiting agent and a surfactant to prepare nickel oxide, comprising the following steps:

[0092] Step S1, using gelatin as an organic macromolecular template and size limiting agent. Add 1g of gelatin to 20mL of deionized water and stir thoroughly to accelerate dissolution; then place the gelatin solution on a magnetic heating stirrer, heat to 50°C, and continue stirring until the gelatin is completely dissolved and the solution becomes transparent;

[0093] Step S2, using nickel nitrate hexahydrate Ni(NO3)2·6H2O as a metal nickel source, adding 1 g of nickel nitrate hexahydrate Ni(NO3)2·6H2O into the gelatin solution, and continuing to stir until dissolved;

[0094] Step S3, using polyvinyl pyrrolidone (PVP) as a surfactant, adding 1 g of polyvinyl pyrrolidone (PVP) to the mixed solution of step S2, and stirring thoroughly until dissolved;

[0095] Step S4, preparing 7% by mass dilute ammonia water as an alkali source, dripping the dilute ammonia water dropwise into the mixed solution of step S3, adjusting the pH to 8, so as to perform a precipitation reaction to generate nickel hydroxide Ni(OH)2; the chemical reaction formula of this step is as follows:

[0096] Ni(NO3)2+2NH4OH→Ni(OH)2↓+2NH4NO3

[0097] Step S5, heating the mixture of step S4 to 80° C., continuing to stir for 6 hours to form a gel state, then continuing to heat to 110° C. to evaporate the solution to separate the solid and liquid, stirring for 2 hours, to obtain a xerogel of nickel hydroxide;

[0098] Step S6, washing the nickel hydroxide xerogel with water and ethanol alternately by centrifugation to remove excess PVP and organic matter, and then drying it in an oven at 60° C., taking out the dried precipitate and grinding it in a mortar for 30 minutes, adding a small amount of ethanol during the process to make the powder obtained after grinding more uniformly dispersed, thereby obtaining a nickel hydroxide precursor;

[0099] Step S7, calcining the prepared nickel hydroxide precursor in a muffle furnace at 700°C for 2h (heating rate 5°C / min) to obtain nickel oxide particles. The chemical reaction formula of this step is as follows:

[0100] Ni(OH)2→NiO+H2O

[0101] Please refer to Figure 10, which is a microscopic image of the surface morphology of NiO prepared in Example 7 of the present invention. Fig.10 It can be seen that nickel oxide is mainly plate-shaped and flaky when nickel hydroxide is calcined, and its particle size is relatively large, indicating that gelatin and polyvinyl pyrrolidone are used as additives to prepare nickel hydroxide precursors, and then calcine to generate nickel oxide. In the process, gelatin and polyvinyl pyrrolidone have almost no effect on the regulation of nickel oxide particle size. However, the present invention converts the nickel source into basic nickel carbonate and then calcines it, and the obtained nickel oxide particles have a smaller particle size and a more uniform particle size. The reason is that gelatin and polyvinyl pyrrolidone interact with basic nickel carbonate particles and nickel oxide nanoparticles generated by conversion of basic nickel carbonate through surface groups to control the growth rate and crystal morphology of nanoparticles, making the nickel oxide particles smaller and more uniform in size.

[0102] The method for preparing nickel oxide nanoparticles of the present invention uses gelatin and polyvinyl pyrrolidone as template reagents and surfactants, which can effectively improve the dispersibility of nickel oxide nanoparticles without introducing harmful substances or by-products; and by adjusting the added amounts, the particle size and morphology of the nanoparticles can be regulated to meet the needs of different applications.

[0103] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for preparing nickel oxide nanoparticles, characterized in that: The steps include: Step S1, taking an appropriate amount of gelatin to prepare a gelatin aqueous solution with a mass concentration of 4.76-9.09%; Step S2, using nickel nitrate hexahydrate Ni(NO3)2·6H2O as a metal nickel source, adding the metal nickel salt into a gelatin aqueous solution, stirring, and obtaining a mixed solution A, wherein the mass ratio of nickel nitrate hexahydrate to gelatin is 1:1-2; Step S3, using polyvinyl pyrrolidone as a surfactant, adding it to the mixed solution A, stirring, and obtaining a mixed solution B, wherein the mass ratio of polyvinyl pyrrolidone to gelatin is 1:1-1.5; Step S4, adding an appropriate amount of aqueous ammonia to the mixed solution B to perform a precipitation reaction to generate nickel hydroxide, thereby obtaining a mixture C; Step S5, adding an appropriate amount of carbonate solution to the mixture C to perform a precipitation reaction to generate basic nickel carbonate, thereby obtaining a mixture D; Step S6, heating and evaporating the mixture D to perform solid-liquid separation to obtain a xerogel of basic nickel carbonate; Step S7, washing, drying, and grinding to obtain a basic nickel carbonate precursor; Step S8, calcining the basic nickel carbonate precursor at 650-700° C. to obtain nickel oxide nanoparticles.

2. The method for preparing nickel oxide nanoparticles according to claim 1, characterized in that: In step S4, the concentration of the ammonia water is 7-10%, and the volume ratio of the ammonia water to the mixed solution B is 1:0.2-0.

5.

3. The method for preparing nickel oxide nanoparticles according to claim 1, characterized in that: In step S5, the concentration of carbonate ions in the carbonate solution is 1-1.5 M, and the volume ratio of the carbonate solution to the mixture C is 1:0.5-1.

5.

4. The method for preparing nickel oxide nanoparticles according to claim 3, characterized in that: The carbonate is at least one of sodium carbonate, ammonium carbonate and ammonium bicarbonate.

5. The method for preparing nickel oxide nanoparticles according to claim 1, characterized in that: In step S6, the heating temperature is 80-110°C.

6. The method for preparing nickel oxide nanoparticles according to claim 1, characterized in that: In step S7, deionized water or a mixture of deionized water and ethanol is used as a washing dispersion, and washing is performed by suction filtration or centrifugal separation.

7. The method for preparing nickel oxide nanoparticles according to claim 1, characterized in that: In step S8, the heating rate is 2-5°C / min.

8. A nickel oxide nanoparticle, characterized in that: Prepared by the method according to any one of claims 1 to 7.